Aromatic phenolic resin-based hard carbon material, sodium-ion battery and preparation method thereof
By using aromatic phenolic resin as a precursor and performing a two-step heat treatment, a hard carbon material with a nanoscale microporous structure was prepared, which solved the problem of insufficient performance of existing hard carbon anode materials and achieved high-efficiency charge-discharge and long-cycle stability of sodium-ion batteries.
Patent Information
- Application Number
- CN202310538480.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-05-12
AI Technical Summary
The initial coulombic efficiency and rate performance of existing hard carbon anode materials need to be improved, making it difficult to meet the high-performance requirements of sodium-ion batteries.
Aromatic phenolic resin was used as a precursor to prepare hard carbon materials through a two-step heat treatment method, including pre-pyrolysis and high-temperature pyrolysis, and the process conditions were optimized to form a nanoscale microporous structure.
It improves the initial coulombic efficiency, charge-discharge capacity and cycle stability of hard carbon materials, especially showing excellent performance at high current densities, with a capacity retention of 84.2% after 1000 cycles.
Smart Images

Figure CN116812904B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, specifically to an aromatic phenolic resin-based hard carbon material, a sodium-ion battery, and a method for preparing the same. Background Technology
[0002] In recent years, sodium-ion batteries have been considered an important complement to lithium-ion batteries. Extensive research has focused on developing electrolytes and cathode materials for sodium-ion batteries. High-performance anode materials play an equally important role in further improving the energy density of sodium-ion batteries. Compared to alloy and conversion-based anode materials, which suffer from high plateau voltages and poor cycle stability, hard carbon anode materials are considered promising candidates for sodium-ion battery anode materials due to their lower plateau voltage and acceptable capacity.
[0003] Currently, there are studies on the preparation of hard carbon anode materials using partial resins, but the initial coulombic efficiency and rate performance still need further improvement. Summary of the Invention
[0004] Therefore, it is necessary to provide aromatic phenolic resin-based hard carbon materials, their preparation methods, and their applications in the fabrication of sodium-ion batteries. Sodium-ion batteries prepared using aromatic phenolic resin-based hard carbon materials as anode materials exhibit superior overall performance, including better initial coulombic efficiency, charge-discharge capacity, and cycle stability.
[0005] The present invention adopts the following technical solution:
[0006] This invention provides a method for preparing an aromatic phenolic resin-based hard carbon material, comprising the following steps: preparing aromatic phenolic resin powder; transferring the aromatic phenolic resin powder into a reaction furnace, heating it to 400-900°C under an argon atmosphere for prepyrolysis treatment, and cooling it to obtain a prepyrolysis product; heating the prepyrolysis product to 1000-1800°C under an argon atmosphere for high-temperature pyrolysis treatment, and cooling it to obtain the hard carbon material.
[0007] In some embodiments, the aromatic phenolic resin is selected from at least one of aralkylphenolic resin, biphenyl-type phenolic resin, and bisphenol A-type phenolic resin.
[0008] Preferably, the aromatic phenolic resin is selected from biphenyl-type phenolic resins.
[0009] In some embodiments, the heating rate of the pre-pyrolysis step is 1 to 10 °C / min; and / or the heating rate of the high-temperature pyrolysis step is 1 to 15 °C / min.
[0010] In some embodiments, the temperature of the high-temperature pyrolysis step is preferably 1400–1800°C.
[0011] The present invention also provides an aromatic phenolic resin-based hard carbon material, which is prepared by sequentially subjecting aromatic phenolic resin powder to pre-pyrolysis treatment at 400-900℃, cooling, and then high-temperature pyrolysis treatment at 1000-1800℃.
[0012] The aromatic phenolic resin-based hard carbon material has the following morphology: macroscopically, it consists of irregular blocky particles with nanoscale microporous structures inside. Preferably, the pore size of the nanoscale micropores is less than 2 nm.
[0013] The present invention can also provide a negative electrode sheet, which is prepared using a hard carbon material comprising the methods described above. Preferably, the negative electrode sheet is prepared using a conductive agent, a binder, a solvent, and a hard carbon material comprising the methods described above.
[0014] The present invention can also provide a sodium-ion battery, characterized in that it includes a positive electrode, a separator, the aforementioned negative electrode, and a sodium-ion electrolyte.
[0015] Compared with the prior art, the core advantage of this invention is:
[0016] 1) The method of the present invention uses aromatic phenolic resin as a precursor, which contains a large number of aromatic rings and the raw materials are readily available. When the hard carbon material prepared by the two-step heat treatment is applied to the anode of sodium-ion batteries, compared with other anode materials, the hard carbon anode material prepared by it has excellent first coulombic efficiency, charge-discharge capacity and cycle stability.
[0017] Specifically, aromatic phenolic resin-based hard carbon materials, as anode materials for sodium-ion batteries, exhibit higher reversible specific capacity, reaching 384.8 mAh / g at a current density of 50 mA / g. Even when the current density increases to 1 A / g, the sodium-ion battery capacity remains at 219.9 mAh / g. After 1000 cycles, the capacity retention rate can reach up to 84.2%. Compared to other resin-based hard carbon materials, aromatic phenolic resin-based hard carbon materials show improvements in charge / discharge capacity, rate performance, and cycle performance.
[0018] 2) In particular, the method of the present invention employs a two-step heat treatment: the first step heat treatment can be regarded as pre-pyrolysis, in which some impurities are eliminated and the microstructure of the material becomes more ordered. Further high-temperature pyrolysis is carried out, and the overall charge-discharge performance capacity and rate capability can be improved. Attached Figure Description
[0019] Figure 1 This is a SEM image of the aromatic phenolic resin-based hard carbon material prepared in Example 4. Detailed Implementation
[0020] The present invention will be further described in detail below with reference to specific embodiments, so that those skilled in the art can more clearly understand the present invention. The following embodiments are only used to illustrate the present invention, and are not intended to limit the scope of the present invention. Based on the specific embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention. In the embodiments of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; in the embodiments of the present invention, unless specifically specified, the technical means used are conventional means well known to those skilled in the art.
[0021] In this application, aromatic phenolic resin refers to a class of phenolic resins having a benzene ring structure, wherein such phenolic resins contain at least one benzene ring with a delocalized bond.
[0022] The structural formula of biphenyl-type phenolic resin is as follows:
[0023]
[0024] The structural formula of alkylphenol resin is:
[0025]
[0026] The structural formula of bisphenol A type phenolic resin is:
[0027]
[0028] The structural formula of aliphatic phenolic resin is:
[0029]
[0030] Description of the sources and physicochemical properties of some key materials used in the experiment:
[0031] raw material Commercially available trademarks Physicochemical indicators source Biphenyl-type phenolic resin BNH-851 Hydroxyl equivalent (198-208 g / eq) Hunan Jingyuan New Material Technology Co., Ltd. Arylalkylphenol resin XYH-880 Hydroxyl equivalent (172-180 g / eq) Hunan Jingyuan New Material Technology Co., Ltd. Bisphenol A type phenolic resin BPA-18 Hydroxyl equivalent (100-160 g / eq) Jiangyin Dongpeng International Technology Trade Co., Ltd. Aliphatic phenolic resin PF-8106 Hydroxyl equivalent (104-110 g / eq) Hunan Jingyuan New Material Technology Co., Ltd.
[0032] Example 1
[0033] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material, including the following steps:
[0034] S1, the biphenyl-type phenolic resin is ground into powder by a vibration milling machine to obtain resin powder.
[0035] S2, the resin powder prepared in step S1 is transferred to a tube furnace, argon gas is introduced, and prepyrolysis is performed under the following conditions: the temperature is increased from room temperature to 600℃ at a rate of 1℃ / min, and held at that temperature for 2 hours. After cooling to room temperature, the prepyrolysis product is obtained.
[0036] S3. The prepyrolysis product from step S2 is further subjected to high-temperature pyrolysis. The process conditions are: heating from room temperature to 1000℃ at a rate of 2℃ / min and holding at that temperature for 1 hour. After cooling to room temperature, hard carbon material is obtained.
[0037] This embodiment also provides a battery application example, the preparation and assembly method of which includes the following steps:
[0038] S1, Preparation of the negative electrode:
[0039] The hard carbon material prepared above was mixed evenly with carbon black and sodium alginate at a mass ratio of 8:1:1. An appropriate amount of deionized water was added, and the mixture was stirred to form a uniformly distributed slurry (for 5 hours). The uniformly mixed slurry was then coated onto a copper foil current collector. After vacuum drying, the negative electrode sheet was formed.
[0040] S2, Battery Assembly:
[0041] In a glove box under an argon atmosphere, the negative electrode sheet prepared in step S1 is used as a separator with glass microfiber, a sodium metal sheet as a counter electrode, nickel foam as a gasket, and a 1 mol / L NaPF6 ethylene glycol dimethyl ether solution as an electrolyte to assemble a button cell HC1.
[0042] Example 2
[0043] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0044] In step S3, the high-temperature pyrolysis processing temperature is adjusted to 1200℃.
[0045] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC2.
[0046] Example 3
[0047] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0048] In step S3, the high-temperature pyrolysis processing temperature is adjusted to 1400℃.
[0049] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC3.
[0050] Example 4
[0051] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0052] In step S3, the high-temperature pyrolysis processing temperature is adjusted to 1600℃.
[0053] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC4.
[0054] Example 5
[0055] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0056] In step S3, the high-temperature pyrolysis processing temperature is adjusted to 1800℃.
[0057] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC5.
[0058] Example 6
[0059] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0060] In step S1, arylalkylphenol resin is used instead of biphenyl phenol resin;
[0061] In step S2, the prepyrolysis process conditions are: heating from room temperature to 700℃ at a rate of 1℃ / min and holding at that temperature for 4 hours;
[0062] In step S3, the high-temperature pyrolysis treatment temperature is adjusted to 1600℃ and held for 5 hours.
[0063] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC6.
[0064] Example 7
[0065] This embodiment provides a method for preparing an aromatic phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0066] In step S1, bisphenol A type phenolic resin is used instead of biphenyl type phenolic resin;
[0067] In step S2, the prepyrolysis process conditions are: heating from room temperature to 600℃ at a rate of 1℃ / min and holding at that temperature for 6 hours;
[0068] In step S3, the high-temperature pyrolysis treatment temperature is adjusted to 1600℃ and held for 7 hours.
[0069] This embodiment also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HC7.
[0070] Comparative Example 1
[0071] This comparative example provides a method for preparing a phenolic resin-based hard carbon material. The preparation method and process steps are basically the same as those in Example 1, with the only difference being:
[0072] In step S1, aliphatic phenolic resin is used instead of biphenyl-type phenolic resin.
[0073] This comparative example also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HCS1.
[0074] Comparative Example 2
[0075] This comparative example provides a method for preparing a phenolic resin-based hard carbon material, comprising the following steps:
[0076] S1, the biphenyl-type phenolic resin is ground into powder by a vibration milling machine to obtain resin powder.
[0077] S2, the resin powder prepared in step S1 is transferred to a tube furnace, argon gas is introduced, and one-step pyrolysis is performed. The process conditions are: the temperature is increased from room temperature to 1000℃ at a rate of 2℃ / min, and held at that temperature for 1 hour. After cooling to room temperature, hard carbon material is obtained.
[0078] This comparative example also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HCS2.
[0079] Comparative Example 3
[0080] This comparative example refers to the optimal experimental example in "CN110817833A_A Preparation Method of Resin-Based Hard Carbon Anode Material", and the specific preparation method includes the following steps:
[0081] S1 uses biphenyl-type phenolic resin as the skeleton and is fully carbonized at 500℃ for 5 hours.
[0082] S2, the sample obtained in step S1 is impregnated with impregnating agent bitumen, and the ratio of resin to impregnating agent is 1:2.
[0083] S3, carbonize the sample prepared in step S2 at 450℃.
[0084] S4. The carbonized material from step S3 is crushed to obtain a material with a median particle size D50 of 20 μm.
[0085] S5. The sample prepared in step S4 is carbonized at a high temperature of 1400℃ to obtain the negative electrode material.
[0086] This comparative example also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HCS3.
[0087] Comparative Example 4
[0088] This comparative example refers to the optimal experimental example in "CN114824257A_A Hard Carbon Anode Material and Its Preparation Method and Application". The specific preparation method includes the following steps:
[0089] S1, place the biphenyl-type phenolic resin into a high-temperature vacuum atmosphere furnace for heat treatment, with a heating rate of 2℃ / min, heating to 210℃, and holding for 1 hour.
[0090] S2, Nitrogen gas is introduced into the high-temperature vacuum atmosphere furnace, and the temperature is continued to rise at a rate of 3℃ / min for 223 min. Next, the heating rate is reduced to 1℃ / min for 221 min, and the temperature is raised to 1100℃, then held for 1 hour. Finally, the temperature is cooled at a rate of 5℃ / min to 25℃.
[0091] S3, after cooling, the material is crushed to ≤2mm by a ceramic double roll crusher, and then finely crushed and classified by an air jet mill and a classifier to obtain hard carbon anode material.
[0092] This comparative example also provides a battery application example, the preparation and assembly method of which is described in Example 1, and is assembled into a button cell HCS4.
[0093] Application performance testing:
[0094] The sodium-ion batteries HC1-HC7 and HCS1-HCS4 prepared in the above examples and comparative examples were subjected to constant current charge-discharge tests: the test voltage range was 0-2V, and the charge-discharge capacity and initial coulombic efficiency of the sodium-ion batteries prepared in each example and comparative example were obtained; the current density (unit: mA / g) was 50, 100, 200, 500, 1000, 2000 and 5000, and the rate performance of the batteries prepared in each example and comparative example was obtained; the current density was 500 mA / g, and the charge-discharge cycle was 1000 cycles, and the cycle retention rate of the charge-discharge performance of the sodium-ion batteries prepared in each example and comparative example was obtained.
[0095] The specific test results are shown in the table below:
[0096]
[0097]
[0098] As can be seen from the table above, the sodium-ion batteries made of aromatic phenolic resin-based hard carbon materials prepared in Examples 1 to 7 have significantly better performance in terms of initial coulombic efficiency, charge-discharge performance, and cycle retention than those in Comparative Examples 1 to 4.
[0099] In particular, compared with Comparative Example 2, the aromatic phenolic resin-based hard carbon materials prepared by the two-step heat treatment method in Examples 1 to 7 have better first coulombic efficiency, charge-discharge performance and cycle retention when applied to sodium-ion battery systems.
[0100] Observation and testing revealed that the hard carbon material prepared in the embodiments of this invention is a hard carbon material with an irregular blocky macroscopic morphology and an internal nanoscale microporous structure. The SEM image of the hard carbon material prepared in Example 4 is shown below. Figure 1 As shown.
[0101] In addition, it is worth noting that, after extensive research, the inventors discovered that:
[0102] 1) In the preparation method of aromatic phenolic resin-based hard carbon materials, the temperature of the first step of pre-pyrolysis is preferably controlled at 400-900℃, and the heating rate is controlled at 1-10℃ / min. The temperature of the second step of high-temperature pyrolysis is preferably controlled at 1400-1800℃, and the heating rate is controlled at 1-15℃ / min. Overall, this is beneficial to controlling the comprehensive performance advantages such as initial coulombic efficiency, charge-discharge performance and cycle retention rate.
[0103] 2) When the process conditions of the first step of pre-pyrolysis and the second high-temperature pyrolysis are the same, compared with bisphenol A type phenolic resin and aralkyl phenolic resin, the aromatic phenolic resin used to prepare hard carbon material with biphenyl type phenolic resin as the negative electrode material has better overall performance in terms of initial coulombic efficiency, charge-discharge performance and cycle retention rate.
[0104] It should be noted that the above embodiments are only for further elaboration and explanation of the technical solution of the present invention, and are not intended to further limit the technical solution of the present invention. The method of the present invention is only a preferred embodiment and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing an aromatic phenolic resin-based hard carbon material, characterized in that, Includes the following steps: Preparation of aromatic phenolic resin powder; The aromatic phenolic resin powder was transferred into a reaction furnace and heated to 400-900 °C under an argon atmosphere for prepyrolysis treatment. After cooling, the prepyrolysis product was obtained. Under an argon atmosphere, the temperature is raised to 1000~1800 ℃ to perform high-temperature pyrolysis treatment on the prepyrolysis product. After cooling, hard carbon material is obtained. The aromatic phenolic resin is selected from at least one of aralkyl phenolic resin, biphenyl phenolic resin, and bisphenol A phenolic resin. The heating rate of the preheating step is 1~10℃ / min, and the preheating holding treatment is 1~10 h; The heating rate of the high-temperature pyrolysis step is 1~15 ℃ / min, and the high-temperature pyrolysis holding treatment is 1~12 h.
2. The method for preparing aromatic phenolic resin-based hard carbon material according to claim 1, characterized in that, The aromatic phenolic resin is selected from biphenyl-type phenolic resins.
3. The method for preparing aromatic phenolic resin-based hard carbon material according to claim 1, characterized in that, The temperature for the high-temperature pyrolysis step is 1400~1800 ℃.
4. An aromatic phenolic resin-based hard carbon material, characterized in that, It is prepared by sequentially subjecting aromatic phenolic resin powder to preheating treatment at 400~900 ℃, cooling, and then high-temperature pyrolysis treatment at 1000~1800 ℃.
5. The aromatic phenolic resin-based hard carbon material according to claim 4, characterized in that, The aromatic phenolic resin-based hard carbon material has an irregular blocky particle morphology, and the particles contain a nanoscale microporous structure.
6. A negative electrode sheet, characterized in that, It is prepared using a hard carbon material comprising any one of claims 1 to 3.
7. The negative electrode sheet according to claim 6, characterized in that, It is prepared using a conductive agent, a binder, a solvent, and a hard carbon material comprising any one of the methods described in claims 1 to 3.
8. A sodium-ion battery, characterized in that, It includes a positive electrode, a separator, a negative electrode as described in claim 6 or 7, and a sodium ion electrolyte.
Citation Information
Patent Citations
Preparation method of resin-based hard carbon negative electrode material
CN110817833A
Hard carbon negative electrode material and preparation method and application thereof
CN114824257A
Preparation method of novolac epoxy resin-based hard carbon material, hard carbon material and sodium ion battery
CN115010109A