A lithium transition metal composite oxide, an electrochemical device, and an electronic device
By adjusting the twin structure angle of lithium transition metal composite oxides and introducing element A, the problem of twin structure instability in lithium-ion batteries under high voltage was solved, thereby improving the cycle performance and structural stability of the batteries.
Patent Information
- Application Number
- CN202311009828.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2041-11-11
AI Technical Summary
The twinned structure of lithium-ion batteries is unstable under high voltage, making them prone to cracking and affecting cycle performance.
By controlling the angle between the transition metal layers in the first and second regions of the twin structure of lithium transition metal composite oxide to 65° to 80°, and introducing elements such as Mg, Al, and Ti at the grain boundaries, the grain boundary structure is modified to form a stable twin structure.
It improves the cycle performance and structural stability of lithium-ion batteries under high voltage and reduces the risk of twin structure cracking.
Smart Images

Figure CN116826022B_ABST
Abstract
Description
[0001] This application is a divisional application of application number 202111333551.6, filed on November 11, 2021, entitled "A Lithium Transition Metal Composite Oxide, Electrochemical Device and Electronic Device". Technical Field
[0002] This application relates to the field of electrochemical technology, and in particular to a lithium transition metal composite oxide, an electrochemical device, and an electronic device. Background Technology
[0003] Lithium-ion batteries have advantages such as high energy density, high open-circuit voltage, low self-discharge rate, long cycle life, and good safety, and are widely used in portable energy storage, electronic devices, electric vehicles, and other fields. However, this also places higher demands on the overall performance of lithium-ion batteries, such as good cycle performance at high voltages (e.g., greater than 4.2V). Summary of the Invention
[0004] The purpose of this application is to provide a lithium transition metal composite oxide, an electrochemical device, and an electronic device to improve the cycling performance of the electrochemical device under high voltage.
[0005] The first aspect of this application provides a lithium transition metal composite oxide, wherein the lithium transition metal composite oxide has a twinned structure, the twinned structure comprising a first crystal region and a second crystal region, with a grain boundary between the first crystal region and the second crystal region, the first crystal region comprising a first region within 20 nm of the grain boundary, the second crystal region comprising a second region within 20 nm of the grain boundary, and the angle between the transition metal layers in the first region and the second region being 65° to 80°. By controlling the angle between the transition metal layers in the first region and the second region to be 65° to 80°, the stress and strain between the first crystal region and the second crystal region during charge and discharge can be reduced, the stability of the twinned structure can be improved, and thus the cycle performance of the electrochemical device under high voltage can be improved.
[0006] In some embodiments of this application, the transition metal layer in the first region includes at least one of Co, Mn, or Ni. In some embodiments of this application, the transition metal layer in the second region includes at least one of Co, Mn, or Ni. The main body of both the first and second regions is a layered oxide material containing Co / Ni / Mn, which fuses and grows to form twin boundaries under high temperature. The first and second regions include the aforementioned transition metal elements and both exhibit a layered structure, connected by twinning, which is a low-energy connection method that is beneficial to structural stability.
[0007] In some embodiments of this application, the grain boundaries contain element A, which includes at least one of Mg, Al, Ti, Zr, La, Nb, Hf, Zn, Y, or F. By including element A, the grain boundaries between the first and second crystal regions can be modified, improving the stability of the grain boundary structure and thus reducing the risk of twinning cracking.
[0008] In some embodiments of this application, the first region includes a third region within 10 nm of the grain boundary and a fourth region between 10 nm and 20 nm of the grain boundary. Based on the total molar amount of Co, Mn, and Ni in the third region, the molar percentage of element A in the third region is X; based on the total molar amount of Co, Mn, and Ni in the fourth region, the molar percentage of element A in the fourth region is Y, satisfying X / Y ≥ 2. This is more conducive to improving the structural stability near the grain boundary in the first crystal region, reducing the risk of twinning cracking, and thus improving the structural stability of the lithium transition metal composite oxide under high voltage.
[0009] In some embodiments of this application, X is 0.2% to 2.5%. In this case, the structural stability near the grain boundaries in the first crystal region can be better guaranteed.
[0010] In some embodiments of this application, the area of the second crystal region in the cross-section of the lithium transition metal composite oxide is 30% to 60% based on the area of the cross-section. By adjusting the area ratio of the second crystal region within the above range, it is beneficial to improve the rate performance and cycle performance of the electrochemical device.
[0011] In some embodiments of this application, the lithium transition metal composite oxide includes a substrate and a first layer located on the surface of the substrate, the first layer comprising a metal fluoride. When the first layer comprises a metal fluoride, side reactions between the substrate surface and the electrolyte can be suppressed, improving the stability of the surface structure of the lithium transition metal composite oxide, thereby improving the cycle performance of the electrochemical device.
[0012] In some embodiments of this application, the lithium transition metal composite oxide satisfies at least one of the following characteristics: (a) the metal fluoride includes at least one of CoF2, CoF3, CoFO, MgF2, NaF, or AlF3; and (b) the thickness of the first layer is 1 nm to 8 nm. When the lithium transition metal composite oxide satisfies at least one of characteristics (a) to (b), it is beneficial to improve the cycle performance of the electrochemical device.
[0013] A second aspect of this application provides an electrochemical device comprising a positive electrode, the positive electrode comprising a positive electrode material layer, the positive electrode material layer comprising a positive electrode active material, and the positive electrode active material comprising a lithium transition metal composite oxide as described in any of the foregoing embodiments.
[0014] In some embodiments of this application, the electrochemical device is fully disassembled to obtain a positive electrode sheet. A circular piece with a diameter of 1.4 cm from the positive electrode sheet is taken and assembled with lithium metal to form a coin cell. The coin cell is charged to 4.7V, wherein the included angle β in the lithium transition metal composite oxide is 70° to 86°.
[0015] In some embodiments of this application, the electrochemical device is fully disassembled to obtain the positive electrode. Two circular pieces with a diameter of 1.4 cm from the positive electrode are then assembled with lithium metal to form a first coin cell and a second coin cell, respectively. The first coin cell is charged to 4.5V, and the second coin cell is charged to 4.7V. In the lithium transition metal composite oxide of the first coin cell, the angle between the transition metal layers in the first region and the transition metal layers in the second region is α; in the lithium transition metal composite oxide of the second coin cell, the angle between the transition metal layers in the first region and the transition metal layers in the second region is β, satisfying |β-α|≤5°. When the electrochemical device satisfies the above characteristics, it indicates that the strain between the first and second regions of the lithium transition metal composite oxide is small during charging and discharging, and the twinned structure has good stability.
[0016] In some embodiments of this application, the proportion of positive electrode active material particles with twinned structures is between 35% and 75%, based on the number of positive electrode active material particles. Maintaining the proportion of positive electrode active material particles with twinned structures within this range is beneficial for improving the rate performance and cycle performance of the electrochemical device.
[0017] In some embodiments of this application, the electrochemical device further includes an electrolyte comprising a fluorocarbonate compound, wherein the mass percentage of the fluorocarbonate compound is from 0.05% to 15% based on the mass of the electrolyte. The introduction of the fluorocarbonate compound can form a protective layer at the interface of the twinned structure, reducing side reactions between the lithium transition metal complex oxide and the electrolyte, thereby improving the cycle performance of the electrochemical device.
[0018] In some embodiments of this application, the fluorocarbonate compound includes at least one of monofluoroethylene carbonate, difluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate.
[0019] A third aspect of this application provides an electronic device that includes the electrochemical device in any of the foregoing embodiments.
[0020] This application provides a lithium transition metal composite oxide, an electrochemical device, and an electronic device. The lithium transition metal composite oxide has a twinned structure, comprising a first crystal region and a second crystal region, with a grain boundary between the first and second crystal regions. The first crystal region includes a first area within 20 nm of the grain boundary, and the second crystal region includes a second area within 20 nm of the grain boundary. The angle between the transition metal layers in the first and second crystal regions is 65° to 80°. By adjusting the angle between the first and second regions to 65° to 80°, the stability of the twinned structure can be improved, thereby improving the cycling performance of the electrochemical device under high voltage. Attached Figure Description
[0021] To more clearly illustrate the technical solutions of this application and the prior art, the accompanying drawings used in the embodiments and the prior art are briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application.
[0022] Figure 1 This is a scanning electron microscope image of the cross-section of the positive electrode in Example 1-1;
[0023] Figure 2 This is a scanning electron microscope image of a lithium transition metal composite oxide with a twinned structure in the cross-section of the positive electrode sheet in Example 1-1;
[0024] Figure 3 The image shows a transmission electron microscope (TEM) image of a lithium transition metal composite oxide obtained by disassembling the electrochemical device after it was fully charged in Example 1-1, assembling the positive electrode with lithium metal to form a coin cell, and charging it to 4.7V.
[0025] Figure 4 The graphs show the capacity retention rate of the electrochemical devices in Examples 1-1 and Comparative Examples 1-1 as a function of the number of cycles. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. All other technical solutions obtained by those skilled in the art based on the embodiments of this application fall within the scope of protection of this application.
[0027] It should be noted that, in the specific embodiments of this application, lithium-ion batteries are used as an example of electrochemical devices to explain this application, but the electrochemical devices of this application are not limited to lithium-ion batteries.
[0028] The inventors of this application have discovered that positive electrode active materials with twinned structures, such as lithium cobalt oxide, can provide multi-directional migration pathways for lithium ions, thereby improving the rate performance of electrochemical devices. However, twinned structures are unstable under high voltages, especially at grain boundaries, where they are prone to cracking. This can lead to side reactions between the material and the electrolyte, affecting the cycle performance of the electrochemical device and making it difficult to meet the needs of practical applications.
[0029] The first aspect of this application provides a lithium transition metal composite oxide, wherein the lithium transition metal composite oxide has a twinned structure, the twinned structure comprising a first crystal region and a second crystal region, with a grain boundary between the first crystal region and the second crystal region, the first crystal region comprising a first region within 20 nm of the grain boundary, the second crystal region comprising a second region within 20 nm of the grain boundary, and the angle between the transition metal layers in the first region and the transition metal layers in the second region being 65° to 80°. For example, the angle can be 65°, 70°, 75°, 80° or any range thereof. The lithium transition metal composite oxide can be used as a positive electrode active material in electrochemical devices. The inventors of this application have discovered that by controlling the angle between the first region and the second region to be 65° to 80°, the stress and strain between the first crystal region and the second crystal region during charge and discharge can be reduced, the stability of the twinned structure can be improved, and thus the cycle performance of the electrochemical device under high voltage can be improved. In this application, the first crystal region refers to a region on one side of the twin grain boundary where the transition metal layers in the crystal structure have the same orientation, and the second crystal region refers to a region on the other side of the twin grain boundary, different from the first crystal region, where the transition metal layers in the crystal structure have the same orientation. The aforementioned included angle refers to the angle formed when the orientations of the transition metal layers in the first region and the second region are extended to intersect at the grain boundary. Furthermore, if the lithium transition metal composite oxide exists as a positive electrode active material in an electrochemical device, the aforementioned included angle refers to the angle between the transition metal layers in the first region and the transition metal layers in the second region of the lithium transition metal composite oxide in the positive electrode sheet after the electrochemical device is fully filled and disassembled.
[0030] In some embodiments of this application, the transition metal layer in the first region includes at least one of Co, Mn, or Ni. In some embodiments of this application, the transition metal layer in the second region includes at least one of Co, Mn, or Ni. By including the aforementioned transition metals in both the first and second regions, the interfacial compatibility between the first and second regions is improved, thereby enhancing the stability of the twin structure.
[0031] In some embodiments of this application, the grain boundaries contain element A, which includes at least one of Mg, Al, Ti, Zr, La, Nb, Hf, Zn, Y, or F. The inventors of this application have discovered that by including element A, the grain boundaries between the first and second crystal regions can be modified, improving the stability of the grain boundary structure and thus reducing the risk of twinning cracking. For example, when element A includes Mg, O at the grain boundary can form Mg-O bonds with Mg, improving the stability of the O structure; for example, when element A includes F, it can form a localized disordered structure, dispersing stress and thus reducing the risk of twinning cracking.
[0032] In some embodiments of this application, the molar percentage of element A in the grain boundary is from 0.2% to 2.5%, based on the total molar amount of Co, Mn, and Ni in the grain boundary. For example, the mass percentage of element A can be 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, or any range thereof. By controlling the molar percentage of element A within the above range, it is beneficial to improve the stability of the grain boundary structure, thereby reducing the risk of twinning cracking and thus improving the cycling performance of the electrochemical device at high voltage.
[0033] In some embodiments of this application, the first region includes a third region within 10 nm of the grain boundary and a fourth region between 10 nm and 20 nm of the grain boundary. Based on the total molar amount of Co, Mn, and Ni in the third region, the molar percentage of element A in the third region is X; based on the total molar amount of Co, Mn, and Ni in the fourth region, the molar percentage of element A in the fourth region is Y, satisfying: X / Y ≥ 2, preferably 2 ≤ X / Y ≤ 12. The value of X / Y can be 2, 3, 4, 5, 6, 7, 8, 9, 10, or any range thereof.
[0034] In some embodiments of this application, X is from 0.2% to 2.5%. For example, the value of X can be 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, or any range therebetween. An X value of 0.2% to 2.5% is more conducive to improving the structural stability near the grain boundaries in the first crystal region, reducing the risk of twinning cracking, and thus improving the structural stability of lithium transition metal composite oxides under high voltage. This application does not impose any particular restriction on the value of Y, as long as X / Y ≥ 2, for example, 0% < Y ≤ 1.0%.
[0035] In some embodiments of this application, the area of the second crystal region in the cross-section of the lithium transition metal composite oxide is between 30% and 60%, based on the area of the cross-section. For example, the area percentage of the second crystal region can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any range therebetween. By adjusting the area percentage of the second crystal region within the above range, it is beneficial to improve the rate performance and cycle performance of the electrochemical device.
[0036] In some embodiments of this application, the lithium transition metal composite oxide includes a substrate and a first layer located on the surface of the substrate, the first layer comprising a metal fluoride. The inventors of this application have discovered that when the lithium transition metal composite oxide has a first layer comprising a metal fluoride, side reactions between the substrate surface and the electrolyte can be suppressed, improving the stability of the surface structure of the lithium transition metal composite oxide, thereby improving the cycle performance of the electrochemical device.
[0037] In some embodiments of this application, the metal fluoride includes at least one of CoF2, CoF3, CoFO, MgF2, NaF, or AlF3.
[0038] In some embodiments of this application, the thickness of the first layer is from 1 nm to 8 nm. For example, the thickness of the first layer can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, or any range thereof. By adjusting the thickness of the first layer within the above range, it is beneficial to improve the cycle performance and rate performance of the electrochemical device.
[0039] This application does not impose any particular limitation on the preparation method of lithium transition metal composite oxides, as long as the purpose of this application can be achieved. For example, the preparation method of lithium transition metal composite oxides may include, but is not limited to, the following steps: mixing a transition metal source and a dopant source and preparing an aqueous solution, obtaining a precipitate by co-precipitation, then performing a first calcination, grinding and sieving to obtain a first intermediate product; then mixing the first intermediate product with a lithium source and performing a second calcination, grinding and sieving to obtain a second intermediate product; then mixing the second intermediate product with a dopant source and performing a third calcination, grinding and sieving to obtain the lithium transition metal composite oxide. This application does not impose any particular limitation on the temperature T1 and time t1 of the first calcination, the temperature T2 and time t2 of the second calcination, and the temperature T3 and time t3 of the third calcination, as long as the purpose of this application can be achieved. For example, T1 is 500℃ to 1000℃, t1 is 5h to 15h; T2 is 800℃ to 1500℃, t2 is 5h to 15h; T3 is 500℃ to 1000℃, t3 is 5h to 15h.
[0040] Lithium transition metal composite oxides include Li x Ni y Coz Mn k Z q O 2±a T a , wherein Z includes at least one of B, Mg, Al, Si, P, S, Ti, Cr, Fe, Cu, Zn, Ga, Y, Zr, Mo, Ag, W, In, Sn, Sb, La, Nb, Hf or Ce, and T is a halogen; wherein 0.2<x≤1.2, 0≤y≤1, 0≤z≤1, 0≤k≤1, 0≤q≤1, y, z and k are not 0 at the same time, and 0≤a≤1.
[0041] A second aspect of the present application provides an electrochemical device, which includes a positive electrode plate, the positive electrode plate includes a positive electrode material layer, the positive electrode material layer includes a positive electrode active material, and the positive electrode active material includes the lithium transition metal composite oxide according to any one of the aforementioned embodiments. The lithium transition metal composite oxide provided by the present application has good structural stability, so that the electrochemical device provided by the present application has good cycle performance.
[0042] In some embodiments of the present application, the electrochemical device is fully discharged and then disassembled to obtain a positive electrode plate, a wafer with a diameter of 1.4 cm taken from the positive electrode plate is assembled with lithium metal into a button cell, the button cell is charged to 4.7 V, wherein the included angle β in the lithium transition metal composite oxide is 70° to 86°. For example, the included angle in the lithium transition metal composite oxide is 70°, 72°, 75°, 78°, 80°, 82°, 85°, 86°, or any range therebetween. When charged to 4.7 V, the included angle in the lithium transition metal composite oxide falls within the above range, which indicates that the change of the included angle between the transition metal layer in the first region and the transition metal layer in the second region is small at high voltage, the stability of the twin crystal structure can be improved, so as to improve the cycle performance of the electrochemical device at high voltage.
[0043] In some embodiments of this application, the electrochemical device is fully disassembled to obtain the positive electrode. Two circular pieces with a diameter of 1.4 cm from the positive electrode are then assembled with lithium metal to form a first coin cell and a second coin cell, respectively. The first coin cell is charged to 4.5V, and the second coin cell is charged to 4.7V. In the lithium transition metal composite oxide of the first coin cell, the angle between the transition metal layers in the first region and the transition metal layers in the second region is α; in the lithium transition metal composite oxide of the second coin cell, the angle between the transition metal layers in the first region and the transition metal layers in the second region is β, satisfying |β-α|≤5°. This indicates that the strain between the first and second regions of the lithium transition metal composite oxide is small during the high-voltage range of the charge-discharge process, and the twinned structure has good stability. For example, |β-α| can be 0.1°, 0.5°, 1°, 2°, 3°, 4°, 5°, or any range thereof. This application does not impose any particular limitation on the assembly method of the coin cells; assembly methods known in the art can be used.
[0044] In some embodiments of this application, the proportion of positive electrode active material particles with twinned structures is between 35% and 75%, based on the number of particles. For example, the proportion of positive electrode active material particles with twinned structures is 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or any range therebetween. By controlling the proportion of positive electrode active material particles with twinned structures within the above range, it is beneficial to improve the rate performance and cycle performance of the electrochemical device.
[0045] In some embodiments of this application, the positive electrode active material may also include positive electrode active materials known in the art, such as, but not limited to, at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, or lithium manganese iron phosphate.
[0046] In some embodiments of this application, the electrochemical device includes an electrolyte comprising a fluorocarbonate compound, wherein the mass percentage of the fluorocarbonate compound is from 0.05% to 15% based on the mass of the electrolyte. For example, the mass percentage of the fluorocarbonate compound can be 0.05%, 0.5%, 1%, 5%, 10%, 15%, or any range thereof. The inventors of this application have discovered that the introduction of the fluorocarbonate compound can form a protective layer at the interface of the twinned structure, reducing side reactions between the lithium transition metal composite oxide and the electrolyte, thereby improving the cycle performance of the electrochemical device.
[0047] In some embodiments of this application, the fluorocarbonate compound includes at least one of monofluoroethylene carbonate, difluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate.
[0048] In some embodiments of this application, the positive electrode material layer includes a binder. In some embodiments of this application, the binder may be, but is not limited to, at least one of polyacrylamide, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyamide-imide, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyvinylidene fluoride, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), aqueous acrylic resin, carboxymethyl cellulose (CMC), or sodium carboxymethyl cellulose (CMC-Na).
[0049] The positive electrode typically includes a positive current collector. In this application, the positive current collector is not particularly limited, as long as it achieves the purpose of this application. For example, it may include, but is not limited to, aluminum foil, aluminum alloy foil, or composite current collectors. In this application, the thickness of the positive current collector is not particularly limited, as long as it achieves the purpose of this application, for example, a thickness of 8 μm to 12 μm. In this application, the positive electrode material layer can be disposed on one or both surfaces along the thickness direction of the positive current collector. It should be noted that the "surface" here can be the entire area of the positive current collector or a portion of it; there are no particular limitations in this application, as long as the purpose of this application is achieved.
[0050] In this application, the positive electrode material layer may also include a conductive agent. This application does not impose any particular limitation on the conductive agent, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metallic materials, or conductive polymers. The aforementioned carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The aforementioned carbon fibers may include, but are not limited to, vapor-grown carbon fibers (VGCF) and / or carbon nanofibers. The aforementioned metallic materials may include, but are not limited to, metal powders and / or metal fibers; specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum, or silver. The aforementioned conductive polymers may include, but are not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, or polypyrrole.
[0051] Optionally, the positive electrode may further include a conductive layer located between the positive electrode current collector and the positive electrode material layer. This application does not impose any particular limitation on the composition of the conductive layer; it can be a conductive layer commonly used in the art, such as, but not limited to, the conductive agent and the binder described above.
[0052] The electrochemical device of this application also includes a negative electrode sheet, which typically comprises a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. This application does not impose any particular limitation on the negative electrode current collector, as long as it achieves the purpose of this application. For example, it may include, but is not limited to, copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or composite current collectors. In this application, there is no particular limitation on the thickness of the negative electrode current collector, as long as it achieves the purpose of this application, for example, a thickness of 4 μm to 12 μm. In this application, the negative electrode material layer may be disposed on one or both surfaces along the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a part of the negative electrode current collector; this application does not impose any particular limitation, as long as it achieves the purpose of this application.
[0053] In this application, the negative electrode material layer includes a negative electrode active material. The negative electrode active material is not particularly limited, as long as it achieves the purpose of this application. Examples include, but are not limited to, natural graphite, artificial graphite, mesophase microcarbon spheres, hard carbon, soft carbon, silicon, silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, and spinel-structured lithiated TiO2-Li4Ti5O. 12 Or at least one of Li-Al alloys.
[0054] In this application, the negative electrode material layer may also include a conductive agent. This application does not have any particular limitation on the conductive agent, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of the above-mentioned conductive agents.
[0055] In this application, the negative electrode material layer may also include an adhesive. This application does not have any particular restrictions on the adhesive, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of the above-mentioned adhesives.
[0056] Optionally, the negative electrode may further include a conductive layer located between the negative electrode current collector and the negative electrode material layer. This application does not impose any particular limitation on the composition of the conductive layer; it can be a conductive layer commonly used in the art, and may include, but is not limited to, the aforementioned conductive agent and binder.
[0057] The electrochemical device of this application also includes a separator membrane. This application does not impose any particular limitation on the separator membrane, as long as it achieves the purpose of this application. For example, it can be at least one of the following: polyethylene (PE), polypropylene (PP), polyolefin (PO) membranes primarily composed of polytetrafluoroethylene, polyester membranes (e.g., polyethylene terephthalate (PET) membranes), cellulose membranes, polyimide (PI) membranes, polyamide (PA) membranes, spandex, aramid membranes, woven membranes, nonwoven membranes (non-woven fabrics), microporous membranes, composite membranes, separator paper, rolled membranes, or spun membranes, preferably PP. The separator membrane of this application can have a porous structure, and the pore size is not particularly limited, as long as it achieves the purpose of this application. For example, the pore size can be from 0.01 μm to 1 μm. In this application, the thickness of the separator membrane is not particularly limited, as long as it achieves the purpose of this application. For example, the thickness can be from 5 μm to 500 μm.
[0058] For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, membrane, or composite membrane with a porous structure, and the material of the substrate layer may include, but is not limited to, at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing polymers and inorganic materials.
[0059] The inorganic layer may include, but is not limited to, inorganic particles and inorganic layer binders. This application does not impose any particular limitation on the inorganic particles, as long as they achieve the purpose of this application. For example, they may include, but are not limited to, at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. This application does not impose any particular limitation on the inorganic layer binder. For example, it may include, but is not limited to, at least one of polyvinylidene fluoride, a copolymer of polyvinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene. The polymer layer contains a polymer, and the polymer material may include, but is not limited to, at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, or poly(vinylidene fluoride-hexafluoropropylene).
[0060] In this application, the electrolyte may further include a non-aqueous solvent and a lithium salt. This application does not particularly limit the non-aqueous solvent, as long as it achieves the purpose of this application; for example, it may include, but is not limited to, at least one of carbonate compounds, carboxylic acid ester compounds, ether compounds, or other organic solvents. The aforementioned carbonate compounds may include, but are not limited to, at least one of chain carbonate compounds or cyclic carbonate compounds. The aforementioned chain carbonate compounds may include, but are not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), or methyl ethyl carbonate (MEC). The aforementioned cyclic carbonates may include, but are not limited to, at least one of ethylene carbonate (EC), vinylene carbonate (VC), propylene carbonate (PC), butyl carbonate (BC), or vinyl ethylene carbonate (VEC). The aforementioned carboxylic acid ester compounds may include, but are not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerate, mevalonate lactone, or caprolactone. The aforementioned ether compounds may include, but are not limited to, at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran. The aforementioned other organic solvents may include, but are not limited to, at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, or phosphate esters.
[0061] This application does not impose any particular limitation on the lithium salt, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, LiBOB, or lithium difluoroborate. Preferably, the lithium salt includes LiPF6.
[0062] The electrochemical device described in this application is not particularly limited and may include any device in which an electrochemical reaction occurs. In some embodiments, the electrochemical device may include, but is not limited to, lithium metal secondary batteries, lithium-ion secondary batteries (lithium-ion batteries), lithium polymer secondary batteries, or lithium-ion polymer secondary batteries.
[0063] The preparation process of electrochemical devices is well known to those skilled in the art, and this application does not impose any particular limitations. For example, it may include, but is not limited to, the following steps: stacking the positive electrode, separator, and negative electrode in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain the electrochemical device; or stacking the positive electrode, separator, and negative electrode in sequence, and then fixing the four corners of the entire stacked structure with tape to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain the electrochemical device. In addition, overcurrent protection elements, conductive plates, etc., may be placed in the packaging bag as needed to prevent pressure rise and overcharging / discharging inside the electrochemical device.
[0064] A third aspect of this application provides an electronic device that includes the electrochemical device in any of the foregoing embodiments. The electrochemical device provided by this application has good cycle performance, thereby providing the electronic device with a long service life.
[0065] The electronic device described in this application is not particularly limited and can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, laptops, pen-based computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, and lithium-ion capacitors, etc.
[0066] This application provides a lithium transition metal composite oxide, an electrochemical device, and an electronic device. The lithium transition metal composite oxide has a twinned structure, comprising a first crystalline region and a second crystalline region, with a grain boundary between the first and second crystalline regions. The first crystalline region includes a first area within 20 nm of the grain boundary, and the second crystalline region includes a second area within 20 nm of the grain boundary. The angle between the transition metal layers in the first and second crystalline regions is 65° to 80°. By controlling the angle between the transition metal layers in the first and second regions to 65° to 80°, the stress and strain between the first and second crystalline regions during charge and discharge can be reduced, improving the stability of the twinned structure and thus enhancing the cycle performance of the electrochemical device under high voltage.
[0067] Example
[0068] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.
[0069] Test methods and equipment:
[0070] Capacity retention test:
[0071] In an environment of 25°C, the lithium-ion battery was charged at a constant current of 0.2C until the upper limit voltage reached 4.6V. Then, it was charged at a constant voltage until the current was less than 50μA, and then discharged at a constant current of 0.2C until the final voltage reached 3.0V. The discharge capacity of the first cycle was recorded. Then, the same procedure was repeated for 100 charge and discharge cycles, and the discharge capacity of the 100th cycle was recorded. The capacity retention rate was calculated as (discharge capacity of the 100th cycle / discharge capacity of the first cycle) × 100%.
[0072] Ratio performance test:
[0073] In an environment of 25℃, the lithium-ion battery was charged at a constant current of 0.2C until the upper limit voltage reached 4.6V. Then, it was charged at a constant voltage until the current was less than 50μA, followed by constant current discharge at 0.2C until the final voltage reached 3.0V. The 0.2C discharge capacity was recorded. This constant current and constant voltage charging process was then repeated, followed by constant current discharge at 2C until the final voltage reached 3.0V. The 2C discharge capacity was recorded. Rate performance = 2C discharge capacity / 0.2C discharge capacity × 100%.
[0074] Testing of included angle and elemental content:
[0075] The lithium-ion battery is at 10mA / cm 2The sample was fully discharged to 3.0V at a current density and allowed to stand for 10 minutes before being disassembled in a glove box to obtain the positive electrode. The positive electrode was then transferred to a scanning electron microscope (SEM) equipped with a focused ion beam (model: FEI VionPlasma FIB) to process a sample suitable for transmission scanning electron microscopy (STEM, model: FEI Titan3 G2 60-300). The sample surface was protected with Pt and processed with a Ga ion beam, with a sample thickness not exceeding 100 nm. The sample was then cleaned using a low-voltage mode to remove any residual surface material. The sample was observed under STEM at an appropriate magnification, and an electron microscope image containing lattice fringes of the first region in the first crystal region and the second region in the second crystal region was taken. Image processing software was used to measure the angle between the lattice fringes in the first region and the second region at the grain boundary; this angle represents the angle between the transition metal layers in the first and second regions after full discharge. Simultaneously, data was acquired using X-ray energy dispersive spectroscopy (EDS) at an appropriate magnification to obtain the elemental content of the grain boundaries, the third region within the first region, and the fourth region of the positive electrode active material. Data was collected from at least three different locations, and the average value was taken as the final result.
[0076] A 1.4 cm diameter disc from the above positive electrode is assembled with lithium metal to form a coin cell battery. The electrolyte is the basic electrolyte in Example 1-1 below, with an injection volume of 50 μL. The coin cell battery is charged and discharged to 4.5V and 4.7V respectively. The coin cell battery is disassembled, and the above steps are repeated to measure the angle between the transition metal layer in the first region and the transition metal layer in the second region, thereby calculating |β-α|.
[0077] The content of different elements in the positive electrode active material was tested using an inductively coupled plasma optical generator.
[0078] Figure 1 A scanning electron microscope (SEM) image of the cross-section of the positive electrode sheet in Example 1-1 is shown. Figure 2 The image shows a scanning electron microscope (SEM) image of a lithium transition metal composite oxide with a twinned structure in the cross-section of the positive electrode sheet in Example 1-1. As can be seen from the image, the positive electrode active material contains lithium transition metal composite oxide particles with a twinned structure. Figure 3 The image shows a transmission electron microscope (TEM) image of the lithium transition metal composite oxide obtained after the electrochemical device in Example 1-1 was fully disassembled and the positive electrode was obtained. The positive electrode was then assembled with lithium metal to form a coin cell and charged to 4.7V. The angle β between the transition metal layer in the first region and the transition metal layer in the second region is 78°.
[0079] First layer thickness test:
[0080] The sample was observed under STEM. At an appropriate magnification, electron microscope images of the particle edges including the first layer were taken. Five measurement points were randomly selected on the surface of the first layer. The minimum distance from each measurement point to the substrate surface was measured using image processing software. The average value was taken as the thickness of the first layer.
[0081] Particle count percentage test:
[0082] In the cross-sectional photograph of the positive electrode sheet, a region with a length of 500 μm is randomly selected, and the proportion of positive electrode active material particles with twinned structures in the region is counted as the particle count percentage.
[0083] Second crystal region area ratio test:
[0084] The sample was observed under STEM. At an appropriate magnification, electron microscope images of the cross-section were taken. The area of the second crystal region was calculated as S2, the total area of the cross-section was S, and the area ratio of the second crystal region was S2 / S.
[0085] Example 1-1
[0086] <Preparation of Positive Electrode Active Materials>
[0087] (1) Prepare an aqueous solution by mixing CoSO4, MgSO4 and Al(NO3)3 in a Co, Mg and Al molar ratio of 98.2:0.8:1. Add ammonia and ammonium carbonate to adjust the pH to above 8.5 and obtain carbonate precipitate through precipitation process. Bake in an oven at 60℃, and control the water content of the carbonate precipitate to be not less than 7%. Then put it into a muffle furnace and calcine it once in an air atmosphere. The calcine temperature T1 is 750℃, the calcine time t1 is 12h, and the air flow rate is 10L / min. Then grind and sieve to obtain the first intermediate product.
[0088] (2) The first intermediate product was mixed with Li2CO3 and placed in a muffle furnace for secondary calcination in air atmosphere. The calcination temperature T2 was 1000℃, the calcination time t2 was 12h, and the air flow rate was 10L / min. Then, the mixture was ground and sieved to obtain the second intermediate product. The ratio of the number of moles of Li in Li2CO3 to the sum of the number of moles of Co, Mg and Al was 1.05:1.
[0089] (3) The second intermediate product was mixed with Al2O3 and MgO in a mass ratio of 100:0.1:0.05 and placed in a muffle furnace. The mixture was then calcined three times in an air atmosphere. The calcination temperature T3 was 600℃, the calcination time t3 was 8h, and the air flow rate was 10L / min. The positive electrode active material was then obtained by grinding and sieving.
[0090] <Preparation of the positive electrode>
[0091] The positive electrode active material, conductive carbon black (conductive agent), and polyvinylidene fluoride (PVDF) binder were mixed in a mass ratio of 97:1.4:1.6. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 70%. The positive electrode slurry was uniformly coated onto one surface of a positive electrode current collector aluminum foil and dried to obtain a positive electrode sheet with a single-sided coating of the positive electrode material. The above steps were repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of the positive electrode material. The positive electrode sheet was then cold-pressed and cut to obtain the final positive electrode sheet.
[0092] <Preparation of Negative Electrode Sheets>
[0093] Artificial graphite (negative electrode active material), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (thickener) (mass ratio 97:2:1) were mixed with deionized water and stirred evenly under vacuum to obtain a negative electrode slurry with a solid content of 75%. The negative electrode slurry was uniformly coated onto one surface of a copper foil current collector and dried to obtain a negative electrode sheet with a single-sided coating of negative electrode material. The above steps were repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of negative electrode material. Finally, the negative electrode sheet was obtained after cold pressing and cutting.
[0094] <Preparation of Electrolyte>
[0095] In a dry argon-atmospheric glove box, PC, EC, and DEC were mixed in a mass ratio of 1:1:1 to obtain an organic solvent. Lithium salt LiPF6 was then added to the organic solvent, dissolved, and mixed thoroughly to obtain the basic electrolyte. The mass concentration of LiPF6 in the electrolyte was 12.5%.
[0096] <Preparation of the separating membrane>
[0097] A porous PE film with a thickness of 7μm was used.
[0098] <Preparation of Lithium-ion Batteries>
[0099] The positive electrode, separator, and negative electrode prepared above are stacked in sequence and wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, degassing, and edge trimming, a lithium-ion battery is obtained.
[0100] Examples 1-2
[0101] Except for the following steps in the <Preparation of Positive Electrode Active Material>: (1) Co, Mg, Al molar ratio is 97:0.8:2.2, pH is adjusted to above 8.9, T1 is 780℃, (2) T2 is 1050℃, t2 is 16h, and (3) the mass ratio of the second intermediate product to Al2O3 and MgO is 100:0.1:0.5, the rest are the same as in Example 1-1.
[0102] Examples 1-3
[0103] Except for the fact that in step (1) of the <Preparation of Positive Electrode Active Material>, the molar ratio of Co, Mg, and Al is 99:0.3:0.7, T1 is 550℃, and t1 is 6h, and in step (3) the mass ratio of the second intermediate product to Al2O3 and MgO is 100:0.1:0.5, the rest is the same as in Example 1-1.
[0104] Example 2-1
[0105] Except for the fact that in step (1) of the <Preparation of Positive Electrode Active Material>, the molar ratio of Co, Mg, and Al is 98.7:0.3:1 and 0.5% of MgO is added during the first calcination, and the mass ratio of the second intermediate product to Al2O3 and MgO in step (3) is 100:0.1:0.1, the rest is the same as in Example 1-1.
[0106] Example 2-2
[0107] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4 and Al(NO3)3 are mixed in an aqueous solution at a Co:Al molar ratio of 99:1 and MgO is added during the first calcination, and in step (3) the mass ratio of the second intermediate product to Al2O3 and MgO is 100:0.1:0.15, the rest is the same as in Example 1-1.
[0108] Example 2-3
[0109] Except for step (1) of the <Preparation of Positive Electrode Active Material>, where the molar ratio of Co, Mg, and Al is 98.5:0.5:1, the rest is the same as in Example 1-1.
[0110] Examples 2-4
[0111] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4 and TiO2 are mixed at a Co:Ti molar ratio of 99.7:0.3, and in step (3) in which the second intermediate product is mixed with TiO2 at a mass ratio of 100:0.05, the rest is the same as in Example 1-1.
[0112] Examples 2-5
[0113] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4 and Nb2O5 are mixed at a Co:Nb molar ratio of 99.7:0.3, and in step (3) in which the second intermediate product is mixed with Nb2O5 at a mass ratio of 100:0.01, the rest is the same as in Example 1-1.
[0114] Examples 2-6
[0115] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4 and ZnSO4 are mixed at a Co:Zn molar ratio of 99.7:0.3, and in step (3) in which the second intermediate product is mixed with ZnO at a mass ratio of 100:0.01, the rest is the same as in Example 1-1.
[0116] Examples 2-7
[0117] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4 and NH4F are mixed at a Co:F molar ratio of 99.7:0.3, and in step (3) in which the second intermediate product is mixed with NH4F at a mass ratio of 100:0.01, the rest is the same as in Example 1-1.
[0118] Examples 2-8
[0119] Except for step (1) of the <Preparation of Positive Electrode Active Material>, in which CoSO4, MgSO4, Al(NO3)3 and NH4F are mixed in a Co, Mg, Al and F molar ratio of 99.5:0.1:0.1:0.3, the rest is the same as in Example 1-1.
[0120] Example 3-1
[0121] Except for step (2) of the <Preparation of Positive Active Material>, where T2 is 950°C, t2 is 6h, and air flow rate is 5L / min, the rest is the same as in Example 1-1.
[0122] Example 3-2
[0123] Except for the fact that in step (1) of the <Preparation of Positive Electrode Active Material>, T1 is 800℃ and t1 is 18h, and in step (2) T2 is 1050℃ and the ratio of the number of moles of Li in Li2CO3 to the sum of the number of moles of Co, Mg and Al is 1.06:1, the rest is the same as in Example 1-1.
[0124] Example 4-1
[0125] Except for the step of <Preparation of Electrolyte>, in which ethylene monofluorocarbonate (FEC) is further added to the basic electrolyte, wherein the mass percentage of FEC is 0.5% based on the total mass of the electrolyte, the rest is the same as in Example 1-1.
[0126] Example 4-2
[0127] Except for the step of <Preparation of Electrolyte>, in which ethylene monofluorocarbonate (FEC) and ethylene difluorocarbonate (DFEC) are further added to the basic electrolyte, wherein the mass percentage of FEC is 2.5% and the mass percentage of DFEC is 2.5% based on the total mass of the electrolyte, the rest is the same as in Example 1-1.
[0128] Example 4-3
[0129] Except for the step of <Preparation of Electrolyte>, in which ethylene monofluorocarbonate (FEC) and ethylene difluorocarbonate (DFEC) are further added to the basic electrolyte, wherein the mass percentage of FEC is 5% and the mass percentage of DFEC is 5% based on the total mass of the electrolyte, the rest is the same as in Example 1-1.
[0130] Comparative Example 1-1
[0131] Except for the steps of preparing the positive electrode active material, the rest is the same as in Example 1-1:
[0132] (1) Prepare an aqueous solution by mixing CoSO4, MgSO4 and Al(NO3)3 in a Co, Mg and Al molar ratio of 98.2:0.8:1. Add ammonia and ammonium carbonate to adjust the pH to above 8.0 and obtain carbonate precipitate through precipitation process. Bake in an oven at 60℃, and control the water content of the carbonate precipitate to be not less than 7%. Then put it into a muffle furnace and calcine it once in an air atmosphere. The calcine temperature T1 is 720℃, the calcine time t1 is 12h, and the air flow rate is 10L / min. Then grind and sieve to obtain the first intermediate product.
[0133] (2) The first intermediate product was mixed with Li2CO3 and placed in a muffle furnace for secondary calcination in air atmosphere. The calcination temperature T2 was 950℃, the calcination time t2 was 12h, and the air flow rate was 10L / min. Then, the mixture was ground and sieved to obtain the positive electrode active material. The ratio of the number of moles of Li in Li2CO3 to the sum of the number of moles of Co, Mg and Al was 1.05:1.
[0134] Comparative Examples 1-2
[0135] Except for the steps of preparing the positive electrode active material, the rest is the same as in Example 1-1:
[0136] (1) Prepare an aqueous solution by mixing CoSO4, MgSO4 and Al(NO3)3 in a Co, Mg and Al molar ratio of 98.2:0.8:1. Add ammonia and ammonium carbonate to adjust the pH to above 8.5 and obtain carbonate precipitate through precipitation process. Bake in an oven at 120℃, and control the water content of the carbonate precipitate to be not less than 7%. Then put it into a muffle furnace and calcine it once in an air atmosphere. The calcine temperature T1 is 950℃, the calcine time t1 is 8h, and the air flow rate is 30L / min. Then grind and sieve to obtain the first intermediate product.
[0137] (2) The first intermediate product was mixed with LiOH and placed in a muffle furnace for secondary calcination in air atmosphere. The calcination temperature T2 was 900℃, the calcination time t2 was 12h, and the air flow rate was 30L / min. Then, the mixture was ground and sieved to obtain the positive electrode active material. The ratio of the number of moles of Li in LiOH to the sum of the number of moles of Co, Mg and Al was 1.05:1.
[0138] The test results of each embodiment and comparative example are shown in Tables 1 to 4.
[0139] Table 1
[0140]
[0141] As can be seen from Examples 1-1 to 1-3, Comparative Examples 1-1 and 1-2, when the included angle of the lithium transition metal composite oxide is within the range of this application, the resulting lithium-ion battery exhibits better cycle performance at high voltage than the lithium-ion battery obtained in the comparative examples. Figure 4 As can be seen, during the cycling process, the capacity retention rate of Example 1-1 is consistently higher than that of Comparative Example 1-1; and after 100 cycles, the capacity retention rate of Example 1-1 is significantly higher than that of Comparative Example 1-1. This is because the angle between the first and second transition metal layers is within the aforementioned range, which reduces the stress and strain between the first and second crystal regions during charging and discharging, thereby improving the stability of the twinned structure and thus enhancing the cycling performance of the electrochemical device at high voltage. From Examples 1-1 to 1-3, Comparative Example 1-1, and Comparative Example 1-2, it can also be seen that the lithium transition metal composite oxides in Examples 1-1 to 1-3 exhibit smaller angle changes at 4.7V and 4.5V |(β-α)|, indicating that the lithium transition metal composite oxides in these examples exhibit smaller strain between the first and second crystal regions during the high-voltage segment of the charging and discharging process, resulting in better stability of the twinned structure.
[0142] As can also be seen from Table 1, the rate performance of Examples 1-1 to 1-3 is better than that of Comparative Examples 1-1 and 1-2. This is because when the angle between the transition metal layers of the first region and the second region is within the above range, the barrier for lithium ion transfer at this interface is lower and the transmission impedance is smaller, thereby improving the dynamic performance of the twin structure and thus enabling the lithium-ion battery to have better rate performance.
[0143] Table 2
[0144]
[0145] As can be seen from Examples 1-1, 2-1 to 2-8, when X / Y ≥ 2, the resulting lithium-ion battery exhibits good cycle performance. This is because the first crystal region has a relatively high amount of element A near the grain boundaries, which is more conducive to improving the structural stability of the first crystal region near the grain boundaries and reducing the risk of twin structure cracking, thereby improving the structural stability of lithium transition metal composite oxides under high voltage. Furthermore, it can be seen that when element A includes element F, the resulting lithium-ion battery has even better cycle performance. This is because element A includes F, which, on the one hand, can form a local disordered structure, dispersing stress and thus reducing the risk of twin structure cracking; on the other hand, it can improve the stability of the O structure at the grain boundaries and reduce the risk of degradation at the grain boundaries.
[0146] Table 3
[0147] 4.7V angle β Percentage of particles (%) Capacity retention rate (%) Ratio performance (%) Example 1-1 78 55 80 93 Example 3-1 78 36 70 86 Example 3-2 78 73 72 95
[0148] As can be seen from Examples 1-1, 3-1 and 3-2, when the proportion of positive electrode active material particles with twinned structures is within the range of this application, the resulting lithium-ion battery can have both good cycle performance and rate performance.
[0149] Table 4
[0150]
[0151] As can be seen from Examples 1-1, 4-1 to 4-3, the addition of fluorinated carbonate compounds to the electrolyte can further improve the cycle performance of lithium-ion batteries at high voltages. This is because, on the one hand, during charging and discharging, the surface of the positive electrode active material particles can react with the fluorinated carbonate compounds to form a protective layer of metal fluorides, improving the stability of the surface structure of the positive electrode active material particles; on the other hand, the introduction of fluorinated carbonate compounds can form a protective layer at the interface where the twinned structure breaks, reducing the side reactions between lithium transition metal composite oxides and the electrolyte, thereby improving the cycle performance of the electrochemical device.
[0152] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.
Claims
1. An electrochemical device comprising a positive electrode, said positive electrode comprising a positive electrode material layer, said positive electrode material layer comprising a positive electrode active material, said positive electrode active material comprising a lithium transition metal composite oxide, wherein, The lithium transition metal composite oxide has a twinned structure, which includes a first crystal region and a second crystal region, with a grain boundary between the first crystal region and the second crystal region. The first crystal region includes a first region within 20 nm of the grain boundary, and the second crystal region includes a second region within 20 nm of the grain boundary. The angle between the transition metal layer in the first region and the transition metal layer in the second region is 65° to 80°. The transition metal layer in the first region includes at least one of Co, Mn, or Ni. The transition metal layer in the second region includes at least one of Co, Mn, or Ni. The grain boundary contains element A, which includes at least one of Mg, Al, Ti, Zr, La, Nb, Hf, Zn, Y, or F.
2. The electrochemical device according to claim 1, wherein, The first region includes a third region within 10 nm of the grain boundary and a fourth region between 10 nm and 20 nm of the grain boundary. Based on the total number of moles of Co, Mn, and Ni in the third region, the molar percentage of element A in the third region is X; based on the total number of moles of Co, Mn, and Ni in the fourth region, the molar percentage of element A in the fourth region is Y, satisfying: X / Y≥2.
5.
3. The electrochemical device according to claim 2, wherein, X ranges from 0.2% to 2.5%.
4. The electrochemical device according to claim 1, wherein, In the cross-section of the lithium transition metal composite oxide, the area of the second crystal region accounts for 30% to 60% based on the area of the cross-section.
5. The electrochemical device according to claim 1, wherein, The lithium transition metal composite oxide includes a matrix and a first layer located on the surface of the matrix, the first layer comprising a metal fluoride.
6. The electrochemical device according to claim 5, wherein, The lithium transition metal composite oxide satisfies at least one of the following characteristics: (a) The metal fluoride includes at least one of CoF2, CoF3, MgF2, NaF, or AlF3; (b) The thickness of the first layer is 1 nm to 8 nm.
7. The electrochemical device according to claim 1, wherein, The electrochemical device is disassembled after being fully filled to obtain the positive electrode. Two circular pieces with a diameter of 1.4 cm from the positive electrode are taken and assembled with lithium metal to form a first coin cell and a second coin cell, respectively. The first coin cell is charged to 4.5V and the second coin cell is charged to 4.7V. In the first coin cell, the included angle of the lithium transition metal composite oxide is α; in the second coin cell, the included angle of the lithium transition metal composite oxide is β, satisfying: |β-α|≤5°.
8. The electrochemical device according to claim 7, wherein, β ranges from 70° to 86°.
9. The electrochemical device according to claim 1, wherein, Based on the number of particles of the positive electrode active material, the proportion of positive electrode active material particles with twinned structures is 35% to 75%.
10. The electrochemical device according to claim 1, further comprising an electrolyte comprising a fluorocarbonate compound, wherein the fluorocarbonate compound comprises 0.05% to 15% by mass based on the mass of the electrolyte.
11. The electrochemical device according to claim 10, wherein the fluorocarbonate compound comprises at least one selected from the following: monofluoroethylene carbonate, difluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate.
12. An electronic device comprising the electrochemical device according to any one of claims 1 to 11.
Citation Information
Patent Citations
High-voltage lithium ion battery with excellent high-low temperature performance
CN111900480A
Lithium nickel manganese oxide, its manufacturing method and lithium-ion secondary cell using the same
JP2004002141A