Method for the preparation of metal-loaded porous carbon-based nanoplatelet composites, products thereof and uses thereof
The preparation of metal-loaded porous carbon-based nanosheet composite materials by solid-phase ball milling and high-temperature pyrolysis technology solves the problem of cumbersome preparation of non-platinum metal ORR electrocatalysts, and achieves efficient and stable oxygen reduction reaction electrocatalytic performance, which is convenient for large-scale application in fuel cells and metal-air batteries.
Patent Information
- Application Number
- CN202310853884.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-07-12
AI Technical Summary
In the existing technology, the preparation process of non-platinum metal oxygen reduction reaction (ORR) electrocatalysts is complicated, which limits their application in fuel cells and metal-air batteries. In addition, platinum material resources are limited and costly.
A method combining solid-phase ball milling and high-temperature pyrolysis was used to prepare metal-loaded porous carbon-based nanosheet composites. By ball milling and segmented pyrolysis of EDTA salt and phthalocyanine salt, highly dispersed nanomaterials were formed, avoiding the agglomeration and loss of nanoparticles caused by the liquid-phase method.
The prepared material exhibits excellent electrocatalytic activity and stability in the oxygen reduction reaction, simplifies the preparation process, facilitates large-scale production, and is suitable for fuel cells and metal-air batteries.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical energy materials, specifically relating to the preparation and application of a metal-loaded porous carbon-based nanosheet composite material. Background Technology
[0002] Fuel cells and metal-air batteries are next-generation green energy devices and electrochemical new energy technologies that the country is vigorously developing, with extremely broad application prospects. Regardless of whether it's a fuel cell or a metal-air battery, their cathode processes involve the oxygen reduction reaction (ORR). Since ORR is a kinetically slow process, it requires materials with strong electrocatalytic activity to proceed effectively. Currently, the most active materials for ORR electrocatalysis are still platinum or platinum-based substances. However, due to the limited resources and extremely uneven distribution of platinum, its use is very expensive, severely limiting the large-scale practical application of fuel cells and metal-air batteries. Therefore, developing non-platinum metal ORR electrocatalysts with electroactivity comparable to platinum catalysts is of great significance for the practical application of electrochemical new energy.
[0003] Currently, although extensive research and development have been conducted on non-precious metal ORR electrocatalysts, their preparation processes are generally too cumbersome, hindering practical applications. Therefore, developing new technologies with superior performance, stability, reliability, simple preparation processes, and ease of large-scale production is crucial for the practical application of these catalysts. This invention combines solid-phase ball milling with high-temperature pyrolysis technology to prepare highly dispersed nanomaterials through simple steps, avoiding the agglomeration of nanoparticles caused by liquid-phase methods and losses due to various separation and filtration processes. The material of this invention exhibits excellent ORR electrocatalytic activity and stable performance, making it applicable to fuel cells and metal-air batteries, and possessing significant practical value. Summary of the Invention
[0004] The purpose of this invention is to provide a metal-loaded porous carbon-based nanosheet composite material, and also to provide a method for preparing and applying the metal-loaded porous carbon-based nanosheet composite material.
[0005] To achieve the above objectives, the embodiment of the present invention is as follows: a method for preparing a metal-loaded porous carbon-based nanosheet composite material, comprising the following steps: (1) Add EDTA salt to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. Ball mill at 400 r / min for 6 hours. Then add phthalocyanine salt to the agate jar and continue ball milling the mixture at 400 r / min for 6 hours. After that, take out the solid mixture, add ethanol, stir and filter. Repeat this process 2-3 times to remove the ethylene glycol. Finally, dry at 50°C for 6 hours to obtain precursor-1. The EDTA salt includes disodium EDTA or dipotassium EDTA; The phthalocyanine salts include iron phthalocyanine or cobalt phthalocyanine; The mass ratio of EDTA salt to phthalocyanine salt is 10:(0.5 ~ 5).
[0006] (2) Mix precursor-1, F127, organic carbon source and dicyandiamide, grind thoroughly and evenly in an appropriate amount of ethanol, and then dry at 50°C for 2 hours to obtain precursor-2. F127 refers to a copolymer of propylene oxide and ethylene oxide; The organic carbon source refers to glucose, sucrose, or starch; The mass ratio of precursor-1, F127, organic carbon source and dicyandiamide is 1:(0 ~ 0.2):(0 ~ 0.2):(0 ~ 1).
[0007] (3) Place precursor-2 in a boat-shaped crucible and transfer it to a tube furnace. Under a nitrogen atmosphere, heat it to 100°C at a heating rate of 4°C / min and hold it at this temperature for 1 hour. Then raise the temperature to 260°C and hold it at this temperature for 1 hour. Continue to raise the temperature to 500°C and hold it at this temperature for 1 hour. Then raise the temperature to 800°C and hold it at this temperature for 2 hours. Finally, cool it to room temperature. The resulting black powder is called precursor-3. (4) Add precursor-3 to a 0.5 M H2SO4 solution at 50℃ and keep stirring for 1 hour. Then filter, wash twice with water, and finally wash once with ethanol. The resulting solid is dried at 50℃ for 3 hours and then ground to obtain the sample.
[0008] A metal-loaded porous carbon-based nanosheet composite material prepared according to the method described above.
[0009] Application of a metal-loaded porous carbon-based nanosheet composite material prepared by the method described above in the electrocatalysis of oxygen reduction reaction.
[0010] This invention first fully disperses EDTA salt in a high-energy planetary ball mill to form nano-sized fine particles. The energy generated during the ball milling process is absorbed by ethylene glycol with a certain viscosity, thus stabilizing the nanoparticles. Subsequently, ball milling further breaks down phthalocyanine salt molecules, creating fragment groups that come into full contact with the nano-sized EDTA salt. EDTA's strong coordination ability allows it to bind with these fragment groups, stabilizing the particles. Next, staged pyrolysis is performed in the presence of a carbon source and a pore-forming agent: a low-temperature stage allows the pore-forming agent and EDTA to be fully dispersed in the solid mixture; a medium-temperature stage allows dicyandiamide to form a carbon-based sheet template; and a final high-temperature stage forms a graphitized sheet-like carbon-based composite. The material of this invention exhibits stable electrocatalytic performance for oxygen reduction reactions, and the process is simple and easy to scale up, showing broad application prospects in fuel cells and metal-air batteries. Implementation
[0011] Example
[0012] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 0.5 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1, 0.2 g of F127, 0.2 g of glucose and 10 g of dicyandiamide were mixed and ground evenly in an appropriate amount of ethanol. Then the mixture was dried at 50°C for 2 hours to obtain precursor-2. (3) Place the above precursor-2 in a boat-shaped crucible and transfer it to a tube furnace. Under a nitrogen atmosphere, heat it to 100°C at a heating rate of 4°C / min and hold it at this temperature for 1 hour. Then raise the temperature to 260°C and hold it at this temperature for 1 hour. Continue to raise the temperature to 500°C and hold it at this temperature for 1 hour. Then raise the temperature to 800°C and hold it at this temperature for 2 hours. Finally, cool it to room temperature. The resulting black powder is called precursor-3. (4) Add precursor-3 to a 0.5 M H2SO4 solution at 50℃ and keep stirring for 1 hour. Then filter, wash twice with water, and finally wash once with ethanol. The resulting solid is dried at 50℃ for 3 hours and then ground to obtain the sample.
[0013] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.48 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.41 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 4.3 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.10 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.18 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 0.44 mA / cm². 2 .
[0014] Example
[0015] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1, 0.25 g of F127, 0.25 g of glucose and 10 g of dicyandiamide were mixed and ground evenly in an appropriate amount of ethanol. Then the mixture was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0016] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.51 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.44 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 5.5 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.09 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.15 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.4 mA / cm². 2 .
[0017] Example
[0018] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 5 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1, 0.3 g of F127, 0.3 g of glucose and 12 g of dicyandiamide were mixed and ground evenly in an appropriate amount of ethanol. Then the mixture was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0019] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.55 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.44 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 6.1 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.06 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.13 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.8 mA / cm². 2 .
[0020] Example
[0021] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of EDTA dipotassium salt was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1, 0.25 g of F127 and 10 g of dicyandiamide were mixed and ground evenly in an appropriate amount of ethanol. Then the mixture was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0022] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.52 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.40 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 5.7 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.1 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.17 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.6 mA / cm². 2 .
[0023] Example
[0024] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1, 0.25 g of F127 and 0.25 g of glucose were mixed and ground evenly in an appropriate amount of ethanol. Then the mixture was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0025] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.47 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.39 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 5.4 mA / cm². 2In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.1 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.18 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.2 mA / cm². 2 .
[0026] Example
[0027] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1 was mixed with 0.25 g of F127 and ground evenly in an appropriate amount of ethanol. Then it was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0028] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.48 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.37 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 5.1 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.11 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.18 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 4.8 mA / cm². 2 .
[0029] Example
[0030] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of EDTA dipotassium salt was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) Mix the above precursor-1 with 10 g of dicyandiamide, grind it thoroughly with an appropriate amount of ethanol, and then dry it at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0031] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.54 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.43 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 6.1 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.07 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.12 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.8 mA / cm². 2 .
[0032] Example
[0033] A method for preparing a metal-loaded porous carbon-based nanosheet composite material includes the following steps: (1) 10 g of disodium EDTA was added to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol. The mixture was ball-milled at 400 r / min for 6 hours. Then, 2 g of phthalocyanine salt was added to the agate jar, and the mixture was ball-milled at 400 r / min for 6 hours. The solid mixture was then removed, ethanol was added, and the mixture was stirred and filtered. The ethylene glycol was removed after the mixture was filtered and the reaction was repeated 2-3 times. Finally, the mixture was dried at 50°C for 6 hours to obtain precursor-1. (2) The above precursor-1 was mixed with 0.25 g of glucose and ground thoroughly in an appropriate amount of ethanol. Then it was dried at 50°C for 2 hours to obtain precursor-2. (3) and (4) are the same as steps (3) and (4) in Example 1.
[0034] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.50 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.42 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 5.7 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.1 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.12 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.6 mA / cm². 2 .
[0035] Example
[0036] Replace iron phthalocyanine in Example 3 with iron phthalocyanine, and the other steps are the same as in Example 3 (1), (2), (3) and (4).
[0037] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.55 V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.46 V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 6.2 mA / cm². 2 In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.04 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.11 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 6.0 mA / cm². 2 .
[0038] Example
[0039] Replace iron phthalocyanine in Example 7 with iron phthalocyanine, and the other steps are the same as in Example 7 (1), (2), (3) and (4).
[0040] (5) The electrocatalytic activity of the oxygen reduction reaction of the sample was tested in a conventional three-electrode system. The results are as follows: In 0.1M HClO4 solution, the onset potential of the oxygen reduction reaction was 0.56V (vs Ag / AgCl, sat.KCl), the half-wave potential of the oxygen reduction reaction was 0.45V (vs Ag / AgCl, sat.KCl), and the limiting current density of the oxygen reduction reaction was 6.1 mA / cm². 2In 0.1 M NaOH solution, the onset potential of the oxygen reduction reaction is -0.05 V (vs Ag / AgCl, sat.KCl), the half-wave potential is -0.12 V (vs Ag / AgCl, sat.KCl), and the limiting current density is 5.9 mA / cm². 2 .
Claims
1. A method for preparing a metal-loaded porous carbon-based nanosheet composite material, characterized in that, Includes the following steps: (1) Add EDTA salt to the agate jar of a high-energy planetary ball mill, along with agate grinding balls and an appropriate amount of ethylene glycol, and ball mill at 400 r / min. Then add phthalocyanine salt to the agate jar and continue ball milling the mixture at 400 r / min. After that, take out the solid mixture, add ethanol, stir and filter. After repeated filtration, replace the ethylene glycol in the mixture. Finally, dry at 50°C to obtain precursor-1. The EDTA salt includes disodium EDTA or dipotassium EDTA; The phthalocyanine salts include iron phthalocyanine or cobalt phthalocyanine; The mass ratio of EDTA salt to phthalocyanine salt is 10:(0.5 ~ 5); (2) Mix precursor-1, F127, organic carbon source and dicyandiamide, grind thoroughly and evenly in an appropriate amount of ethanol, and then dry at 50°C for 2 hours to obtain precursor-2. F127 refers to a copolymer of propylene oxide and ethylene oxide; The organic carbon source refers to glucose, sucrose, or starch; The mass ratio of precursor-1, F127, organic carbon source and dicyandiamide is 1:(0 ~ 0.2):(0 ~ 0.2):(0 ~ 1); (3) Place precursor-2 in a boat-shaped crucible and transfer it to a tube furnace. Under a nitrogen atmosphere, heat it to 100°C at a heating rate of 4°C / min and hold it at this temperature for 1 hour. Then raise the temperature to 260°C and hold it at this temperature for 1 hour. Continue to raise the temperature to 500°C and hold it at this temperature for 1 hour. Then raise the temperature to 800°C and hold it at this temperature for 2 hours. Finally, cool it to room temperature. The resulting black powder is called precursor-3. (4) Add precursor-3 to a 0.5 M H2SO4 solution at 50℃, stir continuously, filter, wash with water, and finally wash with ethanol. Dry the resulting solid at 50℃, grind it, and obtain the sample.
2. A metal-loaded porous carbon-based nanosheet composite material prepared according to claim 1.
3. The application of a metal-loaded porous carbon-based nanosheet composite material prepared according to claim 1 in the electrocatalysis of oxygen reduction reaction.
Citation Information
Patent Citations
Oxygen reduction catalyst with high substance transfer rate and preparation method and application thereof
CN115101760A
Method for pre-treating biological waste