A method for preparing a borohydride-based solid electrolyte doped with fluorine element in situ

By in-situ doping fluorine into borohydride-based solid electrolytes, nanoscale fluorides are generated, solving the compatibility problem between the electrolyte and the electrode, improving the electrochemical performance of all-solid-state batteries, and making them suitable for large-scale production.

CN116826154BActive Publication Date: 2026-11-24UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310865996.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2026-11-24
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

Existing borohydride-based solid electrolytes cannot generate nanoscale fluorides in situ at the electrolyte/electrode interface, leading to compatibility issues with lithium metal anodes and high-voltage cathodes. This affects the lithium dendrites and interface impedance of all-solid-state batteries, limiting their commercial application.

Method used

In-situ doping of fluorine in borohydride is achieved by mixing borohydride-based solid electrolyte with fluoride and then heating the mixture. Fluoride is generated in-situ at the electrolyte/electrode interface. The mixing method is manual grinding, mechanical ball milling or mechanical vibration. The heating and holding temperature is controlled between 100 and 500°C and the time is 0.1 to 20 hours.

Benefits of technology

The nanoscale doping of fluorine in borohydride-based solid electrolytes has been achieved, which improves the compatibility between the electrolyte and the electrode, enhances the operating voltage and cycle performance of all-solid-state batteries, and makes them suitable for large-scale commercial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116826154B_ABST
    Figure CN116826154B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a fluorine-doped borohydride-based solid electrolyte, comprising the following steps: (1) mixing a borohydride-based solid electrolyte and a fluoride compound to obtain a mixture; (2) heating and holding the mixture to obtain a fluorine-doped borohydride-based solid electrolyte. This invention, employing the above-described method for preparing a fluorine-doped borohydride-based solid electrolyte, achieves fluorine doping in borohydrides and enables in-situ generation of fluorides at the electrolyte / electrode interface, thus solving the compatibility problem of borohydride-based solid electrolytes with electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of all-solid-state battery electrolyte technology, and in particular to a method for preparing a fluorine-doped borohydride-based solid electrolyte. Background Technology

[0002] Solid electrolytes are mainly classified into oxide, sulfide, chloride, and hydride types. Among them, solid electrolytes represented by lithium lanthanum zirconium oxide, lithium germanium phosphorus sulfide, and lithium carbon boron hydride can achieve ionic conductivity of up to 10 at room temperature. -3 ~10 -2 Scm -1 Its value has approached or even exceeded that of liquid electrolytes, basically meeting the requirements for electrolyte conductivity in commercial batteries. However, in the process of developing practical all-solid-state batteries, it has been realized that interface problems between the solid electrolyte and the positive and negative electrode materials can seriously affect the overall performance of all-solid-state batteries, such as interfacial impedance and dendrite growth. Therefore, to achieve high energy density and long-cycle stability in all-solid-state batteries, the interface problem between the solid electrolyte and the positive and negative electrode materials is crucial.

[0003] Borohydrides, as a relatively new class of solid electrolyte materials, have attracted considerable attention. See Halide-stabilized LiBH4, a room-temperature lithium fast-ion conductor. 2009, Journal of American Chemical Society, 2009, 131:894-5. Maekawa et al. found that the high-temperature phase of lithium borohydride can be stabilized at room temperature by adding lithium halides, and pointed out that it is stable above 40 mA cm⁻¹. -2 Even at high current densities, the lithium metal / lithium borohydride interface remains stable. (See *All-solid-state lithium battery with LiBH4 solidelectrolyte*. *Journal of Power Sources*, 2013, 226:61-4). Takahashi et al. found that lithium borohydride reacts with charged lithium cobalt oxide to form LiBO2, Li2O, Co3O4, and CoO(OH), causing increased interfacial impedance and battery failure. They effectively suppressed the interfacial reaction by depositing a 25nm thick layer of lithium phosphate on the surface of lithium cobalt oxide using pulsed laser deposition.

[0004] Fluorides exhibit high electrochemical stability; for example, lithium fluoride is stable to almost all electrode materials. Furthermore, their high ratio of ionic to electronic conductivity is beneficial for reducing interfacial impedance. However, the absolute value of ionic conductivity in fluorides is relatively low, requiring them to be present at the nanoscale to exert their ionic conductivity. Therefore, achieving in-situ generation of nanoscale fluorides at the electrolyte / electrode interface through fluorine doping in borohydride-based solid electrolytes is crucial for advancing the practical application of borohydride-based solid electrolytes.

[0005] The existing methods for fluorinating borohydride-based solid electrolytes include the following: (1) See Inside or Outside: Origin of Lithium Dendrite Formation of All Solid-State Electrolytes. Advanced Energy Materials, 2019, 9, 1902123, where LiBH4 is directly mixed with LiF and ball-milled. This method does not involve in-situ reaction and cannot achieve in-situ generation of nanoscale fluorides at the electrolyte / electrode interface; (2) See In situ forming LiF nanodecorated electrolyte / electrode interfaces for stable all-solid-state batteries. Materials Today Nano, 2020, 10, 100079, where LiBH4 and LiBF4 are reacted in situ. This method uses in-situ reaction, but the product generated is Li2B. 12 H 12 Unlike LiF, where fluorine is not incorporated into the borohydride lattice, in-situ generation of nanoscale fluorides at the electrolyte / electrode interface is also impossible. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing a fluorine-doped borohydride-based solid electrolyte, in order to solve the problem that the aforementioned borohydride-based solid electrolyte cannot be well compatible with both a lithium metal anode and a high-voltage cathode, resulting in lithium dendrite formation and interface impedance issues in all-solid-state batteries, which seriously affect their large-scale commercial application.

[0007] To achieve the above objectives, the present invention provides a method for preparing a fluorine-doped borohydride-based solid electrolyte, comprising the following steps: (1) A mixture is obtained by mixing a borohydride-based solid electrolyte and a fluoride; (2) The mixture is heated and kept at a constant temperature to obtain a fluorine-doped borohydride-based solid electrolyte.

[0008] Preferably, the borohydride-based solid electrolyte in step (1) is LiBH4 or Li2B. 12 H 12 LiCB9H 10 LiCB 11 H 12 NaBH4, Na2B 12 H 12 NaCB9H 10 NaCB 11 H 12 Mg(BH4)2, MgB 12 H 12 and its derivatives.

[0009] Preferably, the fluorinated hydride in step (1) is LiHF2, NaHF2, KHF2, Mg(HF2)2 and its derivatives.

[0010] The reaction equation for the borohydride-based solid electrolyte with hydride is as follows: M A B x H y +M B (HF2) z =M A B x H y-z F z +M B F z + z H2.

[0011] Preferably, the molar ratio of the borohydride-based solid electrolyte and the fluoride in step (1) is between 6:1 and 1:6.

[0012] Preferably, the mixing method in step (1) is one or more of manual grinding, mechanical ball milling, and mechanical vibration.

[0013] Preferably, the heating and heat preservation temperature in step (2) is between 100 and 500°C, and the heat preservation time is between 0.1 and 20 hours.

[0014] Therefore, the method for preparing a fluorine-doped borohydride-based solid electrolyte with the above-described structure has the following beneficial effects: (1) This invention realizes the doping of fluorine in borohydride and can generate fluoride in situ at the electrolyte / electrode interface, thus solving the compatibility problem of borohydride-based solid electrolyte with electrode.

[0015] (2) The solid electrolyte prepared in this invention can achieve high operating voltage and good cycle performance.

[0016] (3) The preparation process described in this invention is simple, has good repeatability, and is suitable for large-scale commercial production.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1 XRD patterns of different samples in Example 1; Figure 2 The following are the FTIR spectra of different samples in Example 1; Figure 3 This is a hydrogen release test diagram during the heating and heat preservation process in the preparation of the solid electrolyte material in Example 2; Figure 4 TEM image of the product in Example 2; Figure 5 The conductivity diagrams for different fluorine-doped solid electrolytes in Example 2 are shown. Figure 6 The graph shows the performance test results of the fluorine-doped solid electrolyte in the Li||Li battery in Example 3. Figure 7 The graph shows the performance test results of the fluorine-doped solid electrolyte in the Na||Na3V2(PO4)3 battery in Example 4. Figure 8 The graph shows the performance test results of the fluorine-doped solid electrolyte in the Mg||TiS2 battery in Example 5. Figure 9 The graph shows the performance test results of the undoped material in the Li||Li battery in Comparative Example 1. Figure 10 The graph shows the performance test results of the undoped material in the Na||Na3V2(PO4)3 battery in Comparative Example 2. Figure 11 The graph shows the performance test results of the solid electrolyte in Comparative Example 3 in a Na||Na3V2(PO4)3 battery. Detailed Implementation

[0019] The present invention will be further described below. It should be noted that this embodiment is based on the present technical solution and provides detailed implementation methods and specific operation processes, but the present invention is not limited to this embodiment.

[0020] Example 1 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Na2B 12 H 12 The mixture was ball-milled with NaHF2 at a molar ratio of 1:1, then heated to 250°C and held for 20 hours to obtain fluorine-doped Na2B.12 H 12 Solid electrolyte.

[0021] like Figure 1 and Figure 2 As shown, the obtained fluorine-doped Na2B 12 H 12 XRD and FTIR characterization of the solid electrolyte confirmed that its main component is Na₂B. 12 H 11 The reaction was carried out using F and NaF, and a unique nanostructure was obtained.

[0022] Example 2 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Na2B 12 H 12 The mixture was ball-milled with NaHF2 at molar ratios of 1:0.75, 1:1.5, and 1:3, and then heated to 280°C and held at that temperature for 10 hours to obtain fluorine-doped Na2B. 12 H 12 Solid electrolyte.

[0023] like Figure 3 As shown, with increasing heating and holding temperatures, the amount of hydrogen released remains almost unchanged below 150°C, but increases significantly between 150°C and 250°C. This indicates that at this temperature, Na₂B… 12 H 12 It reacts chemically with NaHF2.

[0024] like Figure 4 As shown, the prepared fluorine-doped Na2B 12 H 12 The solid electrolyte is made up of nano-sized particles.

[0025] like Figure 5 As shown, the obtained fluorine-doped Na2B 12 H 12 The conductivity of the solid electrolyte was tested, and its room temperature conductivity was 10. -6 Up to 10 -3 S cm -1 The range is [range], and it increases significantly with increasing temperature.

[0026] Example 3 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Li2B 12 H 12 The mixture was shaken and mixed with LiHF2 at a molar ratio of 1:1, then heated to 220°C and held for 20 hours to obtain fluorine-doped Li2B.12 H 12 Solid electrolyte.

[0027] like Figure 6 As shown, the obtained fluorine-doped Li2B 12 H 12 The solid electrolyte was assembled into a Li-symmetric battery and its cycle stability was tested. It could cycle stably for 800 hours without short circuit.

[0028] Example 4 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Na2B 12 H 12 The mixture was ball-milled with NaHF2 at a molar ratio of 1:1, then heated to 250°C and held at that temperature for 15 hours to obtain fluorine-doped Na2B. 12 H 12 Solid electrolyte.

[0029] like Figure 7 As shown, the obtained fluorine-doped Na2B 12 H 12 The solid electrolyte was assembled into a Na||Na3V2(PO4)3 battery, which could stably cycle for 100 cycles and achieve a specific capacity of 97.4 mAh g after cycling. -1 .

[0030] Example 5 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Mg(BH4)2∙2NH3 and KHF2 were ball-milled at a molar ratio of 2:1, and then heated to 200℃ and held for 20 hours to obtain fluorine-doped Mg(BH4)2∙2NH3 solid electrolyte.

[0031] like Figure 8 As shown, the obtained fluorine-doped Mg(BH4)2∙2NH3 solid electrolyte was assembled into a Mg||TiS2 battery, which could be cycled for 50 cycles and the specific capacity reached 80 mAh g after cycling. -1 above.

[0032] Comparative Example 1 A method for preparing a borohydride-based solid electrolyte includes the following steps: Li2B 12 H 12 Ball milling was performed, followed by heating to 280°C and holding for 10 hours to obtain undoped Li₂B. 12 H 12 Solid electrolyte.

[0033] like Figure 9 As shown, undoped Li2B 12 H 12 The solid electrolyte was assembled into a Li-symmetric cell and subjected to cycle stability testing. After 200 hours of cycling, a short circuit occurred.

[0034] Comparative Example 2 A method for preparing a borohydride-based solid electrolyte includes the following steps: Na2B 12 H 12 Ball milling was performed, followed by heating to 250°C and holding for 15 hours to obtain undoped Na₂B. 12 H 12 Solid electrolyte.

[0035] like Figure 10 As shown, undoped Na2B 12 H 12 The solid electrolyte was assembled into a Na||Na3V2(PO4)3 battery, and its specific capacity was less than 40 mAh g after 40 cycles. -1 .

[0036] Comparative Example 3 A method for preparing a fluorine-doped borohydride-based solid electrolyte includes the following steps: Na2B 12 H 12 Na2B was obtained by ball milling and mixing with NaF. 12 H 12 -NaF composite solid electrolyte.

[0037] like Figure 11 As shown, Na2B 12 H 12 The NaF composite solid electrolyte was assembled into a Na||Na3V2(PO4)3 battery, but its specific capacity was less than 80 mAh g after 40 cycles. -1 .

[0038] Therefore, the present invention provides a method for preparing a fluorine-doped borohydride-based solid electrolyte with the above-mentioned structure. This method achieves in-situ doping of fluorine in the borohydride-based solid electrolyte, which is beneficial for stabilizing the interface between the electrolyte and the electrode. Furthermore, the preparation method is simple, cost-controllable, and suitable for large-scale production. At the same time, the prepared electrolyte has high ionic conductivity and good compatibility with the positive and negative electrodes, which can significantly improve the electrochemical performance of all-solid-state batteries.

[0039] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a fluorine-doped borohydride-based solid electrolyte, characterized in that: Includes the following steps: (1) A mixture is obtained by mixing a borohydride-based solid electrolyte and a fluoride; (2) The mixture is heated and kept at a constant temperature to obtain a fluorine-doped borohydride-based solid electrolyte; The borohydride-based solid electrolyte in step (1) is LiBH4 or Li2B. 12 H 12 LiCB9H 10 LiCB 11 H 12 NaBH4, Na2B 12 H 12 NaCB9H 10 NaCB 11 H 12 Mg(BH4)2, MgB 12 H 12 One of Mg(BH4)2∙2NH3; The fluoride in step (1) is one of LiHF2, NaHF2, KHF2, or Mg(HF2)2.

2. The method for preparing a fluorine-doped borohydride-based solid electrolyte according to claim 1, characterized in that: The molar ratio of the borohydride-based solid electrolyte and the fluoride in step (1) is between 6:1 and 1:

6.

3. The method for preparing a fluorine-doped borohydride-based solid electrolyte according to claim 1, characterized in that: The mixing method in step (1) is one or more of manual grinding, mechanical ball milling, and mechanical vibration.

4. The method for preparing a fluorine-doped borohydride-based solid electrolyte according to claim 1, characterized in that: The heating and heat preservation temperature in step (2) is between 100 and 500°C, and the heat preservation time is between 0.1 and 20 hours.