A dual half-heusler thermoelectric material with high-entropy sublattice structure and a method of making the same

By introducing TiZrHfNbV sublattices into Ti₂FeNiSb₂-based alloys and optimizing the preparation process, a double half-Hessler thermoelectric material with a high-entropy sublattice structure was formed, solving the problem of high lattice thermal conductivity, optimizing electrical transport performance and improving thermoelectric figure of merit, making it suitable for thermoelectric devices.

CN116828958BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310669388.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-07
Publication Date
2026-11-24
Estimated Expiration
2043-06-07

AI Technical Summary

Technical Problem

The high lattice thermal conductivity of existing semi-Hessler thermoelectric materials limits further improvement in thermoelectric figure of merit, and the electrical transport properties and thermal transport properties are mutually restrictive and difficult to optimize simultaneously.

Method used

A high-entropy doping strategy was adopted to introduce TiZrHfNbV sublattices into Ti₂FeNiSb₂-based alloys. Through alloying and preparation process optimization, a double half-Hessler thermoelectric material with a high-entropy sublattice structure was formed, including melting, annealing, ball milling and plasma sintering processes.

Benefits of technology

It effectively reduces lattice thermal conductivity, optimizes electrical transport properties, improves thermoelectric figure of merit, and the material is easy to process, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116828958B_ABST
    Figure CN116828958B_ABST
Patent Text Reader

Abstract

This invention discloses a double half-Hessler thermoelectric material with a high-entropy sublattice structure, the chemical composition of which is Ti. x Zr x Hf x (Nb y V 8‑3x‑y )Fe z Ni 8‑z Sb8 is a high-entropy sublattice of TiZrHfNbV introduced into the Ti site of the double half-Hessler thermoelectric material Ti2FeNiSb2; wherein the elemental proportions of Ti, Zr, Hf, Nb, and V are 0 < 3x + y ≤ 8, and x > 0, y > 0; the elemental proportions of Fe and Ni are 0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of thermoelectric materials technology, specifically relating to a double half-Hessler alloy with a high-entropy sublattice structure and its preparation method. Background Technology

[0002] In today's era of actively advocating green and low-carbon energy development and promoting green and low-carbon energy transformation, thermoelectric devices are considered a promising green energy conversion technology due to their wear-free nature, long service life, and environmental friendliness. They facilitate more convenient and precise temperature control and provide a stable constant-temperature environment. Thermoelectric devices can directly convert waste heat from automobile exhaust and factory flue gas into clean electricity or provide cooling or heating energy through electricity, reducing the use of Freon and the environmental pollution caused by fuel combustion. Thermoelectric devices are mainly composed of P-type and N-type thermoelectric materials. Half-Heulser (ABX) thermoelectric material is a widely mentioned and researched medium- and high-temperature thermoelectric material in recent years. It has high mechanical strength, excellent chemical and thermal stability, and its excellent electrical and thermal transport properties give it a high thermoelectric figure of merit, but its lattice thermal conductivity is higher than other thermoelectric systems (~15-20 W / m). -1 K -1 This limits further improvement in thermoelectric figure of merit.

[0003] Lattice thermal conductivity is related to phonon scattering, lattice softening mechanisms, unit cell size, and the number of atoms per unit cell. Double half-Heulser (DHH) thermoelectric materials are based on equivalent substitution at a specific site in the HH, possessing the chemical formula A2B1B2X2, such as Ti2FeNiSb2 and TiCoSb. Due to the equivalent substitution of two components in the sublattice, DHH often exhibits a lower lattice thermal conductivity (room temperature lattice thermal conductivity ~10 W / m²) compared to its corresponding HH. -1 K -1 High-entropy alloys (HEAs) and their four core effects—high entropy, slow diffusion, severe lattice distortion, and the cocktail effect—have gained prominence in recent years for optimizing electrical and thermal transport properties. Applying entropy engineering to bihalf-Hessler thermoelectric materials, introducing several different elements into their sublattices, can be considered as high-entropy sublattices. The increased entropy through complex composition and configuration, by creating various point defects, mass fluctuations, and strain field fluctuations, may be highly effective in reducing lattice thermal conductivity and altering thermoelectric transport. Chemical disorder and lattice distortion make high-entropy alloys a promising next-generation thermoelectric material.

[0004] On the other hand, electrical transport properties and thermal transport properties are often interrelated and mutually restrictive; optimizing one often comes at the cost of reducing the performance of the other. Designing high-entropy double-half-Helles thermoelectric materials with simultaneously optimized thermal and electrical transport properties through high-entropy doped double-half-Helles thermoelectric materials and process optimization is of great significance for the research and future industrial applications of thermoelectric materials. Summary of the Invention

[0005] The purpose of this invention is to address the above-mentioned problems by providing a high-entropy doped Ti. x Zr x Hf x (Nb y V 8-3x-y )Fe z Ni 8- z Sb8 thermoelectric material further reduces thermal conductivity without significantly reducing electrical transport performance based on the double half-Hessler thermoelectric material, and also provides a method for preparing the material.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] This invention provides a double half-Hessler thermoelectric material with a high-entropy sublattice structure, wherein the chemical composition of the thermoelectric material is Ti. x Zr x Hf x (Nb y V 8-3x-y )Fe z Ni 8-z Sb8 represents the introduction of a high-entropy sublattice of TiZrHfNbV at the Ti site in the bihalf-Hessler thermoelectric material Ti2FeNiSb2.

[0008] The proportions of Ti, Zr, Hf, Nb, and V are such that 0 < 3x + y ≤ 8, and x > 0 and y > 0.

[0009] Since Fe and Ni elements play a dominant role in the band gap of the material, their thermoelectric properties can be optimized by adjusting their content. To ensure the A2B1B2X2 chemical formula characteristics of the dual-half Hessler thermoelectric material, the Fe and Ni element ratio is 0. <z<8。

[0010] Preferably, when x = 2, y = 1, z = 5, the chemical composition of the thermoelectric material is Ti2Zr2Hf2NbVFe5Ni3Sb8; when x = 2, y = 2, z = 5, the chemical composition of the thermoelectric material is Ti2Zr2Hf2Nb2Fe5Ni3Sb8.

[0011] Preferably, the metal raw materials used are all high-purity elemental substances, with the purity of Ti, Zr, Hf, Nb, V, Fe, Ni and Sb being 99% to 99.99%.

[0012] The present invention also provides a method for preparing the double half-Hessler thermoelectric material having a high-entropy sublattice structure, comprising preparing the thermoelectric material according to the chemical composition Ti... x Zr x Hf x (Nb y V 8-3x-y )Fe z Ni 8-z The thermoelectric material is obtained by mixing the elements in the Sb8 molar ratio and then sequentially performing melting, annealing, ball milling, and plasma sintering.

[0013] Specifically, the preparation method includes the following steps:

[0014] S1. Weigh all the metal raw materials according to the molar ratio, and then melt them at high temperature to obtain a pre-alloy;

[0015] S2. The pre-alloy obtained in S1 is subjected to high-temperature annealing;

[0016] S3. The alloy after S2 annealing is ball-milled to obtain alloy powder;

[0017] S4. The powder obtained in S3 is subjected to high-temperature spark plasma sintering to obtain the double half-Hessler thermoelectric material with a high-entropy sublattice structure.

[0018] Preferably, in step S1, in order to ensure that the final composition obtained conforms to the chemical formula of the double half-Hessler thermoelectric material, has no full Hessler secondary phase, and compensates for the volatilization of the low-melting-point element Sb during the preparation process, the total molar mass of elements Ti, Zr, Hf, Nb and V, the total molar mass of elements Fe and Ni, and the molar mass ratio of Sb are 1:1:(1.05~1.1).

[0019] Preferably, in step S1, the high-temperature melting is carried out under an Ar protective atmosphere, and the melting method is electric arc furnace melting, with 3 to 5 melting cycles. The melting process of this invention is a pre-alloying process, the purpose of which is to allow elements with large melting point differences to undergo an alloying process first, preventing the large-scale volatilization of low-melting-point elements during sintering and deviation from the standard stoichiometric ratio. There are no special restrictions on the order of placement of the elemental substances during the melting process. In a specific embodiment of this invention, the actual amount of Sb added is 5 to 10% more than the mass of Sb weighed according to the molar ratio specified in the above technical solution.

[0020] Preferably, in step S2, to promote the homogenization of chemical composition and microstructure while improving the processability of the material, the high-temperature annealing temperature is 800–1000°C, more preferably 900–1000°C. The high-temperature annealing time is 4–14 days, more preferably 5–7 days. After the high-temperature annealing is completed, the cooling method is furnace cooling and oil cooling, preferably furnace cooling.

[0021] Preferably, in step S3, the ball-to-material ratio of the ball mill is 3:1 to 10:1, more preferably 4:1 to 6:1; the rotation speed is 300 to 600 rpm, and the ball milling time is 1 to 12 hours, so as to obtain alloy powders of different particle sizes.

[0022] The ball milling process has no special requirements and can be carried out using a process well known to those skilled in the art. The ball milling time can control the size of the powder obtained after ball milling, which affects the scattering of phonons and charge carriers by factors such as grain boundaries, porosity, and dislocations in the plasma-sintered sample. After ball milling, the present invention preferably includes screening the powder obtained after ball milling through a 200-mesh sieve and then performing vacuum drying; the drying process has no special requirements.

[0023] Preferably, in step S4, the plasma sintering temperature is 800–1000℃, more preferably 950℃; the heating rate is 80–200℃ / min, more preferably 80–100℃ / min; the sintering pressure is 40–70 MPa, more preferably 60 MPa; and the sintering time is 3–15 min, more preferably 5–10 min.

[0024] After sintering, heat preservation, and pressure holding, the plasma is cooled in the furnace. This invention does not impose special requirements on other preparation processes and experimental conditions for the plasma sintering; processes well-known to those skilled in the art can be used.

[0025] The present invention also provides the application of the double half-Hessler thermoelectric material with high-entropy sublattice structure in thermoelectric devices.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] This invention optimizes the thermoelectric properties of a dual-half-Hessler material using a high-entropy strategy. Specifically, it involves elemental doping of Ti sites in a Ti2FeNiSb2-based alloy, introducing a high-entropy sublattice through alloying, and obtaining a dual-half-Hessler thermoelectric material with a high-entropy sublattice structure. The chemical composition of the thermoelectric material is Ti. x Zr x Hf x (Nb y V 8-3x-y )Fe z Ni 8-z Sb8.

[0028] By enhancing the scattering of high-frequency phonons through the high-entropy effect and balancing the scattering of charge carriers and phonons within the material through process control, the high-entropy double half-Hessler thermoelectric material obtained in this invention has a lower lattice thermal conductivity than the existing double half-Hessler thermoelectric material Ti2FeNiSb2-based alloy, while its electrical transport performance is optimized.

[0029] This invention also provides an effective preparation method for the aforementioned double-half Hessler thermoelectric material with a high-entropy sublattice structure, comprising melting-annealing-ball milling-plasma sintering. This method has simple preparation conditions and is easy to implement for mass production. Attached Figure Description

[0030] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0031] Figure 1 The X-ray diffraction (XRD) patterns of the alloys prepared in Examples 1, 2, 3 and Comparative Example 1 are shown.

[0032] Figure 2 This is a schematic diagram of the crystal structure of the double half-Hessler thermoelectric material with a high-entropy sublattice structure.

[0033] Figure 3 Scanning electron microscope (SEM) image of the alloy prepared in Example 1;

[0034] Figure 4 SEM image of the alloy prepared in Example 2;

[0035] Figure 5 SEM image of the alloy prepared in Example 3;

[0036] Figure 6 SEM images of the alloy prepared for Comparative Example 1;

[0037] Figure 7 The optimal power factor (PF) of the alloys obtained in Example 2 and Comparative Example 1. max ), room temperature thermal conductivity (κ);

[0038] Figure 8 The thermoelectric figure of merit (ZT) of the alloys obtained in Example 2 and Comparative Example 1;

[0039] Figure 9These are photographs of the high-entropy double half-Hessler alloy blocks prepared in Examples 1-3 after cutting.

[0040] Figure 10 (a) and Figure 10 (b) Photographs of the alloy block of Comparative Example 2 after it was cut, taken at different times.

[0041] Figure 11 (a) is a photograph of the alloy block of Comparative Example 3 that fractured during the final heat treatment step. Figure 11 (b) is a photograph of the surface cracks on the fractured surface. Detailed Implementation

[0042] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the invention will be described in detail below with reference to specific embodiments. It should be understood that the embodiments described in this specification are merely illustrative and not intended to limit the scope of the invention.

[0043] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.

[0044] Example 1

[0045] Table 1

[0046]

[0047] Weigh and prepare the elements according to the quantities listed in Table 1 (with each metal element having a purity ≥ 99.9%), place them in an electric arc furnace, and heat them to a molten state under a high-purity argon atmosphere while simultaneously stirring electromagnetically to ensure thorough and uniform mixing of the elements. After approximately 2 minutes, turn off the heat source and electromagnetic stirrer, and rapidly cool the material in a water-cooled electric arc furnace. Turn the alloy button ingot over and reheat to melt it. Repeat the above melting process 4 times.

[0048] The obtained button ingots were subjected to vacuum high-temperature heat treatment at 950°C for one week, and then cooled in the furnace.

[0049] After heat treatment, the alloy button ingots are crushed and then ball-milled at a ball-to-material ratio of 4:1, a rotation speed of 450 rpm, and a time of 3 hours. The ball-milled material is then sieved through a 200-mesh sieve and dried in a vacuum chamber.

[0050] The dried alloy powder was poured into a graphite mold and placed in a plasma sintering equipment. The temperature was raised to 950°C at a rate of 100°C / min under a pressure of 60 MPa, and held at that temperature and pressure for 5 minutes for plasma sintering. After sintering, the material was cooled with the furnace to obtain a high-entropy double half-Hessler thermoelectric material with the chemical formula Ti2Zr2Hf2NbVFe5Ni3Sb8.

[0051] Example 2

[0052] Weigh and prepare the elements according to the quantities listed in Table 1 (with each metal element having a purity ≥ 99.9%), place them in an electric arc furnace, and heat them to a molten state under a high-purity argon atmosphere while simultaneously stirring electromagnetically to ensure thorough and uniform mixing of the elements. After approximately 2 minutes, turn off the heat source and electromagnetic stirrer, and rapidly cool the material in a water-cooled electric arc furnace. Turn the alloy button ingot over and reheat to melt it. Repeat the above melting process 4 times.

[0053] The obtained button ingots were subjected to vacuum high-temperature heat treatment at 950°C for one week, and then cooled in the furnace.

[0054] After heat treatment, the alloy button ingots are crushed and then ball-milled at a ball-to-material ratio of 4:1, a rotation speed of 450 rpm, and a time of 1 hour. The ball-milled material is then sieved through a 200-mesh sieve and dried in a vacuum chamber.

[0055] The dried alloy powder was poured into a graphite mold and placed in a plasma sintering equipment. The temperature was raised to 950°C at a rate of 100°C / min under a pressure of 60 MPa, and held at that temperature and pressure for 5 minutes for plasma sintering. After sintering, the material was cooled with the furnace to obtain a high-entropy double half-Hessler thermoelectric material with the chemical formula Ti2Zr2Hf2NbVFe5Ni3Sb8.

[0056] Example 3

[0057] Table 2

[0058]

[0059] Weigh and prepare the elements according to the quantities listed in Table 2 (where the purity of each metal element is ≥99.9%), place them in an electric arc furnace, and heat them to a molten state under a high-purity argon atmosphere. While heating, perform electromagnetic stirring to ensure thorough and uniform mixing of the elements. After approximately 2 minutes, turn off the heat source and electromagnetic stirrer, and rapidly cool the material in a water-cooled electric arc furnace. Turn the alloy button ingot over and reheat to melt it. Repeat the above melting process four times.

[0060] The obtained button ingots were subjected to vacuum high-temperature heat treatment at 950°C for one week, and then cooled in the furnace.

[0061] After heat treatment, the alloy button ingots were crushed and ball-milled at a ball-to-material ratio of 4:1, a rotation speed of 450 rpm, and a time of 12 hours. The ball-milled material was then sieved through a 200-mesh sieve and dried in a vacuum chamber.

[0062] The dried alloy powder was poured into a graphite mold and placed in a plasma sintering equipment. The temperature was raised to 950°C at a rate of 100°C / min under a pressure of 60 MPa, and held at that temperature and pressure for 5 minutes for plasma sintering. After sintering, the material was cooled with the furnace to obtain a high-entropy double half-Hessler thermoelectric material with the chemical formula Ti2Zr2Hf2Nb2Fe5Ni3Sb8.

[0063] Comparative Example 1

[0064] The dual-half Hessler thermoelectric material Ti2FeNiSb2 was prepared according to the method described in Example 1. That is, except for the raw materials and proportions, the preparation process was the same as in Example 1.

[0065] Performance testing

[0066] Test Example 1

[0067] XRD tests were performed on the thermoelectric materials obtained in Examples 1, 2, 3 and Comparative Example 1. The test results are as follows: Figure 1 As shown. Figure 2 This is a schematic diagram of the crystal structure of the high-entropy double half-Hessler thermoelectric material, which has a face-centered cubic structure and features high-entropy sublattice substitution at the Ti sites.

[0068] from Figure 1 It can be seen that the high-entropy double-half-Hessler thermoelectric material has the same crystal structure as the parent double-half-Hessler thermoelectric material, which is consistent with... Figure 2 The diagram shows a schematic of the crystal structure. No obvious impurity peaks were observed, indicating that almost all of the crystals formed a high-entropy sublattice. The diffraction peaks of the embodiment are shifted at a smaller angle compared to the comparative example, indicating that the introduction of the high-entropy sublattice caused lattice distortion, significantly affecting the phonon scattering process of the material.

[0069] Test Example 2

[0070] The thermoelectric materials obtained in Examples 1, 2, 3 and Comparative Example 1 were characterized by SEM microstructure, and the test results are as follows: Figure 3 , 4 As shown in Figures 5 and 6. From Figures 3-6 The non-uniform contrast of the material indicates an uneven distribution of internal elements, resulting in a deviation between the actual and nominal compositions of the high-entropy double-half-Hessler thermoelectric material, indicating phase separation. The circled areas highlight the different contrasts observed in the SEM, which, according to EDS analysis, are due to the uneven distribution of Ti, Zr, Hf, Nb, and V. The elemental proportions in the high-entropy sublattices differ at different contrast levels, but the overall composition conforms to the nominal composition. Furthermore, the material is free of cracks and has few pores, indicating good forming quality.

[0071] Test Example 3

[0072] The electrical conductivity and Seebeck coefficient of the double half-Hessler alloys obtained in Examples 1, 2, 3 and Comparative Example 1 were tested using an electrical performance testing system, and the power factor (PF) was calculated.

[0073] The thermal diffusivity of the double half-Hessler alloys obtained in Examples 1, 2 and Comparative Example 1 was tested using the laser scintillation method. The sample density was measured using the Archimedes displacement method, and the heat capacity was measured using a differential scanner to calculate the total thermal conductivity.

[0074] The thermoelectric figure of merit is calculated based on the power factor and total thermal conductivity.

[0075] Figure 7 The optimal power factor and room temperature thermal conductivity of the alloys obtained in Example 2 and Comparative Example 1 are preferred among Examples 1, 2 and 3. Figure 8 The thermoelectric figure of merit is the better alloy obtained in Example 2 and Comparative Example 1 among Examples 1, 2 and 3.

[0076] from Figure 7 , Figure 8 As can be seen, compared to the comparative example which is a double-half-Hessler thermoelectric material, the high-entropy double-half-Hessler alloy obtained in this invention has lower thermal conductivity and better electrical transport performance by introducing entropy effects and optimizing the preparation process. The maximum thermoelectric figure of merit of the high-entropy double-half-Hessler thermoelectric material described in Example 2 is increased by approximately 400% compared to the comparative example.

[0077] Furthermore, to illustrate that the preparation method of pre-alloying-high-temperature heat treatment-ball milling-plasma sintering is necessary in this invention to obtain the corresponding high-entropy double half-Hessler bulk, this bulk exhibits good machinability, which is a necessary factor for realizing thermoelectric material applications. Comparative Examples 2 and 3 are provided.

[0078] Comparative Example 2

[0079] Weigh and prepare the elements according to the quantities listed in Table 1 (where the purity of each metal element is ≥99.9%), place them in an electric arc furnace, and heat them to a molten state under a high-purity argon atmosphere. While heating, perform electromagnetic stirring to ensure thorough and uniform mixing of the elements. After approximately 2 minutes, turn off the heat source and electromagnetic stirrer, and rapidly cool the material in a water-cooled electric arc furnace. Turn the alloy button ingot over and reheat to melt it. Repeat the above melting process four times.

[0080] After high-temperature melting, the pre-alloyed button ingots are directly crushed and ball-milled (ball-to-material ratio of 4:1, rotation speed of 450 rpm, time of 1 hour) without long-term high-temperature heat treatment; then the ball-milled material is sieved through a 200-mesh sieve and dried in a vacuum chamber.

[0081] The dried alloy powder was poured into a graphite mold and placed in a plasma sintering apparatus. The temperature was raised to 950°C at a rate of 100°C / min under a pressure of 60 MPa, and held at that temperature and pressure for 5 minutes for plasma sintering. After sintering, the material was cooled in the furnace to obtain a high-entropy double half-Hessler thermoelectric material with the chemical formula Ti2Zr2Hf2NbVFe5Ni3Sb8.

[0082] Figure 9 The images show the cut edges of the high-entropy double half-Hessler alloy blocks prepared in Examples 1-3. The cut blocks have smooth edges, proving that they are easy to process.

[0083] Unlike the above embodiments, Comparative Example 2 did not undergo high-temperature heat treatment. The high-entropy double half-Hessler alloy block prepared by pre-alloying-ball milling-plasma sintering had poor machinability. When processing the test sample, it could not be cut with a slow-speed cutter, and it shattered completely when cut with a laser or EDM machine. Figure 10 Comparative Example 2: Photographs of the alloy block after cutting, taken at different times.

[0084] Comparative Example 3

[0085] Weigh and prepare the elements according to the quantities listed in Table 1 (where the purity of each metal element is ≥99.9%), place them in an electric arc furnace, and heat them to a molten state under a high-purity argon atmosphere. While heating, perform electromagnetic stirring to ensure thorough and uniform mixing of the elements. After approximately 2 minutes, turn off the heat source and electromagnetic stirrer, and rapidly cool the material in a water-cooled electric arc furnace. Turn the alloy button ingot over and reheat to melt it. Repeat the above melting process four times.

[0086] After high-temperature melting, the pre-alloyed button ingots are directly crushed and ball-milled (ball-to-material ratio of 4:1, rotation speed of 450 rpm, time of 1 hour) without long-term high-temperature heat treatment; then the ball-milled material is sieved through a 200-mesh sieve and dried in a vacuum chamber.

[0087] The dried alloy powder was poured into a graphite mold and placed in a plasma sintering equipment. The temperature was raised to 950°C at a rate of 100°C / min under a pressure of 60MPa, and held at that temperature and pressure for 5 minutes for plasma sintering. After sintering, the powder was cooled with the furnace.

[0088] The sintered bulk material was subjected to vacuum high-temperature heat treatment at 950℃ for one week, followed by furnace cooling. This yielded a high-entropy double-half-Hessler thermoelectric material with the chemical formula Ti2Zr2Hf2NbVFe5Ni3Sb8.

[0089] The high-entropy double-half-Helles block, which underwent pre-alloying, ball milling, plasma sintering, and high-temperature heat treatment, fractured during the final heat treatment step, as... Figure 11 As shown in (a). Figure 11 (b) shows the surface cracks on the fractured surface, illustrating the importance of the final plasma sintering step, which uses high temperature and high pressure during plasma sintering to densify and press the material to prevent crack propagation and fracture.

[0090] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this invention, and these modifications or substitutions should all be covered within the scope of protection of this invention. Therefore, the scope of protection of this invention should be determined by the scope defined in the claims.

Claims

1. A double half-Hessler thermoelectric material with a high-entropy sublattice structure, characterized in that, The chemical composition of the thermoelectric material is Ti x Zr x Hf x (Nb y V 8-3x-y )Fe z Ni 8-z Sb8, is introducing TiZrHfNbV or TiZrHfNb high entropy sub-lattice at the Ti site of the double half Heusler thermoelectric material Ti2FeNiSb2; When x=2, y=1, z=5, the chemical composition of the thermoelectric material is Ti2Zr2Hf2NbVFe5Ni3Sb8; when x=2, y=2, z=5, the chemical composition of the thermoelectric material is Ti2Zr2Hf2Nb2Fe5Ni3Sb8. The preparation method of the double half-Hessler thermoelectric material with a high-entropy sublattice structure includes the following steps: S1. Weigh all the metal raw materials according to the molar ratio, and then melt them at high temperature to obtain a pre-alloy; S2. The pre-alloy obtained in S1 is subjected to high-temperature annealing; S3. The alloy after S2 annealing is ball-milled to obtain alloy powder; S4. The powder obtained in S3 is subjected to high-temperature spark plasma sintering to obtain the double half-Hessler thermoelectric material with a high-entropy sublattice structure. In step S2, the high-temperature annealing temperature is 800~1000℃, and the high-temperature annealing time is 4~14 days; In step S4, the plasma sintering temperature is 800~1000 ℃, the heating rate is 80~200℃ / min, the sintering pressure is 40~70 MPa, and the sintering time is 3~15 min.

2. The double half-Hessler thermoelectric material with a high-entropy sublattice structure according to claim 1, characterized in that, The thermoelectric material uses high-purity elemental metals, with Ti, Zr, Hf, Nb, V, Fe, Ni and Sb having a purity of 99% to 99.99%.

3. The double half-Hessler thermoelectric material with a high-entropy sublattice structure according to claim 1, characterized in that, In step S1, the total molar mass of elements Ti, Zr, Hf, Nb and V, the total molar mass of elements Fe and Ni, and the molar mass ratio of Sb are 1:1:(1.05~1.1).

4. The double half-Hessler thermoelectric material with a high-entropy sublattice structure according to claim 1, characterized in that, In step S1, the high-temperature melting is carried out under an Ar protective atmosphere, and the melting method is electric arc furnace melting, with the melting process repeated 3 to 5 times.

5. The double half-Hessler thermoelectric material with a high-entropy sublattice structure according to claim 1, characterized in that, In step S3, the ball-to-material ratio of the ball mill is 3:1 to 10:1, the rotation speed is 300 to 600 rpm, and the ball milling time is 1 to 12 h.

6. The application of the double half-Hessler thermoelectric material with a high-entropy sublattice structure as described in any one of claims 1 to 5 in thermoelectric devices.

Citation Information

Patent Citations

  • TiCoSb-based high-entropy thermoelectric material, preparation method thereof and thermoelectric device

    CN108091755A

  • KR20210067006A