Fluidized bed reactor and method for regenerating lithium precursor using the same

By using a fluidized bed reactor and reducing gas treatment, the problem of efficiently and effectively recovering lithium precursors from waste lithium secondary batteries was solved, achieving high-yield and high-purity lithium precursor preparation and improving recovery efficiency.

CN116829512BActive Publication Date: 2026-11-20SK INNOVATION CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280014323.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-11
Filing Date
2022-03-10
Publication Date
2026-11-20
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

Existing technologies make it difficult to efficiently and effectively recover lithium precursors from waste lithium secondary batteries, leading to resource waste and environmental problems.

Method used

A fluidized bed reactor was used to prepare a high-purity lithium precursor by reducing positive electrode active material powders with different particle sizes in a reactor body with a gradually decreasing diameter, combined with reducing gas fluidization and water washing.

Benefits of technology

It achieves high-yield and high-purity lithium precursor recovery, reduces temperature deviation, prevents active material powder deposition, and improves recovery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116829512B_ABST
    Figure CN116829512B_ABST
Patent Text Reader

Abstract

The lithium precursor regeneration method of the present invention prepares positive electrode active material powders containing lithium complex oxide particles and having particle sizes different from each other. The positive electrode active material powders are subjected to reduction treatment in a fluidized bed reactor to prepare a preliminary precursor mixture, wherein the fluidized bed reactor includes a reactor body whose diameter is gradually or progressively reduced from the upper portion to the lower portion. Also, a lithium precursor is recovered from the preliminary precursor mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a fluidized bed reactor and a method for regenerating lithium precursors using the fluidized bed reactor. More specifically, it relates to a fluidized bed reactor and a method for regenerating lithium precursors from compounds containing spent lithium using the fluidized bed reactor. Background Technology

[0002] Rechargeable batteries are batteries that can be repeatedly charged and discharged. With the development of the information communication and display industries, rechargeable batteries are widely used in portable electronic communication devices, such as portable cameras, mobile phones, and laptops. Examples of rechargeable batteries include lithium batteries, nickel-cadmium batteries, and nickel-metal hydride batteries. Among them, lithium batteries have high operating voltage and energy density per unit weight, and are advantageous for charging speed and lightweight design. Therefore, lithium batteries are being actively developed and applied.

[0003] A lithium secondary battery may include an electrode assembly and an electrolyte impregnating the electrode assembly, wherein the electrode assembly includes a positive electrode, a negative electrode, and a separator (membrane). The lithium secondary battery may also include, for example, a pouch-type outer packaging material that contains the electrode assembly and the electrolyte.

[0004] Lithium metal oxide can be used as the positive electrode active material of the lithium secondary battery. The lithium metal oxide may further contain transition metals such as nickel, cobalt, and manganese.

[0005] The lithium metal oxide, which is the positive electrode active material, can be prepared by reacting a lithium precursor with a nickel-cobalt-manganese (NCM) precursor containing nickel, cobalt, and manganese.

[0006] Because the aforementioned high-cost metals are used in the positive electrode active material, the manufacturing cost accounts for more than 20% of the total cost of preparing the positive electrode material. Furthermore, due to the increasing prominence of environmental issues in recent years, methods for recycling positive electrode active materials are being researched. To recycle the positive electrode active material, it is necessary to regenerate the lithium precursor from waste positive electrodes with high efficiency and high purity. Summary of the Invention

[0007] Technical problems to be solved

[0008] One technical problem of the present invention is to provide a fluidized bed reactor for recovering lithium precursors from lithium-containing compounds with high purity and high yield, and a method for regenerating lithium precursors using the fluidized bed reactor.

[0009] Technical solution

[0010] A lithium precursor regeneration method according to an embodiment of the present invention may include the step of preparing a positive electrode active material powder comprising lithium composite oxide particles having different particle sizes. The positive electrode active material powder is then reduced in a fluidized bed reactor to prepare a preliminary precursor mixture, the fluidized bed reactor comprising a reactor body whose diameter gradually decreases from top to bottom. Finally, the lithium precursor is recovered from the preliminary precursor mixture.

[0011] In an exemplary embodiment, the positive electrode active material mixture may comprise a first active material powder, a second active material powder, and a third active material powder with different particle sizes, and the reactor body may include a first region for fluidizing the first active material powder, a second region for fluidizing the second active material powder, and a third region for fluidizing the third active material powder.

[0012] In an exemplary embodiment, the first region, the second region, and the third region can be sequentially arranged from the upper part of the reactor body.

[0013] In an exemplary implementation, the diameter of the first region may be larger than the diameter of the second region, and the diameter of the second region may be larger than the diameter of the third region.

[0014] In an exemplary implementation, the ratio of the diameter of the first region to the diameter of the third region can be 4 to 16.

[0015] In an exemplary embodiment, the ratio of the diameter of the second region to the diameter of the third region can be 2 to 4.

[0016] In an exemplary embodiment, the particle size of the first active substance powder may be smaller than that of the second active substance powder, and the particle size of the second active substance powder may be smaller than that of the third active substance powder.

[0017] In an exemplary embodiment, the particle size of the first active substance powder may be less than 10 μm, the particle size of the second active substance powder may be 10-100 μm, and the particle size of the third active substance powder may be greater than 100 μm.

[0018] In an exemplary embodiment, the preparation of the preliminary precursor mixture may include injecting a reducing gas into the fluidized bed reactor.

[0019] In an exemplary embodiment, the minimum flow rate of the reducing gas in the first region may be below the terminal velocity of the first active substance powder.

[0020] In an exemplary embodiment, the maximum flow rate of the reducing gas in the second region may be greater than or equal to the minimum fluidization rate of the second active substance powder, and the maximum flow rate of the reducing gas in the third region may be greater than or equal to the minimum fluidization rate of the third active substance powder.

[0021] In an exemplary embodiment, the reducing gas can be injected into the interior of the fluidized bed reactor at a flow rate of 8-18 cm / s.

[0022] In an exemplary embodiment, the reactor body may include: a first connecting portion connecting the first region and the second region, and having a diameter that gradually decreases from the first region to the second region; and a second connecting portion connecting the second region and the third region, and having a diameter that gradually decreases from the second region to the third region.

[0023] In an exemplary embodiment, the first connecting portion and the second connecting portion may further include gas injection ports located on the sides.

[0024] In an exemplary embodiment, the gas injection port may be positioned upwards and obliquely on the side of the reactor body.

[0025] In an exemplary embodiment, the angle formed between the side surfaces of the first and second connecting portions and the gas injection port can be 45-90°.

[0026] A fluidized bed reactor for reducing positive electrode active material according to an embodiment of the present invention may include: a reactor body, the diameter of which gradually decreases from top to bottom; an active material injection port through which a plurality of positive electrode active material powders comprising lithium composite oxide particles of different sizes are injected into the interior of the reactor body; and a gas injection port located at the bottom of the reactor body, through which a reducing gas for fluidizing the active material powder is injected.

[0027] In an exemplary embodiment, the fluidized bed reactor of the present invention for reducing positive electrode active material may include: a first connecting portion connecting the first region and the second region, and having a diameter that gradually decreases from the first region to the second region; and a second connecting portion connecting the second region and the third region, and having a diameter that gradually decreases from the second region to the third region.

[0028] In an exemplary embodiment, the first connecting portion and the second connecting portion may further include gas injection ports located on the sides.

[0029] Beneficial effects

[0030] According to the above exemplary embodiments, the lithium precursor regeneration method of the present invention can reduce active material powders with different particle sizes in a fluidized bed reactor, wherein the fluidized bed reactor comprises a reactor body whose diameter gradually decreases from top to bottom. Therefore, it is easier to obtain lithium precursors with high yield and high purity.

[0031] Furthermore, by varying the reactor diameter, temperature deviations based on location within the reactor can be reduced. This allows for smooth fluidization of the positive electrode active material particles, resulting in uniform mixing / reduction throughout the reactor.

[0032] Furthermore, a gas injection port may be included on the side of the fluidized bed reactor. This gas injection port can prevent the active material powder from depositing on the side of the fluidized bed reactor. Therefore, the recovery efficiency of the lithium precursor can be further improved. Attached Figure Description

[0033] Figure 1 This is a schematic flowchart illustrating a lithium precursor regeneration method according to an exemplary embodiment.

[0034] Figure 2 and Figure 3 This is a schematic diagram illustrating a fluidized bed reactor for reducing positive electrode active material according to an exemplary embodiment. Detailed Implementation

[0035] In embodiments of the present invention, a fluidized bed reactor comprising a reactor body whose diameter gradually decreases from top to bottom is used to recover lithium precursors from positive electrode active materials. Therefore, the recovery efficiency of lithium precursors can be further improved.

[0036] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, these are merely exemplary embodiments, and the present invention is not limited to the specific embodiments described herein.

[0037] As used in this specification, the term "precursor" refers to a compound containing a specific metal in order to provide a specific metal contained in a positive electrode active material.

[0038] Figure 1 This is a schematic diagram illustrating a lithium precursor regeneration method according to an exemplary embodiment.

[0039] According to an exemplary implementation, a positive electrode active material powder comprising lithium composite oxide particles having different particle sizes from each other can be prepared (e.g., step S10).

[0040] The positive electrode active material powder may contain lithium composite oxide particles obtained or regenerated from electrical and chemical components. The positive electrode active material powder may contain various lithium composite oxide particles such as lithium oxide, lithium carbonate, and lithium hydroxide.

[0041] The positive electrode active material powder may contain lithium composite oxide particles obtained from or recycled from waste lithium secondary batteries. The waste lithium secondary battery may include an electrode assembly, which includes a positive electrode, a negative electrode, and a separator between the positive and negative electrodes. The positive and negative electrodes may each include a positive electrode active material layer and a negative electrode active material layer coated on a positive electrode current collector and a negative electrode current collector, respectively.

[0042] For example, the positive electrode active material contained in the positive electrode active material layer may include lithium composite oxide particles containing lithium and transition metals.

[0043] In some embodiments, the positive electrode active material may comprise lithium composite oxide particles represented by the following chemical formula 1.

[0044] [Chemical Formula 1]

[0045] Li x M1 a M2 b M3 c O y

[0046] In Formula 1, M1, M2, and M3 can be transition metals selected from Ni, Co, Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, or B. In Formula 1, M1, M2, and M3 can be 0. <x≤1.2,2≤y≤2.2,0<a<1,0<b<1,0<c<1,0<a+b+c≤1。

[0047] In some embodiments, the positive electrode active material may be NCM-based lithium composite oxide particles containing nickel, cobalt, and manganese. The NCM-based lithium composite oxide may be prepared, for example, by reacting a lithium precursor and an NCM precursor (e.g., an NCM oxide) with each other via a co-precipitation reaction.

[0048] However, in addition to cathode materials containing the aforementioned NCM-based lithium composite oxide particles, embodiments of the present invention can also be applied to lithium-containing lithium composite oxide cathode materials.

[0049] For example, the positive electrode can be separated and recycled from the waste lithium secondary battery. As described above, the positive electrode may include a positive electrode current collector (e.g., aluminum (Al)) and a positive electrode active material layer, and the positive electrode active material layer may also include conductive materials and binders in addition to the aforementioned positive electrode active material.

[0050] The conductive material may include, for example, carbon-based materials such as graphite, carbon black, graphene, and carbon nanotubes.

[0051] The adhesive may include, for example, resins such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, and polymethyl methacrylate.

[0052] In some exemplary embodiments, the positive electrode active material powder can be prepared by separating the positive electrode from the waste lithium secondary lithium battery and pulverizing the separated positive electrode.

[0053] For example, the pulverization can be performed using a hammer mill, shredder, cut crusher, impact crusher, etc. In this case, the positive electrode active material powder can be pulverized into powder form, and the positive electrode active material powder can simultaneously contain particles with different particle sizes.

[0054] For example, the positive electrode active material powder may have a multimodal particle size distribution. For instance, a multimodal particle size distribution can refer to a particle size distribution diagram showing multiple main peaks. In this case, the particle size of the positive electrode active material powder may be approximately 1-100 μm.

[0055] For example, the positive electrode active material powder may comprise a first active material powder, a second active material powder, and a third active material powder with different particle sizes. For example, the particle size of the first active material powder may be smaller than that of the second active material powder, and the particle size of the second active material powder may be smaller than that of the third active material powder.

[0056] For example, particles with a particle size of less than about 10 μm contained in the positive electrode active material powder can be defined as first active material powder, particles with a particle size of about 10 to 100 μm can be defined as second active material powder, and particles with a particle size of about 100 μm or more can be defined as third active material powder.

[0057] In some embodiments, the recovered positive electrode may be heat-treated prior to the pulverization. Therefore, the pulverization process can promote the desorption of the positive electrode current collector and remove at least a portion of the binder and conductive material. The heat treatment temperature may be, for example, at about 100-500°C, preferably at about 350-450°C.

[0058] For example, the positive electrode current collector can be removed by immersing the separated positive electrode in an organic solvent. The positive electrode current collector can be removed from the separated positive electrode by centrifugation, and by removing the positive electrode current collector, the mixture of positive electrode active materials can be selectively extracted.

[0059] Through the above process, the positive electrode current collector components such as aluminum are substantially completely separated and removed, and a mixture of the positive electrode active materials in which the content of the carbon-based conductive material and the carbon-based components derived from the binder is removed or reduced can be obtained.

[0060] According to an exemplary implementation, a preliminary precursor mixture can be prepared from positive electrode active material powder (e.g., step S20).

[0061] In some embodiments, a preliminary precursor mixture can be prepared by hydrogen reduction of the positive electrode active material powder. For example, the hydrogen reduction treatment can be carried out in a fluidized bed reactor comprising a reactor body whose diameter gradually decreases from top to bottom. For example, the positive electrode active material powder can be added to the fluidized bed reactor, and a reducing gas can be injected from the bottom of the fluidized bed reactor. For example, the reducing gas can be hydrogen. The structure of the fluidized bed reactor and the reactions within it are described below.

[0062] The initial precursor mixture can be generated by the reducing gas forming a cyclone from the bottom of the fluidized bed reactor and contacting the active substance powder.

[0063] For example, the reducing gas can be mixed with and injected together with the carrier gas in the lower part of the fluidized bed reactor. This improves gas-solid mixing in the fluidized bed to promote the reaction and facilitates the formation of a reaction layer of the initial precursor mixture in the fluidized bed reactor. The carrier gas may, for example, contain inert gases such as nitrogen (N2) or argon (Ar).

[0064] The preliminary precursor mixture may contain hydrogen reduction reactants of lithium-transition metal oxides contained in the active material powder. When an NCM-based lithium oxide is used as the lithium-transition metal oxide, the preliminary precursor mixture may contain reactants containing a preliminary lithium precursor and a transition metal.

[0065] The preliminary lithium precursor may comprise lithium hydroxide, lithium oxide, and / or lithium carbonate. According to an exemplary embodiment, the preliminary lithium precursor is obtained via a hydrogen reduction reaction, thus reducing the mixed content of lithium carbonate.

[0066] The reactants containing transition metals may include Ni, Co, NiO, CoO, and MnO, etc.

[0067] The hydrogen reduction reaction can be carried out at about 400-700°C, preferably at 450-550°C.

[0068] According to an exemplary implementation, a water washing process (e.g., step S30) can be performed after the initial precursor mixture is collected.

[0069] Through the aforementioned water washing process, the preliminary lithium precursor can be substantially converted into a lithium precursor composed of lithium hydroxide. For example, lithium oxide and lithium carbonate mixed in the preliminary lithium precursor can react with water to convert into lithium hydroxide, or be washed away with water. Therefore, a high-purity lithium precursor converted into the desired form of lithium hydroxide can be generated.

[0070] The initial lithium precursor is dissolved by reacting with water, thereby substantially preparing an aqueous solution of lithium hydroxide.

[0071] The reactants containing transition metals in the preliminary precursor mixture may precipitate due to insolubility in water or lack of reaction with water after the water washing treatment. Therefore, the reactants containing transition metals can be separated by filtration to obtain a lithium precursor containing high-purity lithium hydroxide.

[0072] In some embodiments, the water washing process can be carried out under conditions where carbon dioxide (CO2) is absent. For example, the water washing process can be carried out in a CO2-free atmosphere (e.g., an air atmosphere to remove CO2), thus preventing the regeneration of lithium carbonate.

[0073] In one embodiment, the water supplied during the washing process can be purged with a CO2-deficient gas (e.g., nitrogen purging) to create a CO2-free atmosphere.

[0074] In some embodiments, the reactants containing transition metals, after precipitation separation, can be treated with an acid solution to form precursors in the form of acid salts of the respective transition metals. In one embodiment, sulfuric acid can be used as the acid solution. In this case, NiSO4, MnSO4, and CoSO4 can be recovered as the transition metal precursors, respectively.

[0075] As described above, the preliminary precursor mixture generated by hydrogen reduction can be washed with water to obtain a lithium precursor that is essentially composed of lithium hydroxide. Therefore, byproducts such as lithium carbonate are prevented from forming, resulting in a positive electrode active material with higher capacity and longer lifespan.

[0076] The lithium precursor may comprise lithium hydroxide (LiOH), lithium oxide (Li2O), or lithium carbonate (Li2CO3). Lithium hydroxide is advantageous as a lithium precursor in terms of charge / discharge characteristics, lifetime characteristics, and high-temperature stability of lithium secondary batteries. For example, in the case of lithium carbonate, deposition reactions occur on the separator, which may weaken lifetime stability.

[0077] Figure 2 and Figure 3 This is a schematic diagram illustrating a fluidized bed reactor for reducing positive electrode active material according to an exemplary embodiment.

[0078] Reference Figure 2 The fluidized bed reactor 100 for reducing positive electrode active materials of the present invention may include: a reactor body 110, the diameter of which gradually decreases from top to bottom; an active material injection port 103 through which a plurality of active material powders (50, 60, 70) containing lithium composite oxide particles of different sizes are injected into the interior of the reactor body 110; and a gas injection port 105 located in the lower part of the reactor body 110, through which a reducing gas is injected to fluidize the active material powders (50, 60, 70).

[0079] According to some exemplary embodiments, the positive electrode active material powder may comprise a first active material powder 50, a second active material powder 60, and a third active material powder 70 having different particle sizes from each other.

[0080] For example, in the reactor body 110, multiple active material powders (50, 60, 70) can be fluidized separately. For example, the reactor body 110 may include multiple regions with different diameters for fluidizing the multiple active material powders (50, 60, 70) separately.

[0081] For example, the third active material powder 70 with large particle size can be fluidized in the lower part of the reactor body 110, and the first active material powder 50 with small particle size can be fluidized in the upper part of the reactor body 110.

[0082] According to some implementation schemes, the reactor body 110 may include a first region 111 for fluidizing a first active substance powder 50, a second region 112 for fluidizing a second active substance powder 60, and a third region 113 for fluidizing a third active substance powder 70.

[0083] Therefore, during the fluidization process of the positive electrode active material mixture containing multiple active material powders with different particle sizes, the problems of small-particle-size active material powder scattering and leaking or large-particle-size active material powder not being able to be sufficiently fluidized can be effectively prevented.

[0084] Furthermore, by varying the reactor diameter, temperature deviations based on location within the reactor can be reduced. This facilitates the fluidization of the positive electrode active material particles, resulting in uniform particle mixing throughout the reactor. Consequently, excellent reaction efficiency can be achieved even for particle mixtures with varying particle size distributions.

[0085] For example, the diameter D1 of the first region 111 can be larger than the diameter D2 of the second region 112, and the diameter D2 of the second region 112 can be larger than the diameter D3 of the third region 113.

[0086] In this case, the particle size of the first active material powder 50 fluidized in the first region 111 can be smaller than the particle size of the second active material powder 60 fluidized in the second region 112, and the particle size of the second active material powder 60 fluidized in the second region 112 can be smaller than the particle size of the third active material powder 70 fluidized in the third region 113.

[0087] For example, the flow rate of the reducing gas injected into the fluidized bed reactor can be inversely proportional to the square of the diameter of each region. Therefore, the flow rate of the reducing gas in the first region 111 can be slower than that in the second region 112, and the flow rate of the reducing gas in the second region 112 can be slower than that in the third region 113. Thus, in the first region 111, the first active material powder 50 with a small particle size can be easily fluidized, and in the third region 113, the third active material powder 70 with a large particle size can be easily fluidized.

[0088] According to some exemplary embodiments, the ratio of the diameter D1 of the first region 111 to the diameter D3 of the third region 113 can be 5 to 10. For example, the ratio of the diameter D2 of the second region 112 to the diameter D3 of the third region 113 can be 2 to 4.

[0089] For example, when the diameter ratio range described above is met, the fluidization of the first active material powder 50, the second active material powder 60, and the third active material powder 70 can be facilitated more easily. Therefore, the recovery efficiency of the lithium precursor can be further improved.

[0090] According to some exemplary embodiments, the first region 111, the second region 112, and the third region 113 can be sequentially arranged from the upper part of the reactor body 110. In this case, the reducing gas can be injected from the lower part to the upper part of the reactor body 110. Therefore, the diameter of each region can gradually decrease from the upper part to the lower part of the reactor body 110.

[0091] For example, as the diameter of the reactor body 110 gradually decreases from top to bottom, the flow rate of the reducing gas injected into the lower part of the reactor body 110 can gradually decrease from bottom to top. Therefore, a first active material powder 50 with a small particle size can be fluidized in a first region 111 with a large diameter, and a third active material powder 70 with a large particle size can be fluidized in a third region 113 with a small diameter.

[0092] Therefore, during the fluidization process of the positive electrode active material mixture, the problem of reduced lithium precursor recovery efficiency caused by the scattering of active material powder with small particle size or the inability to fluidize active material powder with large particle size can be prevented.

[0093] For example, the gas inlet 105 can be located at the lower part of the reactor body 110 and inject a reducing gas. The reducing gas may, for example, contain hydrogen. For example, the reducing gas can be injected from the lower part of the reactor body 110 and fluidize and reduce the positive electrode active material mixture contained inside the reactor body 110.

[0094] For example, the minimum fluidization rate described below can refer to the minimum flow rate of the reducing gas used to fluidize the positive electrode active material powder (50, 60, 70). For example, the minimum fluidization rate can be calculated using the following formula 1.

[0095] [Formula 1]

[0096]

[0097] In Equation 1, u mf It can be the minimum fluidization rate, ε mf It can be the volume fraction of active substance powder particles, d p The size of the active substance powder particles, ρ g It can be the gas density of a reducing gas, ρ s μ can be the solid density of the active substance powder particles, and μ can be the gas viscosity of the reducing gas. It can be the sphericity of the active substance powder particles, and g can be the acceleration due to gravity.

[0098] For example, the flow rate of the reducing gas in the fluidized bed reactor 100 can vary depending on the diameter of the reactor body 110 included in the fluidized bed reactor 100. For example, the flow rate of the reducing gas can decrease as the diameter of the reactor body 110 increases.

[0099] In some exemplary embodiments, the minimum flow rate in the first region 111 of the reducing gas may be below the terminal velocity of the first active material powder 50. For example, terminal velocity may refer to the velocity of a uniform motion state when an object is descending or moving in a fluid.

[0100] For example, the terminal speed can be calculated using the following formula 2.

[0101] [Equation 2]

[0102]

[0103] In equation 2, u t For terminal speed, d p The size of the active substance powder particles can be considered. It can be used to determine the sphericity of active substance powder particles.

[0104] When the minimum flow rate of the reducing gas in the first region 111 is reduced below the terminal velocity of the first active material powder 50, the problem of scattering of the first active material powder 50, which has a relatively small particle size, can be effectively prevented. Furthermore, as the first active material powder 50 can no longer rise to the top of the fluidized bed reactor 100 and descend, the content of the fluidized first active material powder 50 can be further increased. Therefore, the recovery efficiency of the lithium precursor can be further improved.

[0105] In some exemplary embodiments, the maximum flow rate in the second region 112 of the reducing gas can be greater than or equal to the minimum fluidization rate of the second active material powder 60, and the maximum flow rate in the third region 113 of the reducing gas can be greater than or equal to the minimum fluidization rate of the third active material powder 70.

[0106] In this configuration, the second active material powder 60 and the third active material powder 70, which have large particle sizes, can be fluidized more effectively. Therefore, the problem of the positive electrode active material powder failing to fluidize and depositing at the bottom of the fluidized bed reactor 100 can be effectively prevented.

[0107] In some exemplary embodiments, the reducing gas may be injected into the fluidized bed reactor 100 at a flow rate of 8-18 cm / s or higher.

[0108] For example, when the flow rate range is met, the dispersion of the first active material powder with small particle size can be prevented by the first region with a wide diameter located at the top of the fluidized bed reactor, while the third active material powder with large particle size can be effectively fluidized. Therefore, the recovery efficiency of lithium precursor can be improved.

[0109] According to some exemplary embodiments, the fluidized bed reactor 100 of the present invention for reducing positive electrode active material may include: a first connecting portion 121, the first connecting portion 121 connecting a first region 111 and a second region 112, and the diameter gradually decreasing from the first region 111 to the second region 112; and a second connecting portion 122, the second connecting portion 122 connecting the second region 112 and a third region 113, and the diameter gradually decreasing from the second region 112 to the third region 113.

[0110] In this configuration, the first connecting portion 121 and the second connecting portion 122 prevent abrupt changes in the diameter of the reactor body 110, thereby preventing a rapid decrease in the flow rate of the reducing gas within the reactor body 110. Therefore, as the flow rate of the reducing gas decreases, the problem of active material powder depositing on the sides of the reactor body 110 can be effectively prevented.

[0111] Reference Figure 3 The fluidized bed reactor for reducing positive electrode active material of the present invention may further include a gas injection port 130 disposed on the side of the connection portion 120. For example, a reducing gas or the like can be injected through the gas injection port 130. In this case, the gas injected from the gas injection port 130 can effectively prevent active material powder from depositing on the side of the connection portion 120.

[0112] According to some exemplary embodiments, the gas injection port 130 may be disposed obliquely on the side facing upward toward the reactor body 110. In this case, by disposing the gas injection port 130 facing upward toward the reactor body 110, the problem of positive electrode active material powder (50, 60, 70) depositing on the side of the connection portion 120 can be more effectively prevented.

[0113] According to some exemplary embodiments, the angle α formed between the side of the connector 120 and the gas injection port 130 can be 45-90°. When the angle α formed between the side of the connector 120 and the gas injection port 130 meets the above range, the problem of the active material powder depositing on the side of the connector 120 can be more effectively prevented.

Claims

1. A method for regenerating lithium precursors, comprising the following steps: Prepare multiple positive electrode active material powders containing lithium composite oxide particles and having different particle sizes from each other; The positive electrode active material powder is reduced in a fluidized bed reactor to prepare a preliminary precursor mixture. The fluidized bed reactor includes a reactor body whose diameter gradually decreases from top to bottom. as well as Lithium precursors are recovered from the initial precursor mixture. The positive electrode active material powder comprises a first active material powder, a second active material powder, and a third active material powder with different particle sizes. The reactor body includes a first region for fluidizing the first active substance powder, a second region for fluidizing the second active substance powder, and a third region for fluidizing the third active substance powder. The first region, the second region, and the third region are sequentially arranged from the upper part of the reactor body. The diameter of the first region is larger than the diameter of the second region, and the diameter of the second region is larger than the diameter of the third region. Wherein, the particle size of the first active substance powder is smaller than that of the second active substance powder, and the particle size of the second active substance powder is smaller than that of the third active substance powder.

2. The lithium precursor regeneration method according to claim 1, wherein, The ratio of the diameter of the first region to the diameter of the third region is 4 to 16.

3. The lithium precursor regeneration method according to claim 1, wherein, The ratio of the diameter of the second region to the diameter of the third region is 2 to 4.

4. The lithium precursor regeneration method according to claim 1, wherein, The particle size of the first active substance powder is less than 10 μm, the particle size of the second active substance powder is 10-100 μm, and the particle size of the third active substance powder is greater than 100 μm.

5. The lithium precursor regeneration method according to claim 1, wherein, The step of preparing the preliminary precursor mixture further includes injecting a reducing gas into the fluidized bed reactor.

6. The lithium precursor regeneration method according to claim 5, wherein, The minimum flow rate of the reducing gas in the first region is below the terminal velocity of the first active substance powder.

7. The lithium precursor regeneration method according to claim 5, wherein, The maximum flow rate of the reducing gas in the second region is greater than or equal to the minimum fluidization rate of the second active substance powder, and the maximum flow rate of the reducing gas in the third region is greater than or equal to the minimum fluidization rate of the third active substance powder.

8. The lithium precursor regeneration method according to claim 5, wherein, The reducing gas is injected into the fluidized bed reactor at a flow rate of 8-18 cm / s.

9. The lithium precursor regeneration method according to claim 1, wherein, The reactor body includes: a first connecting portion connecting the first region and the second region, and having a diameter that gradually decreases from the first region to the second region; and a second connecting portion connecting the second region and the third region, and having a diameter that gradually decreases from the second region to the third region.

10. The lithium precursor regeneration method according to claim 9, wherein, The first connecting portion and the second connecting portion further include gas injection ports located on the side.

11. The lithium precursor regeneration method according to claim 10, wherein, The gas injection port faces upwards from the reactor body and is inclined on the side.

12. The lithium precursor regeneration method according to claim 10, wherein, The angle formed between the side surfaces of the first and second connecting parts and the gas injection port is 45-90°.

13. A fluidized bed reactor for reducing positive electrode active material, comprising: The reactor body, the diameter of which gradually decreases from top to bottom; An active material injection port is used to inject multiple positive electrode active material powders containing lithium composite oxide particles of different particle sizes into the interior of the reactor body; and A gas injection port is located at the lower part of the reactor body, through which a reducing gas for fluidizing the active substance powder is injected. The positive electrode active material powder comprises a first active material powder, a second active material powder, and a third active material powder with different particle sizes. The reactor body includes a first region for fluidizing the first active substance powder, a second region for fluidizing the second active substance powder, and a third region for fluidizing the third active substance powder. The first region, the second region, and the third region are sequentially arranged from the upper part of the reactor body. The diameter of the first region is larger than the diameter of the second region, and the diameter of the second region is larger than the diameter of the third region. Wherein, the particle size of the first active substance powder is smaller than that of the second active substance powder, and the particle size of the second active substance powder is smaller than that of the third active substance powder.

14. The fluidized bed reactor for reducing positive electrode active material according to claim 13, wherein, The reactor body includes: a first connecting portion connecting the first region and the second region, and having a diameter that gradually decreases from the first region to the second region; and a second connecting portion connecting the second region and the third region, and having a diameter that gradually decreases from the second region to the third region.

15. The fluidized bed reactor for reducing positive electrode active material according to claim 14, wherein, The first connecting portion and the second connecting portion further include gas injection ports located on the side.

Citation Information

Patent Citations

  • Method for recovering active metals from lithium secondary battery

    CN111936423A