A chlorinated polyolefin-modified waterborne modified acrylate emulsion, and a preparation method and application thereof

Aqueous modified acrylate emulsions were prepared by copolymerizing modified chlorinated polyolefins with acrylate monomers, which solved the problem of poor adhesion between lithium-ion battery separators and ceramics, improved the air permeability of the separators and battery performance, and achieved environmentally friendly preparation of aqueous emulsions.

CN116836654BActive Publication Date: 2026-11-20MEISHAN JINGRUI ELECTRONIC MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310757658.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-07
Publication Date
2026-11-20
Estimated Expiration
2042-01-07

AI Technical Summary

Technical Problem

The existing lithium-ion battery separator has poor adhesion to ceramics, causing lithium-ion batteries to detach during cycling. In addition, the existing solvent-based coating slurry is not environmentally friendly.

Method used

Modified chlorinated polyolefins, such as maleic anhydride or acrylic acid grafted polyvinyl chloride or polypropylene chloride, are copolymerized with acrylate monomers to form an aqueous modified acrylate emulsion. Modified latex is then prepared through emulsion polymerization, thereby achieving the hydration of chlorinated polyolefins and improving adhesion performance.

Benefits of technology

It improves the adhesion between the lithium-ion battery separator and ceramic, enhances the air permeability of the separator and reduces the moisture content, improves the electrical performance of the battery, and the product is an environmentally friendly water-based emulsion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004303428390000051
    Figure BDA0004303428390000051
  • Figure BDA0004303428390000052
    Figure BDA0004303428390000052
  • Figure BDA0004303428390000061
    Figure BDA0004303428390000061
Patent Text Reader

Abstract

The application discloses a kind of water-based modified acrylate emulsion and its preparation method and application in lithium ion battery separator adhesive.The polymerization monomer of water-based modified acrylate emulsion includes acrylate, aromatic monomer and optional other monomers, water-based modified acrylate emulsion also includes modified chlorinated polyolefin, modified chlorinated polyolefin is maleic anhydride or acrylate graft chlorinated polyolefin, chlorinated polyolefin is polyvinyl chloride or polychloropropylene, acrylate, aromatic monomer and optional other monomers are copolymerized to form latex, and modified chlorinated polyolefin is coated in the latex.The application realizes its hydration by dissolving modified chlorinated polyolefin in monomer first, then participating in pre-emulsion polymerization, the water-based modified acrylate emulsion obtained has improved adhesion, when used for lithium ion battery separator bonding, the bonding performance and air permeability of separator are both improved, and moisture content is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention is a divisional application filed on January 7, 2022, with application number 202210015478.6, entitled "An Aqueous Modified Acrylic Emulsion and Its Preparation Method and Application". Technical Field

[0002] This invention belongs to the field of waterborne acrylic emulsions, specifically relating to a chlorinated polyolefin-modified waterborne acrylic emulsion, its preparation method, and its application. Background Technology

[0003] Currently, the main adhesive for lithium-ion battery separators is polyacrylate emulsion. Due to the low surface energy of the separator, it is difficult to wet the separator. Even if the surface tension of the adhesive is reduced, its wetting effect on the separator is still average, resulting in poor adhesion between the separator and the ceramic. Ultimately, this leads to severe detachment during lithium-ion battery cycling.

[0004] In existing technologies, the adhesion between the separator and the ceramic can be improved by adding the adhesion promoter polyvinyl chloride (PVC), thereby enhancing the electrochemical performance of lithium-ion batteries. For example, Chinese patent CN108963150A discloses a battery separator coating slurry, the components of which include PVC, a binder, and a solvent, wherein the binder includes an aqueous acrylic resin solution. This patent's PVC-containing coating slurry is a solvent-based formulation, which cannot be well hydrated and mixed with the aqueous acrylic resin solution. PVC's ability to improve the adhesion and permeability of the acrylic resin is insufficient, and the solvent-based nature of the product is not safe or environmentally friendly. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a new water-based modified acrylate emulsion. Using this water-based modified acrylate emulsion as a separator binder can achieve good bonding between the lithium-ion battery separator and the ceramic, resulting in high air permeability and low moisture content in the separator, thereby improving the electrical performance of the lithium-ion battery.

[0006] To achieve the above objectives, a first aspect of the present invention provides an aqueous modified acrylate emulsion, wherein the polymeric monomers of the aqueous modified acrylate emulsion include acrylate, aromatic monomers and optional other monomers, and the aqueous modified acrylate emulsion further includes a modified chlorinated polyolefin, wherein the modified chlorinated polyolefin is maleic anhydride or acrylic acid-grafted chlorinated polyolefin, wherein the chlorinated polyolefin is polyvinyl chloride or polyvinyl chloride, wherein the acrylate, aromatic monomers and optional other monomers copolymerize to form a latex, and the modified chlorinated polyolefin is encapsulated in the latex.

[0007] The meaning of "optional" is that it can be selected or not, that is, the polymerized monomer may include other monomers or may not include other monomers.

[0008] Furthermore, the number-average molecular weight of the modified chlorinated polyolefin is below 50,000.

[0009] Furthermore, the modified chlorinated polyolefin contains 1-5% by mass of maleic anhydride or acrylic acid.

[0010] Furthermore, the acrylates include methyl methacrylate, butyl acrylate, and isooctyl acrylate.

[0011] Furthermore, the aromatic monomer is selected from one or both of styrene and methylstyrene.

[0012] Furthermore, the optional other monomers are selected from one or more combinations of acrylic acid, methacrylic acid, acrylamide, methacrylamide, hydroxyethyl acrylate, and hydroxyethyl methacrylate.

[0013] More preferably, the optional other monomer is acrylamide.

[0014] In some embodiments of the present invention, the ratio of the acrylate, aromatic monomer and other monomers by weight is 240-350:50-100:5-10.

[0015] In some embodiments of the present invention, the solid content of the water-based modified acrylate emulsion is 30-50% by mass, the viscosity is 10-200 mPa·s, and the particle size of the latex is 200-500 nm.

[0016] In some embodiments of the present invention, the modified chlorinated polyolefin accounts for 1-5% of the mass of the latex.

[0017] As some preferred embodiments of the present invention, the composition of the polymeric monomer, by weight, is as follows:

[0018] 180-200 parts of butyl acrylate;

[0019] 10-50 parts of methyl methacrylate;

[0020] 50-100 parts of isooctyl acrylate;

[0021] 50-100 parts of styrene;

[0022] Acrylamide 5-10 parts.

[0023] More preferably, the waterborne modified acrylate emulsion is obtained by polymerizing the monomers in water in the presence of the modified chlorinated polyolefin, initiator, and emulsifier, wherein, by weight, the modified chlorinated polyolefin is 10-20 parts, the initiator is 0.1-5 parts, the emulsifier is 1-10 parts, and the water is 600-1000 parts.

[0024] Furthermore, the initiator is preferably ammonium persulfate.

[0025] This invention creatively employs maleic anhydride or acrylic acid graft-modified polyvinyl chloride (PVC) or polypropylene (PPC), first dissolving it in liquid monomers. Then, a pre-emulsion is prepared by combining the monomer mixture with emulsifiers, water, and other raw materials. The pre-emulsion is then subjected to emulsion polymerization, and the comonomers undergo emulsion polymerization to obtain a latex that coats the modified PVC or PP in the polymer system. This allows for the effective hydration of hydrophobic PVC or PP in the emulsion system, resulting in a significantly improved adhesive property of the modified PVC or PP-modified acrylate emulsion. This emulsion can be used as a separator binder in lithium-ion batteries, improving the adhesion between the separator and ceramic, thereby enhancing the electrical performance of lithium-ion batteries. Furthermore, because the product is in water-based emulsion form, it is safer and more environmentally friendly than solvent-based slurries.

[0026] The present invention further provides a method for preparing the aforementioned waterborne modified acrylate emulsion, wherein the polymeric monomer includes at least a polymeric monomer that is liquid at room temperature, and the method includes the step of dissolving the modified chlorinated polyolefin using the liquid polymeric monomer, and the step of emulsion polymerization of the polymeric monomer containing the dissolved modified chlorinated polyolefin and other polymeric monomers in water in the presence of an initiator and an emulsifier.

[0027] In some embodiments of the present invention, the polymeric monomer further includes a polymeric monomer that is solid at room temperature, and the method includes the following steps:

[0028] 1) The modified chlorinated polyolefin is dissolved in a liquid polymeric monomer to obtain a liquid monomer mixture. An emulsifier and a solid polymeric monomer are added to water, and then the liquid monomer mixture is added to prepare a pre-emulsion.

[0029] 2) Heat the reactor to 80-85℃, add part of the pre-emulsion and part of the initiator to the reactor, and react for 20-40 minutes;

[0030] 3) At 85-90℃, add the remaining pre-emulsion and the remaining initiator dropwise into the reactor;

[0031] 4) After the addition is complete, keep the temperature at 85-90℃ for 2-4 hours.

[0032] Furthermore, in step 1), the liquid polymerization monomer is butyl acrylate, methyl methacrylate, styrene, and isooctyl acrylate, and the solid polymerization monomer is acrylamide.

[0033] Furthermore, the emulsifier is selected from one or more combinations of anionic surfactants and nonionic surfactants.

[0034] Further, in step 1), the liquid monomer mixture is added under stirring, and after the addition is complete, the mixture is stirred for 20-40 minutes to prepare the pre-emulsion.

[0035] Further, in step 2), 20-30% by mass of pre-emulsion and 20-30% by mass of initiator are added.

[0036] Furthermore, in step 3), the remaining pre-emulsion is added over a period of 3-4 hours, and the remaining initiator is added over a period of 3-4 hours.

[0037] Furthermore, the method also includes step 5) cooling and filtering.

[0038] The present invention also relates to the use of the aforementioned water-based modified acrylate emulsion as a separator binder in lithium-ion batteries.

[0039] Furthermore, the present invention also provides a lithium-ion battery comprising a separator, the separator comprising a substrate and an adhesive, wherein the adhesive comprises an aqueous modified acrylate emulsion according to the present invention.

[0040] Furthermore, the adhesion between the substrate and the adhesive is greater than 25N, the air permeability is greater than 190S / 100cc, and the moisture content is less than 540ppm.

[0041] Furthermore, the lithium-ion battery is a power battery, providing power to tools. Even further, it is a battery that powers electric vehicles, electric trains, electric bicycles, golf carts, and the like.

[0042] Due to the implementation of the above technical solutions, the present invention has the following advantages compared with the prior art:

[0043] Chlorinated polyethylene or chlorinated polypropylene are hydrophobic polymers that are difficult to emulsify in water. Directly mixing them with aqueous acrylate emulsions cannot produce a uniform and stable aqueous emulsion. This invention uses modified chlorinated polyethylene or chlorinated polypropylene and a special polymerization process to achieve the hydration of chlorinated polyethylene or chlorinated polypropylene, thereby preparing a stable aqueous acrylate emulsion modified with chlorinated polyethylene or chlorinated polypropylene.

[0044] This invention uses hydrophilic monomers, such as maleic anhydride or acrylic acid, to graft-modify polyvinyl chloride (PVC) or polypropylene (PPC). The introduction of these hydrophilic monomers allows the modified PVC or PCC to dissolve in the monomers. Water and emulsifiers are then added to form a pre-emulsion, which is then prepared using a dropwise starved emulsion polymerization method to form a modified latex. The latex obtained from the copolymerization of the comonomers coats the modified chlorinated polyolefin, thereby achieving the hydration of the hydrophobic PVC or PCC adhesion promoter. The resulting waterborne modified acrylic emulsion exhibits significantly improved adhesion properties. When used for bonding lithium-ion battery separators, it enhances the adhesion and permeability of the separator while reducing its moisture content. Detailed Implementation

[0045] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In the present invention, unless otherwise specified, when referring to content or percentage (%), it refers to mass content and mass percentage.

[0046] Example 1

[0047] Mix 200 parts by weight of butyl acrylate, 30 parts by weight of methyl methacrylate, 75 parts by weight of styrene, and 80 parts by weight of isooctyl acrylate. Add 15 parts by weight of maleic anhydride-grafted polyvinyl chloride (molecular weight of 50,000, maleic anhydride content of 1%) and stir until the maleic anhydride-grafted polyvinyl chloride is completely dissolved to obtain a liquid monomer mixture. Add 5 parts by weight of emulsifier SDS and 8 parts by weight of acrylamide to 700 parts by weight of deionized water and stir until dissolved. Slowly add the liquid monomer mixture while stirring and stir for 30 minutes until the stirred liquid becomes a milky white emulsion, thus preparing the pre-emulsion. The reactor was heated to 82°C, and 1 / 4 of the pre-emulsion and 1 / 4 of the ammonium persulfate were added to the reactor. The reaction was allowed to proceed for 30 minutes. The remaining pre-emulsion and initiator were then added dropwise to the reactor at 88°C, with the pre-emulsion added for 180 minutes and the initiator added for 190 minutes. After the addition was complete, the mixture was kept at 86°C for 4 hours. The mixture was then cooled to 45°C, filtered, and bottled to obtain an aqueous modified acrylate emulsion with a viscosity of 20 mPa·s and a latex particle size of 290 nm.

[0048] Example 2

[0049] The preparation process of the waterborne modified acrylate emulsion is basically the same as in Example 1, except that maleic anhydride-grafted polyvinyl chloride is replaced with acrylic acid-grafted polyvinyl chloride (molecular weight of 40,000, mass percentage of acrylic acid of 2.4%). A waterborne modified acrylate emulsion is obtained with a viscosity of 15 mPa·s and a latex particle size of 300 nm.

[0050] Example 3

[0051] The preparation process of the waterborne modified acrylate emulsion is basically the same as in Example 1, except that maleic anhydride-grafted polyvinyl chloride is replaced with maleic anhydride-grafted polyvinyl chloride (molecular weight of 35,000, mass percentage of maleic anhydride of 3.5%). A waterborne modified acrylate emulsion is obtained with a viscosity of 18 mPa·s and a latex particle size of 356 nm.

[0052] Example 4

[0053] The preparation process of the waterborne modified acrylate emulsion is basically the same as in Example 1, except that maleic anhydride-grafted polyvinyl chloride is replaced with acrylic acid-grafted polyvinyl chloride (molecular weight of 20,000, mass percentage of acrylic acid of 4%). A waterborne modified acrylate emulsion is obtained with a viscosity of 18 mPa·s and a latex particle size of 340 nm.

[0054] Comparative Example 1

[0055] The preparation process of the ordinary acrylic emulsion is basically the same as in Example 1, except that maleic anhydride-grafted polyvinyl chloride is not added. An ordinary acrylic emulsion is obtained with a viscosity of 16 mPa·s and a latex particle size of 321 nm.

[0056] Comparative Example 2

[0057] When 200 parts by weight of butyl acrylate, 30 parts by weight of methyl methacrylate, 75 parts by weight of styrene and 80 parts by weight of isooctyl acrylate were mixed and 15 parts by weight of polyvinyl chloride with a molecular weight of 50,000 were added, it was found that the mixture could not be dissolved and subsequent pre-emulsion polymerization could not be carried out.

[0058] Example 5

[0059] The water-based modified acrylic emulsions of Examples 1-4 and the ordinary acrylic emulsion of Comparative Example 1 were used to prepare the binder for the lithium-ion battery separator. This binder was then used to bond the PE substrate to prepare the separator. The separator preparation process employed common techniques in this field. The formulation of the separator binder is shown in Table 1 below.

[0060] Table 1

[0061]

[0062] The obtained diaphragm was tested, and the results of the adhesion between the substrate PE and the adhesive (which forms a coating), the air permeability of the diaphragm, and the moisture content are shown in Table 2.

[0063] Table 2

[0064]

[0065]

[0066] It is evident that after modifying the acrylate emulsion with modified chlorinated polyolefin, the adhesion between the substrate PE and the binder (forming a coating) is significantly improved, the air permeability of the diaphragm is enhanced, and the moisture content is reduced.

[0067] Example 6

[0068] The process for preparing the diaphragm is basically the same as in Example 5, except that the amount of acrylic emulsion is reduced and the formulation of the diaphragm binder is shown in Table 3 below.

[0069] Table 3

[0070]

[0071] The obtained diaphragm was tested, and the results of the adhesion between the substrate PE and the adhesive (which forms a coating), the air permeability of the diaphragm, and the moisture content are shown in Table 4.

[0072] Table 4

[0073]

[0074]

[0075] It is evident that when the amount of modified acrylic emulsion is reduced, the adhesion between the substrate PE and the adhesive (which forms a coating) remains unchanged, the air permeability is improved, and the moisture content is significantly reduced.

[0076] It should be noted that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments have been described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0077] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A separator binder for lithium-ion batteries, comprising an aqueous modified acrylate emulsion, wherein the monomers of the aqueous modified acrylate emulsion include acrylates, aromatic monomers, and other monomers besides acrylates and aromatic monomers, characterized in that: The aqueous modified acrylate emulsion further includes a modified chlorinated polyolefin, wherein the modified chlorinated polyolefin is maleic anhydride or acrylic acid-grafted chlorinated polyolefin, and the chlorinated polyolefin is polyvinyl chloride or polyvinyl chloride. The acrylate, aromatic monomers, and other monomers copolymerize to form a latex, and the modified chlorinated polyolefin is encapsulated in the latex. The mass percentage of maleic anhydride or acrylic acid in the modified chlorinated polyolefin is 1-5%; the modified chlorinated polyolefin accounts for 1-5% of the mass of the latex. The acrylate is a mixture of methyl methacrylate, butyl acrylate, and isooctyl acrylate; the aromatic monomer is selected from one or two of styrene and methylstyrene; the other monomers are selected from one or more combinations of acrylic acid, methacrylic acid, acrylamide, and methacrylamide. The feed ratio of the acrylate, aromatic monomer and other monomers by mass is 240-350:50-100:5-10; The aqueous modified acrylate emulsion is prepared by a method comprising the steps of dissolving the modified chlorinated polyolefin using acrylate and aromatic monomers, and emulsion polymerization of the polymeric monomers and other monomers containing the modified chlorinated polyolefin in water in the presence of an initiator and an emulsifier.

2. The separator adhesive for lithium-ion batteries according to claim 1, characterized in that: The modified chlorinated polyolefin has a number average molecular weight of less than 50,000; and / or the waterborne modified acrylate emulsion has a solid content of 30-50% by mass, a viscosity of 10-200 mPa·s, and a latex particle size of 200-500 nm.

3. The separator adhesive for lithium-ion batteries according to claim 1 or 2, characterized in that: The composition of the polymeric monomer, by weight, is as follows: 180-200 parts of butyl acrylate; 10-50 parts of methyl methacrylate; 50-100 parts of isooctyl acrylate; 50-100 parts of styrene; Acrylamide 5-10 parts.

4. The separator adhesive for lithium-ion batteries according to claim 3, characterized in that: The waterborne modified acrylate emulsion is obtained by polymerizing the monomers in water in the presence of the modified chlorinated polyolefin, initiator, and emulsifier, wherein, by weight, the modified chlorinated polyolefin is 10-20 parts, the initiator is 0.1-5 parts, the emulsifier is 1-10 parts, and the water is 600-1000 parts.

5. A method for preparing a separator binder for a lithium-ion battery according to any one of claims 1 to 4, characterized in that: The method includes the steps of dissolving the modified chlorinated polyolefin using acrylates and aromatic monomers, and the steps of emulsion polymerization of the polymeric monomers and other monomers containing the dissolved modified chlorinated polyolefin in water in the presence of an initiator and an emulsifier.

6. The method for preparing a separator binder for lithium-ion batteries according to claim 5, characterized in that: The polymeric monomer further includes polymeric monomers that are solid at room temperature, and the method includes the following steps: 1) The modified chlorinated polyolefin is dissolved in a mixture of acrylate and aromatic monomers to obtain a liquid monomer mixture. An emulsifier and a solid polymeric monomer are added to water, and then the liquid monomer mixture is added to prepare a pre-emulsion. 2) Heat the reactor to 80-85℃, add part of the pre-emulsion and part of the initiator to the reactor, and react for 20-40 minutes; 3) At 85-90℃, add the remaining pre-emulsion and the remaining initiator dropwise into the reactor; 4) After the addition is complete, keep the temperature at 85-90℃ for 2-4 hours.

7. The method for preparing a separator binder for lithium-ion batteries according to claim 6, characterized in that: The aromatic monomer is styrene, and the solid polymeric monomer is acrylamide; and / or, the emulsifier is selected from one or more combinations of anionic surfactants and nonionic surfactants.

8. The method for preparing a separator binder for lithium-ion batteries according to claim 6, characterized in that: In step 1), the liquid monomer mixture is added under stirring, and after the addition is complete, the mixture is stirred for 20-40 minutes to prepare the preemulsion; and / or, in step 2), 20-30% by mass of the preemulsion and 20-30% by mass of the initiator are added; and / or, in step 3), the remaining preemulsion is added over a period of 3-4 hours, and the remaining initiator is added over a period of 3-4 hours; and / or, the method further includes step 5), cooling and filtration.

Citation Information

Patent Citations

  • Coating slurry for diaphragm and preparation method thereof, battery diaphragm, and lithium-ion battery

    CN108963150A

  • Waterborne polyvinyl chloride-based adhesive emulsion and preparation method thereof

    CN109161025A