Preparation method of anti-humidity formaldehyde sensor material and device application thereof

By using a composite material of fluorine-containing organic functionalized graphene and oxygen-vacancy-rich oxides, and activating it with visible light catalysis, the problems of low response and high humidity influence of traditional formaldehyde sensors at room temperature have been solved, achieving high sensitivity and moisture resistance for formaldehyde detection.

CN116840316BActive Publication Date: 2026-11-24SOUTH CHINA NORMAL UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310825170.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2026-11-24
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

Traditional semiconductor resistive formaldehyde sensors struggle to achieve high response and low detection limits at room temperature, and are susceptible to environmental humidity, leading to decreased sensitivity and accuracy.

Method used

A formaldehyde sensor material with moisture resistance is formed by using fluorine-containing organic functionalized graphene and oxygen-vacancy-rich oxide composite materials, activated by visible light catalysis, and combined with non-covalent bonds such as π-π, hydrogen bonds, and electrostatic forces.

Benefits of technology

It achieves rapid response and recovery of trace formaldehyde at room temperature, with a detection limit as low as 5 ppb, and is moisture resistant, avoiding safety hazards and sensitivity degradation caused by high-temperature operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116840316B_ABST
    Figure CN116840316B_ABST
Patent Text Reader

Abstract

This invention discloses a moisture-resistant formaldehyde sensor material and its device applications. The moisture-resistant formaldehyde sensor material comprises fluorinated organic molecule functionalized graphene and oxygen-vacancy-containing oxide; the mass ratio of the oxygen-vacancy-containing oxide to the fluorinated organic molecule functionalized graphene is 100:(0.5-10). This invention provides a formaldehyde sensing material with visible light photocatalytic activation and moisture-resistant properties. This material effectively combines oxygen-vacancy-rich oxide and functionalized graphene. The oxygen vacancies in the oxide can regulate the absorption of the composite material under visible light. The fluorinated organic molecule functionalized graphene provides a pathway for accepting and transferring photoelectrons, and the presence of fluorine enhances the material's moisture resistance. When irradiated with visible light, it can rapidly respond to and recover from trace amounts of formaldehyde at room temperature, exhibiting high sensitivity and a detection limit as low as 5 ppb.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of gas-sensitive materials technology, specifically to a method for preparing a moisture-resistant formaldehyde sensor material and its device application. Background Technology

[0002] Formaldehyde (HCHO) is a major pollutant causing indoor air pollution. It is found in commonly used engineered wood products, paints, carpets, and wallpapers in interior decoration. Studies have shown that because formaldehyde can bind to and interact with various proteins, inhaling excessive amounts can cause severe burning and irritation of the respiratory tract, local edema, and trigger various respiratory diseases such as chronic bronchitis and asthma. Contact with skin can cause allergic reactions and even skin necrosis. Prolonged exposure to high concentrations of formaldehyde can lead to many potential health risks, such as memory loss, autonomic nervous system disorders, immune system disorders, and even cancer. According to my country's national standard GB / T16127-1995, the maximum permissible concentration of formaldehyde in indoor air is 0.08 mg / m³. 3 (Approximately 80 ppb at room temperature), therefore, the detection of low concentrations of formaldehyde in indoor environments has become an urgent problem to be solved in modern life.

[0003] Traditional semiconductor resistive sensors typically use metal oxides. While metal oxides offer advantages such as excellent gas-sensing performance, low cost, and wide availability, they are difficult to manufacture for high-response, low-detection-limit sensors. Furthermore, their high operating temperature (200–500°C) requires a stable heat source to respond to gases. However, high temperatures can degrade sensor lifespan, increase manufacturing complexity, and lead to sensitivity degradation. High-temperature environments also pose safety hazards. Recent research has found that ultraviolet (UV) light irradiation can effectively reduce the operating temperature of metal oxide sensors; however, short-wavelength UV light still consumes significant power, and prolonged exposure can even cause damage and harm to humans. In contrast, visible light has lower energy consumption and is more environmentally friendly, posing less harm to humans and making it a better choice for activating gas sensors. Through years of research, the performance of gas sensors has been greatly improved. However, ambient humidity significantly affects the baseline and sensitivity of gas-sensitive materials, reducing sensor accuracy and greatly complicating sensor calibration. Therefore, developing a universal method to address the humidity sensitivity issue of gas sensors is of great importance. Summary of the Invention

[0004] To overcome the shortcomings of the prior art, the present invention provides a formaldehyde sensor material with visible light catalytic activation and moisture resistance, and a method for preparing the same.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] The first aspect of this invention provides a moisture-resistant formaldehyde sensor material, the moisture-resistant formaldehyde sensor material comprising fluorine-containing organic molecule functionalized graphene and oxygen-vacancy-containing oxides;

[0007] The mass ratio of the oxygen-containing vacancy oxide to the fluorine-containing organic functionalized graphene is 100:(0.5-10).

[0008] The fluorinated organic molecules described in this invention can bind to graphene through non-covalent bonds such as π-π, hydrogen bonds, electrostatic forces, van der Waals forces, and hydrophobic forces, without damaging the inherent properties of graphene.

[0009] The oxygen-vacancy-containing oxide described in this invention is an oxide rich in oxygen vacancies obtained by any means, and the oxygen-vacancy-containing oxide has visible light absorption characteristics.

[0010] Preferably, the mass ratio of the oxygen-containing vacancy oxide to the fluorine-containing organic functionalized graphene is 100:(1-10); in some preferred embodiments of the present invention, the mass ratio of the oxygen-containing vacancy oxide to the fluorine-containing organic functionalized graphene is 100:1.

[0011] Preferably, the particle size of the oxygen-containing vacancy oxide is 10-100 nm; more preferably, the particle size of the oxygen-containing vacancy oxide is 40-60 nm.

[0012] Preferably, the oxygen-vacancy-containing oxide is an oxygen-vacancy-containing metal oxide, which includes at least one of indium oxide, zinc oxide, tungsten oxide, tin oxide, and titanium dioxide; more preferably, the oxygen-vacancy-containing metal oxide includes at least one of indium oxide and zinc oxide.

[0013] Preferably, the oxygen-containing vacancy oxide is prepared by a method comprising the following steps: dispersing metal nitrate and urea in a solvent, reacting at 70-90°C for 10-14 hours, then centrifuging, washing, drying, and calcining under a protective atmosphere to obtain the oxygen-containing vacancy oxide.

[0014] More preferably, in the method for preparing the oxygen-containing vacancy oxide, the solvent includes N,N-dimethylformamide (DMF).

[0015] More preferably, in the method for preparing the oxygen-containing vacancy oxide, the molar ratio of the metal nitrate to urea is 1:(10-50).

[0016] More preferably, in the method for preparing the oxygen-containing vacancy oxide, the centrifugation speed is 9000-11000 r / min and the time is 5-15 min.

[0017] More preferably, in the method for preparing the oxygen-containing vacancy oxide, the drying temperature is 50-70℃ and the drying time is 20-28h.

[0018] More preferably, in the method for preparing the oxygen-containing vacancy oxide, the calcination temperature is 350-450℃ and the calcination time is 1-3h; even more preferably, in the method for preparing the oxygen-containing vacancy oxide, the calcination temperature is 380-420℃ and the calcination time is 1.5-2.5h.

[0019] Preferably, the fluorinated organic functionalized graphene is obtained by supramolecular assembly of fluorinated organic molecules and graphene oxide; the fluorinated organic molecules include 8-(trifluoromethyl)quinoline-4-amine (CasNo: 243977-15-3 ), 8-fluoroquinoline-4-amine (CasNo: 148401-38-1 ), 4-amino-2,8-bis(trifluoromethyl)-quinoline (CasNo: 917561-99-0 ), 6-trifluoromethyl-4-aminoquinoline (CasNo: 247113-89-9 ), 7-(trifluoromethyl)-1H-indazole-3-amine (CasNo: 60330-35-0 At least one of the following.

[0020] Preferably, the mass ratio of the fluorinated organic molecule to graphene oxide is (5-100):1.

[0021] Preferably, the fluorine-containing organic functionalized graphene is prepared by a method comprising the following steps:

[0022] Fluorine-containing organic molecules were dispersed in an alcohol solution, and graphene oxide dispersion was added. The mixture was stirred and reacted at 90-130℃ for 4-8 hours. After filtration, the fluorine-containing organic molecule functionalized graphene was obtained.

[0023] More preferably, in the preparation method of the fluorinated organic molecular functionalized graphene, the reaction is carried out at 95-125℃ for 5-7 hours, followed by filtration to obtain the fluorinated organic molecular functionalized graphene.

[0024] In this invention, the graphene oxide dispersion can be graphene oxide dispersed in an aqueous solution, an alcohol solution, or other conventional solvents.

[0025] A second aspect of the present invention provides a method for preparing the aforementioned formaldehyde-resistant sensor material, comprising the following steps:

[0026] The oxygen-containing vacancy oxide was dispersed in a fluorine-containing organic molecule functionalized graphene dispersion, and then subjected to ultrasonication, centrifugation, and drying to obtain the moisture-resistant formaldehyde sensor material.

[0027] Preferably, the centrifugation speed is 7000-9000 r / min and the time is 5-15 min.

[0028] Preferably, the drying temperature is 50-70℃ and the drying time is 10-14h.

[0029] A third aspect of the present invention provides a formaldehyde sensor, comprising:

[0030] Gas-sensitive electrode; the surface of the gas-sensitive electrode is coated with the moisture-resistant formaldehyde sensor material;

[0031] Light source; used to irradiate the gas-sensitive electrode;

[0032] Measurement circuit; used to connect the gas-sensitive electrode.

[0033] Preferably, the wavelength of the light source is 390-780nm; the light source of the present invention can use a wavelength of 400-650nm, or white light (mixed light); more preferably, the wavelength of the light source is 400-650nm; in some preferred embodiments of the present invention, the wavelength of the light source is 405nm.

[0034] Preferably, the intensity of the light source is 0.1-10 mW / cm². 2 .

[0035] Compared with the prior art, the beneficial effects of the present invention are:

[0036] This invention provides a formaldehyde sensing material with visible light catalytic activation and moisture resistance. This material effectively combines oxygen-vacancy-rich oxides and functionalized graphene. The oxygen vacancies in the oxides regulate the absorption of the composite material under visible light, while the F-containing functionalized graphene provides a pathway for accepting and transferring photoelectrons, and the presence of F enhances the material's moisture resistance. When irradiated with visible light, it exhibits rapid response and recovery to trace amounts of formaldehyde at room temperature, demonstrating high sensitivity and a detection limit as low as 5 ppb.

[0037] This invention provides a formaldehyde sensing material that is activated by visible light catalysis and has moisture resistance. Compared with the prior art, this method optimizes the amount of fluorine-containing organic functionalized graphene incorporated into oxygen-vacancy-rich oxides, adjusts the light absorption capacity of the composite material under visible light, and its ability to resist water molecules in the atmosphere, and successfully prepares a formaldehyde sensing material that is activated by visible light catalysis and has moisture resistance.

[0038] This invention provides a formaldehyde sensing material with visible light photocatalytic activation and moisture resistance. The material uses simple, non-toxic, and low-cost raw materials. During the reaction, fluorine-containing organic molecules are bonded to graphene through non-covalent bonds such as π-π, hydrogen bonds, electrostatic forces, van der Waals forces, and hydrophobic interactions. This process preserves the two-dimensional planar structure and intrinsic properties of graphene while improving the dispersibility of the reduced graphene and avoiding its self-conjugated stacking. Furthermore, the introduction of fluorine-containing organic molecules enhances the material's moisture resistance.

[0039] This invention provides a method for preparing a formaldehyde sensing material with visible light catalytic activation and moisture resistance, which improves upon the problems of high operating temperature, low sensitivity, and susceptibility to humidity associated with traditional metal oxide materials. This preparation method is simple, environmentally friendly, and uses low visible light energy, posing no harm to the human body. Attached Figure Description

[0040] Figure 1 This is a flowchart illustrating the preparation process of the moisture-resistant formaldehyde sensing material according to an embodiment of the present invention.

[0041] Figure 2 The images show the SEM morphology and particle size distribution of the oxygen-vacancy-rich metal oxide from Example 1 of this invention.

[0042] Figure 3 SEM images of reduced graphene oxide and reduced graphene oxide functionalized with F-containing organic molecules;

[0043] Figure 4 SEM morphology image of the moisture-resistant formaldehyde sensing material prepared in an embodiment of the present invention;

[0044] Figure 5 The infrared spectra of the reduced graphene oxide and the reduced graphene oxide functionalized with F-containing organic molecules of the present invention are shown.

[0045] Figure 6 This is a comparison of the response of the composite material prepared in Example 1 of the present invention to 800 ppb formaldehyde with the response of the oxide rich in oxygen vacancies to formaldehyde.

[0046] Figure 7 The results of the cyclic stability test of ATQ-rGO@In2O3-1 prepared in Example 1 of this invention against 100ppb formaldehyde are shown.

[0047] Figure 8 The test curves and linear fitting curves of ATQ-rGO@In2O3-1 prepared in Example 1 of this invention against different concentrations of formaldehyde are shown.

[0048] Figure 9The test curves of ATQ-rGO@In2O3-1 prepared in Example 1 of the present invention under 405nm wavelength visible light irradiation, different humidity levels, and the same concentration of formaldehyde are shown.

[0049] Figure 10 The selective test results of ATQ-rGO@In2O3-1 prepared in Example 1 of the present invention for formaldehyde detection under visible light irradiation at a wavelength of 405nm are shown.

[0050] Figure 11 The test curves of ATQ-rGO@ZnO-1 prepared in Example 2 of the present invention under 405nm wavelength visible light irradiation and at different humidity levels with the same concentration of formaldehyde are shown.

[0051] Figure 12 The test curves of ATQ-rGO@In2O3-1 in Example 3 of the present invention under white light (mixed light) irradiation and at different humidity levels for the same concentration of formaldehyde;

[0052] Figure 13 The test curves of rGO@In2O3-1 prepared in Comparative Example 1 of this invention under 405nm wavelength visible light irradiation, different humidity levels, and the same concentration of formaldehyde are shown. Detailed Implementation

[0053] The specific embodiments of the present invention will be further described below. It should be noted that these descriptions are for the purpose of aiding understanding the present invention, but do not constitute a limitation thereof. Furthermore, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0054] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods, and the experimental materials used in the following embodiments are all available through conventional commercial channels.

[0055] Example 1

[0056] This embodiment synthesizes a visible-light-activated, moisture-resistant formaldehyde sensing material doped with oxygen-vacancy-rich indium oxide and containing the F-organic molecule (8-(trifluoromethyl)quinoline-4-amine) functionalized graphene, and performs formaldehyde gas-sensing performance testing, such as... Figure 1 As shown, the specific steps are as follows:

[0057] S1. Disperse 1 mmol of indium nitrate and 0.03 mol of urea in 60 mL of N,N-dimethylformamide (DMF), stir magnetically to form a transparent solution, and react at 80 °C for 12 h.

[0058] S2. The product obtained in step S1 is centrifuged at 10000 r / min for 10 min, the supernatant is discarded, the precipitate is washed three times with anhydrous ethanol, and dried at 60℃ for 24 h to obtain ordinary indium oxide white blocky substance. It is then ground to obtain white solid powder. The white indium oxide powder is then calcined at 400℃ for 2 h in an argon atmosphere to obtain light yellow granular indium oxide nanoparticles rich in oxygen vacancies with a diameter of 40-60 nm.

[0059] S3. 1000 mg of 8-(trifluoromethyl)quinoline-4-amine (ATQ) was dispersed in anhydrous ethanol, and 1 mL of graphene oxide dispersion (10 mg / mL) was added to it. The mixture was stirred at 60 °C for 1 hour, and then transferred to a reaction vessel. The mixture was reacted at 120 °C for 5 hours to allow ATQ to fully assemble with graphene through π-π interactions and to completely reduce graphene oxide, thereby obtaining ATQ-modified reduced graphene oxide.

[0060] S4. After cooling to ambient temperature, filter the product to remove excess solvent and ATQ, and then redisperse it in 10 mL of anhydrous ethanol to obtain a stable supramolecular assembly ATQ-rGO dispersion.

[0061] S5. Add 50 mg of indium oxide nanoparticles prepared in step S2, 0.5 mL of ATQ-rGO dispersion and 5 mL of anhydrous ethanol into a beaker and disperse evenly (the mass ratio of indium oxide to functionalized graphene is 100:1). After sonicating this mixture at room temperature for 30 minutes, supramolecular assembly dispersion A is obtained.

[0062] S6. After centrifuging the product at 8000 rpm for 10 minutes, redisperse it in 5 mL of anhydrous ethanol to obtain functionalized graphene indium oxide composite material dispersion B.

[0063] S7. Dry in a vacuum oven at 60℃ for 12 hours to obtain product C, which is the visible light photocatalytic activated formaldehyde sensor material with moisture resistance, denoted as ATQ-rGO@In2O3-1.

[0064] SEM images of indium oxide rich in oxygen vacancies, such as Figure 2 As shown in (a), indium oxide is in the form of uniform particles, with most particles having a diameter between 40 and 60 nm. Figure 2 -(b) is a particle size distribution diagram of indium oxide particles.

[0065] SEM electron microscopy analysis of the functionalized graphene material containing F organic molecules prepared by S3 revealed that the functionalized reduced graphene oxide was in sheet form (e.g., Figure 3 -b), compared to unfunctionalized graphene (such as... Figure 3-a) It can be seen that the modification containing F molecules reduces the stacking of graphene, as shown in the infrared spectrum (e.g. Figure 5 The results show that the F-containing molecules were successfully assembled with reduced graphene oxide.

[0066] The SEM morphology of the prepared composite material ATQ-rGO@In2O3-1 is as follows: Figure 4 As shown, indium oxide particles are uniformly distributed on both sides of the functionalized graphene. Figure 4 Figures a and b in the image are both SEM images of ATQ-rGO@In2O3-1.

[0067] The operation steps of the ATQ-rGO@In2O3-1 composite material in gas sensitive monitoring in this invention are as follows:

[0068] Step 1: Take 10 μL of the above dispersion B and coat it onto the interdigitated electrode, then dry it at 70°C to obtain the electrode for gas-sensitive testing.

[0069] Step 2: Fix a visible light source with a wavelength of 405nm 1.5cm directly above the interdigitated electrodes, and adjust the light density of the source to 1.5mW / cm². 2 The electrode plates are connected to the gas-sensitive testing equipment, providing a 1V bias voltage to the interdigital electrodes of the sensor and a 2V voltage for visible light, and the gas-sensitive test is performed under 405nm light irradiation.

[0070] Test results show that the ATQ-rGO@In2O3-1 composite material exhibits significantly improved performance in response to 800ppb HCHO under a visible light source at a wavelength of 405nm compared to pure indium oxide. Figure 6 Meanwhile, the response value to 100 ppb HCHO is as high as 1.41, and it has good cyclic response characteristics. Figure 7 Simultaneously, concentration gradient tests were performed on the sensor, and linear fitting was conducted. It can be seen that this embodiment exhibits a good linear relationship with different formaldehyde concentrations, and this embodiment successfully reduced the detection limit of formaldehyde to 5 ppb. Figure 8 ).

[0071] Step 3: Fix a visible light source with a wavelength of 405nm 1.5cm directly above the interdigitated electrodes, and adjust the light source density to 1.5mW / cm². 2 The electrode pads are connected to the gas-sensitive testing equipment, providing a 1V bias voltage to the interdigital electrodes of the sensor and a 2V voltage for visible light. Gas-sensitive tests are conducted under different humidity conditions under 405nm light irradiation.

[0072] Test results show that the ATQ-rGO@In2O3-1 composite material exhibits a relatively stable response value to 800 ppb HCHO under different humidity conditions. Figure 9As can be seen, the composite material of graphene functionalized with F-containing organic molecules and indium oxide rich in oxygen vacancies possesses certain moisture resistance. Furthermore, selective testing was performed on the sensor prepared using the sensing material of Example 1, and the results are as follows... Figure 10 As shown. By Figure 10 The results show that the sensing material prepared in Example 1 has excellent selectivity for formaldehyde detection.

[0073] Example 2

[0074] This embodiment synthesizes a visible-light-activated, moisture-resistant formaldehyde sensing material by synthesizing F-containing organic molecule (8-(trifluoromethyl)quinoline-4-amine) functionalized graphene doped with oxygen-vacancy-rich zinc oxide, and tests its formaldehyde gas-sensing performance. The specific steps are as follows:

[0075] S1. 1000 mg of 8-(trifluoromethyl)quinoline-4-amine (ATQ) was dispersed in anhydrous ethanol, and 1 mL of graphene oxide dispersion (10 mg / mL) was added. The mixture was stirred at 60 °C for 1 hour, then transferred to a reaction vessel and reacted at 120 °C for 5 hours. This allowed ATQ to fully assemble with graphene through π-π interactions and be completely reduced, resulting in ATQ-modified reduced graphene oxide.

[0076] S2. After cooling to ambient temperature, the product is filtered to remove excess solvent and free ATQ, and then redispersed in 10 mL of anhydrous ethanol to obtain a stable supramolecular assembly ATQ-rGO dispersion.

[0077] S3. Add 50 mg of zinc oxide nanoparticles containing oxygen vacancies prepared according to the method in Example 1, 0.5 mL of ATQ-rGO dispersion and 5 mL of anhydrous ethanol into a beaker and disperse evenly (the mass ratio of zinc oxide to functionalized graphene is 100:1). After sonicating this mixture at room temperature for 30 minutes, supramolecular assembly dispersion A is obtained.

[0078] S4. After centrifuging the product at 8000 rpm for 15 minutes, redisperse it in 5 mL of anhydrous ethanol to obtain functionalized graphene zinc oxide composite material dispersion B.

[0079] S5. Dry in a vacuum oven at 60℃ for 12 hours to obtain product C, which is the visible light photocatalytic activated formaldehyde sensor material with moisture resistance, denoted as ATQ-rGO@ZnO-1.

[0080] The operation steps of the ATQ-rGO@ZnO-1 composite material in gas-sensitive monitoring in this invention are as follows:

[0081] Step 1: Take 10 μL of the above dispersion B and coat it onto the interdigitated electrode, then dry it at 70°C to obtain the electrode for gas-sensitive testing.

[0082] Step 2: Fix a visible light source with a wavelength of 405nm 1.5cm directly above the interdigitated electrodes, and adjust the light density of the source to 1.5mW / cm². 2 The electrode pads were connected to the gas-sensitive testing equipment, providing a 1V bias voltage to the interdigital electrodes of the sensor and a 2V voltage for visible light. Gas-sensitive tests were conducted under 405nm light irradiation and at different humidity levels.

[0083] Test results show that the ATQ-rGO@ZnO-1 composite material exhibits the following response values ​​to 500 ppb HCHO under different humidity conditions: Figure 11 It can be seen that the composite material of graphene functionalized with organic molecules and zinc oxide rich in oxygen vacancies has certain moisture resistance, which further confirms that the composite of graphene functionalized with F organic molecules and metal oxide rich in oxygen vacancies has moisture resistance.

[0084] Example 3

[0085] This embodiment prepares a gas-sensitive composite material. The difference between this embodiment and embodiment 1 is that in the gas-sensitive detection step 2, the 405nm visible light source is replaced with a commonly used white light (mixed light) source, such as a mobile phone light or a flashlight. Other operations are the same as in embodiment 1.

[0086] Test results show that the ATQ-rGO@In2O3-1 composite material exhibits a response value as high as 1.48 to 1 ppm HCHO under commonly used white light (mixed light) and different humidity conditions. Figure 12 As shown, the ATQ-rGO@In2O3-1 composite material exhibits similar response values ​​to formaldehyde under commonly used white light (mixed light) light sources and different humidity levels, indicating that the composite material made of graphene with a few molecules of F functionalized and indium oxide rich in oxygen vacancies has certain moisture resistance properties.

[0087] Comparative Example 1

[0088] The synthesis and testing of formaldehyde sensing materials based on unfunctionalized reduced graphene doped with indium oxide were performed in this comparative example. The specific steps are as follows:

[0089] S1. Disperse 2.5 mL of graphene oxide dispersion (10 mg / mL) in anhydrous ethanol, stir at 60 °C for 1 hour, then transfer to a reaction vessel and react at 120 °C for 5 hours to obtain reduced graphene oxide.

[0090] S2. After cooling to ambient temperature, filter the product to remove excess solvent, and redisperse it in 10 mL of anhydrous ethanol to obtain rGO dispersion.

[0091] S3. Add 50 mg of indium oxide nanoparticles, 0.5 mL of rGO dispersion and 5 mL of anhydrous ethanol to a beaker and disperse evenly (the mass ratio of indium oxide to reduced graphene oxide is 100:1). After mixing, sonicate at room temperature for 30 minutes to obtain dispersion A.

[0092] S4. After centrifuging the product at 8000 rpm for 15 minutes, redisperse it in 5 mL of anhydrous ethanol to obtain reduced graphene oxide indium oxide composite material dispersion B.

[0093] S5 was dried in a vacuum oven at 60℃ for 12 h to obtain the control product C, denoted as rGO@In2O3-1.

[0094] The operation steps of the rGO@In2O3-1 composite material in gas-sensitive monitoring in this invention are as follows:

[0095] Step 1: Take 10 μL of the above dispersion B and coat it onto the interdigitated electrode, then dry it at 70°C to obtain the electrode for gas-sensitive testing.

[0096] Step 2: Fix a visible light source with a wavelength of 405nm 1.5cm directly above the interdigitated electrodes, and adjust the light source density to 2mW / cm². 2 The electrode plates are connected to the gas-sensitive testing equipment, providing a 1V bias voltage to the interdigital electrodes of the sensor and a 2V voltage for visible light, and the gas-sensitive test is performed under 405nm light irradiation.

[0097] Step 3: Fix a visible light source with a wavelength of 405nm 1.5cm directly above the interdigitated electrodes, and adjust the light source density to 1.5mW / cm². 2 The electrode pads are connected to the gas-sensitive testing equipment, providing a 1V bias voltage to the interdigital electrodes of the sensor and a 2V voltage for visible light. Gas-sensitive tests are conducted under different humidity conditions under 405nm light irradiation.

[0098] Test results show that the response value of rGO@In2O3-1 composite material to 1 ppm HCHO decreases with increasing humidity under different humidity conditions. Figure 13 It can be seen that the composite material of reduced graphene oxide and oxygen-vacancy-rich indium oxide does not have moisture resistance, which further illustrates that fluorine-containing organic molecule functionalized graphene effectively improves the moisture resistance of the composite material.

[0099] The embodiments of the present invention have been described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and these variations still fall within the protection scope of the present invention.

Claims

1. A moisture-resistant formaldehyde sensor material, characterized in that, The moisture-resistant formaldehyde sensor material comprises fluorine-containing organic molecular functionalized graphene and oxygen-vacancy-containing oxides. The mass ratio of the oxygen-containing vacancy oxide to the fluorine-containing organic molecule functionalized graphene is 100:(0.5-10). The oxygen-vacancy-containing oxide is an oxygen-vacancy-containing metal oxide, which includes at least one of indium oxide, zinc oxide, tungsten oxide, tin oxide, and titanium dioxide. The fluorinated organic molecule functionalized graphene is obtained by supramolecular assembly of fluorinated organic molecules and graphene oxide. The preparation method is as follows: fluorinated organic molecules are dispersed in an alcohol solution, graphene oxide dispersion is added, stirred, reacted at 90-130 °C for 4-8 h, filtered, and the fluorinated organic molecule functionalized graphene is obtained. The fluorinated organic molecule includes at least one of 8-(trifluoromethyl)quinoline-4-amine, 8-fluoroquinoline-4-amine, 4-amino-2,8-bis(trifluoromethyl)-quinoline, 6-trifluoromethyl-4-aminoquinoline, and 7-(trifluoromethyl)-1H-indazole-3-amine.

2. The moisture-resistant formaldehyde sensor material according to claim 1, characterized in that, The particle size of the oxygen-containing vacancy oxide is 10-100 nm.

3. The moisture-resistant formaldehyde sensor material according to claim 2, characterized in that, The oxygen-containing vacancy oxide is prepared by a method comprising the following steps: dispersing metal nitrate and urea in a solvent, reacting at 70-90°C for 10-14 hours, then centrifuging, washing, drying, and calcining under a protective atmosphere to obtain the oxygen-containing vacancy oxide.

4. The moisture-resistant formaldehyde sensor material according to claim 1, characterized in that, The mass ratio of the fluorinated organic molecules to graphene oxide is (5-100):

1.

5. A method for preparing the moisture-resistant formaldehyde sensor material according to any one of claims 1-4, characterized in that, Includes the following steps: The oxygen-containing vacancy oxide was dispersed in a fluorine-containing organic molecule functionalized graphene dispersion, and then subjected to ultrasonication, centrifugation, and drying to obtain the moisture-resistant formaldehyde sensor material.

6. A formaldehyde sensor, characterized in that, include: Gas-sensitive electrode; the surface of the gas-sensitive electrode is coated with the moisture-resistant formaldehyde sensor material according to any one of claims 1-4; Light source; used to irradiate the gas-sensitive electrode; Measurement circuit; used to connect the gas-sensitive electrode.

7. The formaldehyde sensor according to claim 6, characterized in that, The wavelength of the light source is 390-780 nm.

8. The formaldehyde sensor according to claim 6, characterized in that, The intensity of the light source is 0.1-10 mW / cm². 2 .

Citation Information

Patent Citations

  • Composite material as well as preparation method and application thereof

    CN113443646A