Aluminum corrosion inhibitor and method of making and using same
By preparing an aluminum corrosion inhibitor with a specific ratio of alcohol ether phosphate, the problems of low-temperature precipitation and excessive foaming of traditional aluminum corrosion inhibitors were solved, achieving a stable and foam-free effect at room temperature, thus improving processing quality and tool life.
Patent Information
- Application Number
- CN202311055834.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-21
AI Technical Summary
Traditional aluminum corrosion inhibitors tend to precipitate solids or generate a large amount of foam at low temperatures, affecting lubrication and cooling effects, resulting in poor surface quality and accelerated tool wear.
Using compounds A and B in a specific ratio, alcohol ether phosphates are prepared through esterification and addition reactions to form an aluminum corrosion inhibitor, which includes a mixture of fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide. The esterification and addition reaction conditions are controlled to ensure good low-temperature performance and low foaming properties.
It achieves long-term stability of aluminum corrosion inhibitor without precipitation at room temperature, and does not generate a large amount of foam during use. It has good low-temperature performance and low foaming properties, which improves the surface quality of the machined surface and the tool life.
Smart Images

Figure CN116855944B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of processing fluids, and in particular to an aluminum corrosion inhibitor, its preparation method, and its application. Background Technology
[0002] Metalworking fluids are liquids used in metalworking, including cutting oils and cutting fluids, primarily serving functions such as lubrication, cooling, rust prevention, rust inhibition, and cleaning. Water-based cutting fluids can be classified into emulsions, semi-synthetic cutting fluids, and fully synthetic cutting fluids. The classification of emulsions, semi-synthetic, and fully synthetic usually depends on the type of base oil in the product. Emulsions are water-soluble cutting fluids that use only mineral oil as a base oil; semi-synthetic cutting fluids contain both mineral oil and chemically synthesized base oils; and fully synthetic cutting fluids use only chemically synthesized base oils (i.e., no mineral oil). The metalworking fluid industry is used in industries such as automotive parts, machinery manufacturing, mold making, shipbuilding, aerospace, and metallurgy. In metalworking, aluminum and aluminum alloys are commonly processed materials. Aluminum alloy cutting fluids are formulated with lubricants, rust inhibitors, aluminum corrosion inhibitors, emulsifiers, and antioxidants, and are used in the processing of aluminum and aluminum alloys.
[0003] Traditional aluminum corrosion inhibitors mainly include chromates, silicates, and phosphates. However, chromium in chromates is extremely harmful to the human body and is rarely used nowadays. Silicates were a commonly used aluminum corrosion inhibitor in the past, but they tend to flocculate and fail over long-term use, mainly due to hydrolysis. At slightly higher concentrations, surface crystallization can occur, making them less than ideal aluminum corrosion inhibitors. While traditional phosphate-based aluminum corrosion inhibitors offer some aluminum corrosion inhibition, they have two drawbacks: firstly, poor low-temperature performance, remaining solid or partially precipitating at room temperature, making them inconvenient to use; secondly, excessive foaming, which can lead to a large amount of air mixed in with the liquid pumped to the machining area, forming a gas-liquid mixture that affects lubrication and cooling, resulting in poor surface finish, burns, and accelerated tool wear. Summary of the Invention
[0004] Therefore, in order to solve the problems of poor low-temperature performance and excessive foaming of aluminum corrosion inhibitors, it is necessary to provide an aluminum corrosion inhibitor that combines corrosion inhibition, good low-temperature performance, and low foaming, as well as its preparation method and application.
[0005] This invention provides an aluminum corrosion inhibitor, comprising compound A and compound B in a mass ratio of (20-70):(20-70); wherein, the structural formula of compound A is as follows: The structural formula of compound B is as follows: R is selected from substituted or unsubstituted straight-chain or branched alkyl groups of C10 to C20, m is selected from integers from 1 to 10, and n is selected from integers from 1 to 20.
[0006] In one embodiment, R is selected from substituted or unsubstituted straight-chain or branched alkane groups of C14 to C18.
[0007] This application also provides a method for preparing the aluminum corrosion inhibitor as described above, comprising the following steps: mixing fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide in a molar ratio of (2-4):1, and carrying out an esterification reaction, wherein the structural formula of the fatty alcohol polyoxyethylene polyoxypropylene ether is as follows:
[0008] In one embodiment, the preparation of the fatty alcohol polyoxyethylene polyoxypropylene ether includes the following steps: mixing fatty alcohol, ethylene oxide and propylene oxide in a molar ratio of 1:(1-10):(1-20) and carrying out an addition reaction.
[0009] In one embodiment, the conditions for the addition reaction include: a temperature of 90°C to 160°C, a pressure of 0.2 MPa to 0.8 MPa, and a reaction time of 1 hour to 6 hours.
[0010] In one embodiment, a catalyst of 0.1% to 1% by total mass of the fatty alcohol, ethylene oxide, and propylene oxide is also added.
[0011] In one embodiment, the catalyst comprises one or more of sodium hydroxide and potassium hydroxide.
[0012] In one embodiment, the fatty alcohol includes one or more of stearyl alcohol, palmitol, lauryl alcohol, and cinnamyl alcohol.
[0013] In one embodiment, the conditions for the esterification reaction include: a temperature of 30°C to 120°C and a reaction time of 1 hour to 10 hours.
[0014] Furthermore, this application also provides a metalworking fluid, including the aluminum corrosion inhibitor described above.
[0015] The aforementioned aluminum corrosion inhibitor, by limiting the structure and ratio of its composition to include two alcohol ether phosphate esters, not only satisfies the corrosion inhibition effect on aluminum and aluminum alloys, but also achieves good low-foaming and low-temperature properties, as well as no precipitation during long-term storage at room temperature and no excessive foaming during use. Attached Figure Description
[0016] Figure 1 The infrared spectrum of stearyl alcohol polyoxyethylene polyoxypropylene ether phosphate in Example 5 is shown. Detailed Implementation
[0017] This invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this invention. Of course, they are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different instances. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or settings discussed.
[0018] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of the invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified. In the description of the present invention, "a number" means at least one, such as one, two, etc., unless otherwise explicitly specified.
[0019] Unless otherwise specified, all percentages, fractions, and ratios are calculated based on the total mass of the compositions of the present invention. Unless otherwise specified, all masses of the listed ingredients give an amount of active substance and therefore do not include solvents or byproducts that may be present in commercially available materials. The term "percentage by mass" may be expressed by the symbol "%".
[0020] The terms “comprising,” “including,” “containing,” “having,” “comprising,” or other variations thereof are intended to cover non-closed inclusion, and no distinction is made between these terms. The term “comprising” means that other steps and ingredients may be added without affecting the final result. The term “comprising” also includes the terms “consisting of” and “substantially composed of.” The compositions and methods / processes of the present invention comprise, consist of, and substantially consist of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. No distinction is made between the terms “efficacy,” “performance,” “effect,” and “potency” herein.
[0021] The terms "preferred," "more preferably," etc., used in this invention refer to embodiments of the invention that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this invention.
[0022] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0024] This invention provides an aluminum corrosion inhibitor, comprising compound A and compound B in a mass ratio of (20-70):(20-70); wherein, the structural formula of compound A is as follows: The structural formula of compound B is
[0025] R is selected from substituted or unsubstituted straight-chain or branched alkyl groups of C10 to C20, m is selected from integers from 1 to 10, and n is selected from integers from 1 to 20.
[0026] Furthermore, the mass ratio of compound A to compound B may be, but is not limited to, 10:10, 20:30, 10:20, 20:50, 10:30, 20:70, 30:20, 30:40, 30:50, 30:70, 20:10, 40:50, 40:70, 50:20, 50:30, 50:40, 50:60, 50:70, 30:10, 60:50, 60:70, 70:20, 70:30, 70:40, 70:50, or 70:60.
[0027] In a specific example, R is selected from substituted or unsubstituted straight-chain or branched alkane groups of C14 to C18.
[0028] Furthermore, R is selected from C 18 H 37 O-, C 16 H 33 O-, C 12 H 25 O- or C 14 H 29 O-.
[0029] This application also provides a method for preparing the aluminum corrosion inhibitor as described above, comprising the following steps: mixing fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide in a molar ratio of (2-4):1, and carrying out an esterification reaction, wherein the structural formula of the fatty alcohol polyoxyethylene polyoxypropylene ether is as follows:
[0030] Furthermore, the molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide is (2.5–3.5):1. Specifically, the molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide can be, but is not limited to, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, or 3.5:1.
[0031] In a specific example, the esterification reaction conditions include: a temperature of 30°C to 120°C and a reaction time of 1 hour to 10 hours.
[0032] Furthermore, the esterification reaction temperature is 50℃~100℃, and the esterification reaction time is 2 hours~6 hours. Specifically, the esterification reaction temperature can be, but is not limited to, 50℃, 60℃, 65℃, 70℃, 75℃, 80℃, 90℃ or 100℃, and the esterification reaction time can be, but is not limited to, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0033] In a specific example, the preparation of fatty alcohol polyoxyethylene polyoxypropylene ether includes the following steps: mixing fatty alcohol, ethylene oxide and propylene oxide in a molar ratio of 1:(1-10):(1-20) and carrying out an addition reaction.
[0034] Furthermore, an addition reaction is carried out by mixing fatty alcohol, ethylene oxide, and propylene oxide in a molar ratio of 1:(1-8):(5-14). Specifically, the molar ratio between fatty alcohol, ethylene oxide, and propylene oxide can be, but is not limited to, 1:1:5, 1:1:6, 1:1:7, 1:1:8, 1:1:9, 1:1:10, 1:1:11, 1:1:12, 1:1:13, 1:1:14, or 1:2:5. 1:2:6, 1:2:7, 1:2:8, 1:2:9, 1:2:10, 1:2:11, 1:2:12, 1:2:13, 1:2:14, 1:3:5, 1:3:6, 1:3:7, 1:3:8, 1:3:9, 1:3:10, 1:3:11, 1:3:13, 1:3:13, 1:3:14, 1:4:5, 1:4:6, 1:4:7, 1:4:8, 1 :4:9, 1:4:10, 1:4:11, 1:4:14, 1:4:14, 1:4:14, 1:5:5, 1:5:6, 1:5:7, 1:5:8, 1:5:9, 1:5:10, 1:5:11, 1:5:12, 1:5:13, 1:5:14, 1:6:5, 1:6:6, 1:6:7, 1:6:8, 1:6:9, 1:6:10, 1:6:11 1:6:12, 1:6:13, 1:6:14, 1:7:5, 1:7:6, 1:7:7, 1:7:8, 1:7:9, 1:7:10, 1:7:11, 1:7:12, 1:7:13, 1:7:14, 1:8:5, 1:8:6, 1:8:7, 1:8:8, 1:8:9, 1:8:10, 1:8:11, 1:8:12, 1:8:13, or 1:8:14.
[0035] In a specific example, the conditions for the addition reaction include: a temperature of 90℃ to 160℃, a pressure of 0.2MPa to 0.8MPa, and a reaction time of 1 hour to 6 hours.
[0036] Furthermore, the conditions for the addition reaction include: a temperature of 120℃ to 150℃, a pressure of 0.3MPa to 0.6MPa, and a time of 2 hours to 6 hours. Specifically, the temperature of the addition reaction can be, but is not limited to, 120℃, 130℃, 140℃, or 150℃; the pressure of the addition reaction can be, but is not limited to, 0.3MPa, 0.4MPa, 0.5MPa, or 0.6MPa; and the time of the addition reaction can be, but is not limited to, 2 hours, 3 hours, 4 hours, 5 hours, or 6 hours.
[0037] In one specific example, a catalyst comprising 0.1% to 1% of the total mass of fatty alcohol, ethylene oxide, and propylene oxide is also added. Preferably, a catalyst comprising 0.1% to 0.5% of the total mass of fatty alcohol, ethylene oxide, and propylene oxide is also added; specifically, the catalyst may be, but is not limited to, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5% of the total mass of the raw materials.
[0038] In one specific example, the catalyst includes one or more of sodium hydroxide and potassium hydroxide. Preferably, the catalyst is potassium hydroxide.
[0039] In one specific example, fatty alcohols include one or more of stearyl alcohol, palmitol, lauryl alcohol, and cinnamyl alcohol.
[0040] Furthermore, this application also provides a metalworking fluid, including the aluminum corrosion inhibitor described above.
[0041] The aforementioned aluminum corrosion inhibitor, by limiting the structure and ratio of its composition to include two alcohol ether phosphate esters, not only satisfies the corrosion inhibition effect on aluminum and aluminum alloys, but also achieves good low-foaming and low-temperature properties, as well as no precipitation during long-term storage at room temperature and no excessive foaming during use.
[0042] The following specific embodiments further illustrate the aluminum corrosion inhibitor of the present invention, its preparation method, and its application in detail. Unless otherwise specified, all raw materials involved in the following specific embodiments are commercially available.
[0043] Example 1
[0044] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 40.7:45.2. as well as R is C 12 H 25 O-, m is 2, n is 8.
[0045] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Lauryl alcohol is added to a pressure reactor as a catalyst for fatty alcohol and potassium hydroxide, nitrogen gas is introduced for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:2:8, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0046] The above-mentioned liquid was added into a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0047] Example 2
[0048] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 40.3:45.0. as well as R is C 14 H 29 O-, m is 2, n is 8.
[0049] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Myristol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:2:8, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0050] The above-mentioned liquid was added into a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0051] Example 3
[0052] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 38.8:38.8. as well as R is C 16 H 33 O-, m is 2, n is 8.
[0053] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Palm alcohol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:2:8, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0054] The above-mentioned liquid was added into a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0055] Example 4
[0056] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 38.8:44.0. as well as R is C 18 H 37 O-, m is 2, n is 8.
[0057] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Stearyl alcohol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:2:8, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0058] The above-mentioned liquid was added into a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0059] Example 5
[0060] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 37.9:43.6. as well as R is C 18 H 37 O-, m is 3, n is 7.
[0061] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Stearyl alcohol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:3:7, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0062] The above-mentioned liquid was added to a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3:1. The temperature was controlled at 65-75°C, and the reaction was continued for 4 hours after the addition was complete to obtain the aluminum corrosion inhibitor of this embodiment. The infrared spectrum of the product of this embodiment is shown below. Figure 1 As shown.
[0063] Example 6
[0064] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 43.6:43.6. as well as R is C 18 H 37 O-, m is 4, n is 6.
[0065] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Stearyl alcohol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:4:6, and the amount of potassium hydroxide catalyst added is 0.2% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0066] The above-mentioned liquid was added to a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 2.5:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0067] Example 7
[0068] This embodiment provides an aluminum corrosion inhibitor, which comprises aluminum corrosion inhibitors in a mass ratio of 28.3:46.6. as well as R is C 18 H 37 O-, m is 6, n is 11.
[0069] The preparation method of the aluminum corrosion inhibitor in this embodiment is as follows: Stearyl alcohol is added to a pressure reactor as a fatty alcohol and potassium hydroxide catalyst, nitrogen gas is purged for protection, and the temperature is raised to about 100°C to remove moisture under vacuum. When the reactor temperature rises to 130-140°C, ethylene oxide is introduced, and after the reaction is complete, propylene oxide is introduced. The molar ratio of fatty alcohol, ethylene oxide, and propylene oxide is 1:6:11. The amount of potassium hydroxide catalyst added is 0.4% of the total mass of the raw materials. After the reaction reaches a constant pressure of 0.4 MPa, the temperature is lowered to 60°C, and the material is filtered out to obtain fatty alcohol polyoxyethylene polyoxypropylene ether.
[0070] The above-mentioned liquid was added to a glass flask, heated to 65°C, and phosphorus pentoxide was added in batches with stirring. The molar ratio between fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide was 3.5:1. The temperature was controlled at 65-75°C. After the addition was completed, the reaction continued for 4 hours to obtain the aluminum corrosion inhibitor of this embodiment.
[0071] The different preparation parameters of Examples 1 to 7 are summarized in the table below.
[0072]
[0073] Comparative Example 1
[0074] The difference between Comparative Example 1 and Example 5 is that Comparative Example 1 does not contain ethylene oxide.
[0075] Comparative Example 2
[0076] The difference between Comparative Example 2 and Example 5 is that Comparative Example 2 does not contain propylene oxide.
[0077] Comparative Example 3
[0078] The difference between Comparative Example 3 and Example 5 is that Comparative Example 3 does not contain phosphorus pentoxide.
[0079] Comparative Example 4
[0080] The difference between Comparative Example 4 and Example 5 lies in the preparation method. The preparation method for this comparative example is as follows: stearyl alcohol and potassium hydroxide catalyst are added to a pressure reactor, nitrogen gas is introduced for protection, and the temperature is raised to approximately 100°C to remove moisture under vacuum. Once the reactor temperature reaches 130–140°C, ethylene oxide and propylene oxide are introduced. After the reaction reaches a constant pressure, the temperature is lowered to 60°C, phosphorus pentoxide is added, and the temperature is controlled at 65–75°C. After the addition is complete, the reaction continues for 4 hours. The material is then filtered to obtain the aluminum corrosion inhibitor of this comparative example.
[0081] The mass determination of compounds A and B in the above embodiments refers to the detection method for lauryl phosphate in QB / T 4948-2016.
[0082] A comparative experiment was conducted to test the corrosion resistance of aluminum alloys using the aluminum corrosion inhibitors provided in the above embodiments and comparative examples. The test methods are as follows:
[0083] Aluminum sheets of grades 606, 7071, and ADC12 were polished to a smooth and bright finish on 230-grit sandpaper and cleaned with alcohol. A test solution was prepared by mixing 0.02% phosphate ester and 1% triethanolamine, then adding 98.98% tap water. The three polished aluminum alloys were semi-immersed in the test solution and dried in a 55°C oven for 1 hour before testing. The triethanolamine was obtained from Petronas. Testing and grading were performed according to GB / T 6144-2010, with grade A being rust-free and having a new shine, grade B being slightly darkened, grade C being moderately darkened, and grade D being severely darkened. The test results are shown in the table below.
[0084] Test sample name Aluminum sheet corrosion Example 1 Grade B Example 2 Grade B Example 3 Grade B Example 4 Grade B Example 5 Grade A Example 6 Grade A Example 7 Grade B Comparative Example 1 Class C Comparative Example 2 Grade B Comparative Example 3 Class D Comparative Example 4 Class C
[0085] The test results in Table 2 demonstrate that the aluminum corrosion inhibitors provided in this embodiment have excellent corrosion inhibition effects. Specifically, the aluminum corrosion inhibitors provided in Examples 5 and 6 exhibit excellent corrosion inhibition effects on aluminum, showing no corrosion. Comparative Examples 1-3 show that the aluminum corrosion inhibitor of this invention is prepared by a stepwise synthesis reaction of fatty alcohols, ethylene oxide, propylene oxide, and phosphorus pentoxide. Its corrosion inhibition effect on aluminum is significantly reduced compared to aluminum corrosion inhibitors lacking any one of these components. Comparative Example 4 shows that the aluminum corrosion inhibitor prepared by the method of this invention has better corrosion inhibition effects than aluminum corrosion inhibitors prepared by other methods.
[0086] Foam comparison experiments were conducted on Examples 5, 6, and Comparative Examples 2-4, respectively.
[0087] The foam test method is as follows: Add 1% aluminum corrosion inhibitor to 99% tap water to obtain the test working solution. Take 50ml and place it in a graduated cylinder, stopper it, and shake it evenly and quickly thirty times by hand. Then let the graduated cylinder stand, press the stopwatch and read the foam height simultaneously, and record the foam height data at 1min, 2min, and 3min. The test results are shown in the table below.
[0088]
[0089] The results above show that the aluminum etching solution prepared in this embodiment has low foam and fast defoaming. Compared with Comparative Examples 2-3, it can be seen that the aluminum corrosion inhibitor prepared by the present invention using several raw materials in a stepwise synthesis reaction has lower foam than that prepared without adding propylene oxide or phosphorus pentoxide. Propylene oxide plays a good role in suppressing foam in the aluminum corrosion inhibitor prepared by the present invention. As shown in Comparative Example 4, the aluminum corrosion inhibitor prepared by the method of the present invention has lower foam than that prepared by other methods. The foam in Example 5 of Examples 2, 5 and 6 is even lower, and the foam stabilizes after 1 minute.
[0090] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0091] The above-described embodiments are merely illustrative of several implementation methods of the present invention, facilitating a detailed and specific understanding of the technical solutions of the present invention. However, they should not be construed as limiting the scope of protection of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. It should be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided by the present invention through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this invention patent should be determined by the content of the appended claims, and the specification can be used to interpret the content of the claims.
Claims
1. An aluminum corrosion inhibitor, characterized in that, The mixture includes compound A and compound B in a mass ratio of (30~50):(40~50); wherein the structural formula of compound A is [insert structural formula here]. The structural formula of compound B is as follows: R is selected from C 18 H 37 O-, m is 3, n is 7, or m is 4, n is 6.
2. A method for preparing the aluminum corrosion inhibitor as described in claim 1, characterized in that, The process includes the following steps: mixing fatty alcohol polyoxyethylene polyoxypropylene ether and phosphorus pentoxide in a molar ratio of (2.5~3):1, and carrying out an esterification reaction, wherein the structural formula of the fatty alcohol polyoxyethylene polyoxypropylene ether is as follows: R is selected from C 18 H 37 O-.
3. The method for preparing the aluminum corrosion inhibitor as described in claim 2, characterized in that, The preparation of the fatty alcohol polyoxyethylene polyoxypropylene ether includes the following steps: mixing stearyl alcohol, ethylene oxide and propylene oxide in a molar ratio of 1: (3~4): (6~7) and carrying out an addition reaction.
4. The method for preparing the aluminum corrosion inhibitor as described in claim 3, characterized in that, The conditions for the addition reaction include: the temperature of the addition reaction is 90℃~160℃, the pressure of the addition reaction is 0.2MPa~0.8MPa, and the time of the addition reaction is 1 hour~6 hours.
5. The method for preparing the aluminum corrosion inhibitor as described in claim 3, characterized in that, A catalyst of 0.1% to 1% by total mass of the stearyl alcohol, ethylene oxide, and propylene oxide is also added.
6. The method for preparing the aluminum corrosion inhibitor as described in claim 5, characterized in that, The catalyst includes one or both of sodium hydroxide and potassium hydroxide.
7. The method for preparing the aluminum corrosion inhibitor according to any one of claims 2 to 6, characterized in that, The conditions for the esterification reaction include: a temperature of 30℃ to 120℃ and a reaction time of 1 hour to 10 hours.
8. A metalworking fluid, characterized in that, Includes the aluminum corrosion inhibitor as described in claim 1.
Citation Information
Patent Citations
Method for preparing isooctanol polyoxyethylene polyoxypropylene ether phosphate ester
CN101941987A
Alcohol ether phosphate and preparation method thereof and trace cutting fluid prepared by same
CN104710610A