A Kagome lattice material Pt2TlTe3 single crystal and its preparation method
The Kagome lattice material Pt₂TlTe₃ single crystal was prepared by melting method, which solved the problem of single crystal growth of polycrystalline materials and provided a stable single crystal material with typical metallic behavior, suitable for research on two-dimensional electronic devices.
Patent Information
- Application Number
- CN202311039562.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-17
AI Technical Summary
Most existing Pt₂TlTe₃ materials are polycrystalline, lacking the conditions for single-crystal growth, making it difficult to study their unique electronic properties and applications.
Kagome lattice material Pt₂TlTe₃ single crystals were prepared by a melting method. By controlling the temperature gradient in a high-temperature furnace and vacuum sealing the raw materials, the purity and impurity-free properties were ensured, resulting in high-quality single crystals.
Stable Pt₂TlTe₃ single crystals were obtained, exhibiting typical metallic behavior, suitable for research on two-dimensional electronic devices, and retaining intrinsic properties, which facilitates subsequent testing and applications.
Smart Images

Figure CN116856062B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a Kagome lattice material Pt2TlTe3 single crystal and its preparation method, belonging to the field of single crystal material technology. Background Technology
[0002] The Kagome lattice is a structure composed of vertically aligned triangles, originally proposed by Japanese physicist Kodi Husimi in 1951. In a Kagome lattice, each atom at a lattice point is connected to four adjacent lattice points, and each lattice point is the connection point of two vertically aligned equilateral triangles. Therefore, the entire lattice structure forms a hexagonal star structure, within which is a honeycomb-like six-membered ring.
[0003] In 2019, Pt₂HgSe₃ was predicted to be a large-bandgap quantum spin Hall insulator, and its quantum spin Hall state has been experimentally verified using scanning tunneling microscopy. The Se atoms in Pt₂HgSe₃ form a Kagome layer. Due to its unique structure, this lattice structure can induce many interesting properties. In this structure, electrons are bound within six-membered rings, forming a flat band with almost no energy dispersion. It is derived from a honeycomb structure, thus retaining the band structure characteristics of a honeycomb structure. Because of these two properties, materials with a Kagome structure have become important objects for experimental research on flat bands and Dirac bands. Many Kagome materials have been discovered theoretically and experimentally to date, such as Fe-Sn alloys, Mn₃X (X=Sn,Ge), and Co₃Sn₂S₂. Existing Pt₂TlTe₃ materials are all polycrystalline, and there are no reference conditions for growing single crystals. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide a Kagome lattice material Pt2TlTe3 single crystal and its preparation method.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows.
[0006] A Kagome lattice material Pt2TlTe3 single crystal, wherein the single crystal structure is: space group P-3m1, a=8.069 Å, b=8.069 Å, c=6.061 Å, α=90°, β=90°, γ=120°.
[0007] A method for preparing Kagome lattice material Pt2TlTe3 single crystal according to the present invention uses a melting method, and the method includes the following steps: (1) According to the stoichiometric ratio of the topological insulator single crystal, weigh the raw materials Pt, Tl and Te in a glove box filled with argon gas with water and oxygen content less than 0.1 ppm. Place the weighed raw materials in a quartz tube with a conical bottom and vacuum seal the quartz tube with an oxyhydrogen flame. The purity of the raw material is greater than or equal to 99.999%; The vacuum degree of the vacuum seal is 1×10⁻⁶. -4 Pa or above; (2) Place the vacuum-sealed quartz tube into a high-temperature furnace, first heat it to 1000~1100℃, keep it at a constant temperature for 6h~24h, then cool it down to 700~800℃, and finally let it cool naturally to room temperature and turn off the high-temperature furnace. (4) Open the quartz tube, take out the crystal and cut it with a wire cutter to obtain a single crystal.
[0008] Preferably, in step (1), the weighing error of each raw material is 0.01%.
[0009] Preferably, in step (1), the vacuum degree of the vacuum seal is 3×10⁻⁶. -4 Pa~5×10 -4 Pa.
[0010] Preferably, in step (2), the vacuum-sealed quartz tube is placed in a high-temperature furnace, heated to 1000-1100℃ for 9-11 hours, kept at a constant temperature for 6-24 hours, then cooled to 700-800℃ at a rate of 1-5℃ / h, and finally cooled naturally to room temperature before the high-temperature furnace is turned off.
[0011] Beneficial effects This invention provides a Kagome lattice material, Pt₂TlTe₃, single crystal, which exhibits typical metallic behavior and is a novel Kagome topological insulator material. This single crystal can be easily exfoliated to obtain a van der Waals material with multiple atomic layers, and this material is highly stable, which is crucial for future research on two-dimensional electronic devices.
[0012] This invention provides a method for preparing Kagome lattice material Pt2TlTe3 single crystals. The melting method avoids introducing impurities, allowing the obtained single crystals to possess intrinsic properties, facilitating subsequent testing and applications. Furthermore, hydrogen gas is used to remove the oxide layer formed on the surface of the raw materials before preparation, thereby improving the quality of the single crystal sample.
[0013] This invention achieves novel single-crystal growth by altering the temperature gradient, enabling elemental substitution across periods and main groups. By experimenting with various growth temperature gradients, this invention identified the optimal temperature for growing Pt₂TlTe₃ single crystals, thus solving the problem of growing from polycrystalline to single-crystal structures. Attached Figure Description
[0014] Figure 1 The image shows the X-ray diffraction (XRD) pattern of the single crystal described in Example 1.
[0015] Figure 2 The image shows the energy dispersive spectroscopy (EDS) spectrum of the single crystal described in Example 1.
[0016] Figure 3 The image shows the RT plot of the electrical properties of the single crystal described in Example 1.
[0017] Figure 4 The image shows the MR spectrum of the electrical properties of the single crystal described in Example 1.
[0018] Figure 5 The image shows a Hall diagram for testing the electrical properties of the single crystal described in Example 1. Detailed Implementation
[0019] The present invention will be further described in detail below with reference to specific embodiments.
[0020] Example 1 A novel Kagome lattice material, Pt₂TlTe₃, and its single-crystal preparation method are disclosed. The method employs a melt-melting process, and the steps are as follows: (1) Weigh 5g of Pt powder, 5g of Tl particles and 5g of Te particles, and put the above raw materials into quartz tubes respectively. Then, use hydrogen to wash the tubes in a vacuum sealing system. Finally, fill the quartz tubes with hydrogen at 0.8 atmospheres and seal the hydrogen inside the quartz tubes. Anneal the above raw materials at a temperature 50°C below their respective melting points to remove the oxide layer on the surface. After annealing, use a diamond cutter to cut a groove around the sealed quartz tube. In an argon-filled glove box (with water and oxygen content less than 0.1 ppm), break open the sealed quartz tube to obtain the raw material with the oxide layer removed, which is used for subsequent crystal preparation. (2) According to the stoichiometric ratio of the topological insulator single crystal, weigh 1.19761g of Pt, 0.62736g of Tl and 1.17502g of Te, the raw materials for removing the oxide layer on the surface in step (1), in a glove box filled with argon gas and with water and oxygen content less than 0.1 ppm, using an electronic balance. The weighing error of each raw material is 0.01%. Place the weighed raw materials in a quartz tube with a conical bottom, and ignite the quartz tube with an oxyhydrogen flame at a vacuum degree of 5×10⁻⁶. -4 The Pa sealing system is sealed; (3) Place the quartz tube that was vacuum sealed in step (2) into a high-temperature furnace, raise the temperature to 1000℃ after 10 hours, and keep it at 1000℃ for 24 hours. Then, lower the temperature to 700℃ at a rate of 2℃ / h, and finally let it cool down to room temperature naturally and turn off the high-temperature furnace. (4) Open the quartz tube, take out the crystal and cut it with a wire cutter to obtain a single crystal.
[0021] The prepared single crystal was characterized by XRD, and the results are as follows: Figure 1 As shown, a comparison with the standard card (ICSD number: 98-007-8787) reveals that all spectral peaks of the single crystal are close to the diffraction peaks of a Pt4Te6Tl2 single crystal, indicating that a Pt4Te6Tl2 single crystal sample has been prepared. The elemental content of the single crystal was analyzed using EDS spectroscopy, and the results are as follows... Figure 2 As shown, characteristic peaks of Pt, Tl and Te appear, and the composition ratio of each element is close to 2:1:3. At the same time, the EDS results between different selected regions are very similar, indicating that the crystal has good homogeneity.
[0022] The electrical properties of the single crystal prepared in Example 1 were tested. The resistivity of Example 1 from 2 K to 300 K as a function of temperature is shown in the figure below. Figure 3 As shown, the resistivity of the Pt₂TlTe₃ sample decreases with decreasing temperature, indicating typical metallic behavior, with a residual resistivity ratio of 2.46. The magnetoresistance versus magnetic field curves at the test temperature T=2K are shown below. Figure 4 As shown, the maximum positive magnetoresistance MR = 33%. The test temperature T = 2K, and the relationship between Hall resistivity and magnetic field is shown in the curve. Figure 5 As shown, the Hall resistance exhibits a deviated linear relationship, indicating that electrons and hole carriers coexist in the Pt2TlTe3 single crystal; however, since the overall slope of the curve is negative, it indicates that electrons dominate in the system.
[0023] Example 2 In this embodiment, in step (3), the quartz tube after vacuum sealing in step (2) is placed in a high-temperature furnace, heated to 1100°C for 10 hours, and kept at 1100°C for 12 hours. Then, it is cooled to 800°C at a rate of 5°C / h, and finally cooled to room temperature naturally and the high-temperature furnace is turned off. The rest is the same as in embodiment 1.
[0024] The single crystal structure and properties of Pt4Te6Tl2 obtained in this embodiment are similar to those in Example 1.
[0025] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.
Claims
1. A Kagome topological insulator material Pt2TlTe3 single crystal, wherein the single crystal structure is: space group P-3m1, a=8.069 Å, b=8.069 Å, c=6.061 Å, α=90°, β=90°, γ=120°; The single crystal is prepared by the following method, the steps of which include: (1) According to the stoichiometric ratio of the topological insulator single crystal, weigh the raw materials Pt, Tl and Te in a glove box filled with argon gas with water and oxygen content less than 0.1 ppm. Place the weighed raw materials in a quartz tube with a conical bottom and vacuum seal the quartz tube with an oxyhydrogen flame. The purity of the raw material is greater than or equal to 99.999%; The vacuum degree of the vacuum seal is 1×10⁻⁶. -4 Pa or above; In step (2), the vacuum-sealed quartz tube is placed in a high-temperature furnace and heated to 1000-1100℃ for 9-11 hours. The temperature is maintained for 6-24 hours, and then cooled to 700-800℃ at a rate of 1-5℃ / h. Finally, it is allowed to cool naturally to room temperature and the high-temperature furnace is turned off. (3) Open the quartz tube, take out the crystal and cut it with a wire cutter to obtain a single crystal.
2. A method for preparing a single crystal of Pt2TlTe3, a Kagome topological insulator material as described in claim 1, characterized in that: The method steps include: (1) According to the stoichiometric ratio of the topological insulator single crystal, weigh the raw materials Pt, Tl and Te in a glove box filled with argon gas with water and oxygen content less than 0.1 ppm. Place the weighed raw materials in a quartz tube with a conical bottom and vacuum seal the quartz tube with an oxyhydrogen flame. The purity of the raw material is greater than or equal to 99.999%; The vacuum degree of the vacuum seal is 1×10⁻⁶. -4 Pa or above; (2) Place the vacuum-sealed quartz tube into a high-temperature furnace, raise the temperature to 1000-1100℃ in 9-11 hours, keep the temperature constant for 6-24 hours, then lower the temperature to 700-800℃ at a rate of 1-5℃ / h, and finally let it cool naturally to room temperature and close the high-temperature furnace. (3) Open the quartz tube, take out the crystal and cut it with a wire cutter to obtain a single crystal.
3. The method for preparing a Kagome topological insulator material Pt2TlTe3 single crystal as described in claim 2, characterized in that: In step (1), the weighing error of each raw material is 0.01%.
4. The method for preparing a Kagome topological insulator material Pt2TlTe3 single crystal as described in claim 2, characterized in that: In step (1), the vacuum degree of the vacuum seal is 3×10⁻⁶. -4 Pa~5×10 -4 Pa.