Method for detecting zeta potential of hydrophobic titanium dioxide

By using slow-drying solvents and inorganic solvents to wet and dilute hydrophobic titanium dioxide, combined with a zeta potential detector, the problem of the inability to quickly test the potential value of hydrophobic titanium dioxide in the prior art is solved, and a rapid and convenient evaluation of dispersion performance is achieved.

CN116879352BActive Publication Date: 2026-11-24CHONGQING VANADIUM TITANIUM TECH CO LTD OF PANGANG GRP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310980772.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-04
Publication Date
2026-11-24
Estimated Expiration
2043-08-04

AI Technical Summary

Technical Problem

Existing technologies cannot quickly and conveniently test the zeta potential value of oleophilic titanium dioxide, making it difficult to evaluate its dispersion performance.

Method used

Hydrophobic titanium dioxide was wetted and diluted using slow-drying solvents such as ethanol, ethylene glycol, propanol, or propylene glycol, and an inorganic solvent such as water was used to prepare the solution, which was then tested using a zeta potential detector.

Benefits of technology

This provides a rapid and convenient method to characterize the dispersibility of hydrophobic titanium dioxide, reducing testing costs and improving the versatility of the detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116879352B_ABST
    Figure CN116879352B_ABST
Patent Text Reader

Abstract

This invention relates to a method for detecting the zeta potential of hydrophobic titanium dioxide, comprising: step a, fully wetting the hydrophobic titanium dioxide; step b, diluting the fully wetted hydrophobic titanium dioxide with an inorganic solvent; and step c, detecting the zeta potential of the diluted solution. The method described in this invention fills the gap in the ability to test the zeta potential value of hydrophobic titanium dioxide, providing another method for judging its dispersibility. Previously, the dispersibility of hydrophobic titanium dioxide could only be judged by testing the filtration pressure value in its carrier resin system (such as PP or PE systems). Testing the filtration pressure value is labor-intensive and resource-intensive, and the results are slow. Using the zeta potential value to represent the dispersibility of hydrophobic titanium dioxide is fast and convenient, providing strong support for new product development or factory testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium dioxide production, specifically relating to a method for detecting the zeta potential of hydrophobic titanium dioxide. Background Technology

[0002] Titanium dioxide (commonly known as titanium white or titanium dioxide powder) is currently the best white pigment in the world. It not only has very stable physical and chemical properties, but also has excellent optical and electrical properties such as high refractive index, best hiding power, best whiteness and brightness. It is widely used in coatings, plastics, papermaking, inks, electronics and other fields.

[0003] The current economic situation is severe for the coatings industry, and the use of titanium dioxide in coatings has decreased to some extent, while its use in the plastics industry has increased. Consumers' requirements for titanium dioxide have also increased accordingly. In order for plastic titanium dioxide to be fully integrated with polyolefins (primarily low-density polyethylene), polystyrene, ABS, polyvinyl chloride, etc., plastic titanium dioxide needs to have excellent oleophilic and hydrophobic properties. As a result, more and more plastic-specific hydrophobic titanium dioxide is being used in the plastics industry.

[0004] To quickly evaluate the dispersion performance of titanium dioxide powder, the zeta potential of the powder is usually tested. The dispersion system formed by solid particles dispersed in a liquid medium is generally neutral and has no inherent potential. However, due to ionization, ion adsorption, ion dissolution, lattice substitution, and triboelectric charging, the surface of the solid particles in the dispersion system often carries a positive or negative charge, while the surrounding liquid phase carries the opposite charge. Under the action of an applied electric field or force, relative motion occurs at the interface between the liquid-attached layer and the diffused layer of the liquid on the surface of the solid particles, generating an electrokinetic potential. This potential difference between the ion layer attached to the solid particles and the neutral phase is the zeta potential.

[0005] Because of its oleophilic nature, the potential value of titanium dioxide cannot be measured using conventional water-based methods, thus making it impossible to quickly characterize the dispersion performance of titanium dioxide through its potential value.

[0006] Therefore, existing technologies still need improvement. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this invention provides a method for testing the potential value of oleophilic titanium dioxide (i.e., hydrophobic titanium dioxide) in order to more quickly and conveniently characterize the dispersion performance of hydrophobic titanium dioxide.

[0008] Specifically, the present invention provides a method for detecting the zeta potential of hydrophobic titanium dioxide, comprising: step a, fully wetting the hydrophobic titanium dioxide; step b, diluting the fully wetted hydrophobic titanium dioxide with an inorganic solvent; and step c, detecting the zeta potential of the diluted solution.

[0009] In embodiments of the present invention, the inorganic solvent includes water.

[0010] In an embodiment of the present invention, in step a, the hydrophobic titanium dioxide is fully wetted by a slow-drying solvent, and the amount of the slow-drying solvent added is 2 to 4 times that of the titanium dioxide powder.

[0011] In embodiments of the present invention, the slow-drying solvent includes one or more of ethanol, ethylene glycol, propanol, and propylene glycol.

[0012] In an embodiment of the present invention, step a includes adding the slow-drying solution to 0.1-0.2g of hydrophobic titanium dioxide.

[0013] In an embodiment of the present invention, step b includes adding water to the fully wetted solution to prepare a solution of 0.8 g / L to 1.2 g / L.

[0014] In an embodiment of the present invention, the method for detecting the zeta potential of hydrophobic titanium dioxide further includes a step of ultrasonically dispersing the diluted solution for a predetermined time before step c.

[0015] In an embodiment of the present invention, the predetermined time is 10-15 minutes.

[0016] In an embodiment of the present invention, step c includes placing the diluted solution in a sample cell and placing the sample cell into a zeta potential detector for detection.

[0017] In an embodiment of the present invention, the sample cell includes an Ω electrode, and step c includes using a syringe to slowly inject the diluted solution into the Ω electrode until the liquid level is flush with the electrode metal sheet.

[0018] The beneficial effects of this invention are as follows: The method for detecting the zeta potential of hydrophobic titanium dioxide provided by this invention fills the gap in the inability to test the potential value of hydrophobic titanium dioxide, providing another method for judging the dispersibility of hydrophobic titanium dioxide. Previously, the dispersibility of hydrophobic titanium dioxide could only be judged by testing the filtration pressure value in its carrier resin system (such as PP, PE system). Testing the filtration pressure value is labor-intensive and resource-intensive, and the results are slow. However, using the zeta potential value to represent the dispersibility of hydrophobic titanium dioxide is fast, convenient, and highly versatile, providing strong support for new product development or factory testing. Attached Figure Description

[0019] Figure 1 The diagram shows a flowchart of a method for detecting the zeta potential of hydrophobic titanium dioxide provided by the present invention. Detailed Implementation

[0020] It should be understood that the embodiments of the invention shown in the exemplary embodiments are merely illustrative. Although only a few embodiments have been described in detail in this invention, those skilled in the art will readily recognize that various modifications are possible without substantially departing from the teachings of the invention. Accordingly, all such modifications should be included within the scope of the invention. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention.

[0021] According to the present invention, a method for detecting the zeta potential of hydrophobic titanium dioxide is provided, such as... Figure 1 As shown, it includes:

[0022] Step a: Thoroughly wet the hydrophobic titanium dioxide;

[0023] Step b: Dilute the fully wetted hydrophobic titanium dioxide with an inorganic solvent;

[0024] Step c: Perform zeta potential detection on the diluted solution.

[0025] In an embodiment of the present invention, in step a, the hydrophobic titanium dioxide can be fully wetted using a slow-drying solvent. A certain amount of hydrophobic titanium dioxide (preferably 0.1-0.2g) can be placed in a beaker, and a certain proportion of slow-drying solvent can be added. The mixture should be manually shaken for 1 minute and then allowed to stand for 2 minutes to fully wet the titanium dioxide. The slow-drying solvent can include one or more of ethanol, ethylene glycol, propanol, and propylene glycol, and the amount of slow-drying solvent added can be 2 to 4 times the amount of titanium dioxide powder. If the amount of powder is too small, less than 2 times the amount of slow-drying solvent, the powder cannot be well wetted by the slow-drying solvent, and some powder will still be hydrophobic after adding water, resulting in a larger test error.

[0026] In an embodiment of the present invention, in step b, the inorganic solvent may include water, preferably pure water. A certain proportion of pure water may be added to the beaker described in step a to dilute it to a solution of 0.8 g / L-1.2 g / L.

[0027] In an embodiment of the present invention, optionally, before step c, the method of the present invention may further include a step of ultrasonically dispersing the diluted solution for a predetermined time, wherein the predetermined time may be 10-15 min. The diluted solution from step b can be placed in an ultrasonic disperser and ultrasonically dispersed for 10-15 min.

[0028] In an embodiment of the present invention, step c includes placing the diluted solution in a sample cell and then placing the sample cell into a zeta potential detector for detection. The sample cell may include an Ω electrode, which may be a built-in Ω electrode in the zeta potential detector. Since the present invention allows for the dilution of hydrophobic titanium dioxide with an inorganic solvent, the diluted solution can be directly detected using the Ω electrode in the zeta potential detector without the need for custom-made electrodes, thereby improving testing versatility and reducing costs. Step c may include slowly injecting the diluted solution into the Ω electrode using a syringe until the liquid level is flush with the electrode metal sheet. Alternatively, the diluted solution or slurry from step b, or a diluted and ultrasonically dispersed solution or slurry, can be slowly injected into the Ω electrode using a syringe until the liquid level is flush with the electrode metal sheet. The Ω electrode is then placed in the zeta potential detector, and appropriate parameters are selected to detect the zeta potential value of the slurry.

[0029] The method described in this invention fills the gap in the inability to test the potential value of hydrophobic titanium dioxide, providing another method for judging the dispersibility of hydrophobic titanium dioxide. Previously, the dispersibility of hydrophobic titanium dioxide could only be judged by testing the filtration pressure value in its carrier resin system (such as PP and PE systems). Testing the filtration pressure value is labor-intensive and resource-intensive, and the results are slow. However, using the zeta potential value to represent the dispersibility of hydrophobic titanium dioxide is fast and convenient, providing strong support for new product development or factory testing.

[0030] The following specific embodiments further illustrate the concept of the present invention. It should be understood that the following embodiments are further illustrative of the present invention and are not intended to limit the scope of the present invention.

[0031] Example 1

[0032] The method for detecting the zeta potential of hydrophobic titanium dioxide according to the present invention includes the following steps:

[0033] 1. Take 0.1g of hydrophobic titanium dioxide No. 1 into a beaker, add 0.2g of propylene glycol, shake manually for 1 minute and let stand for 2 minutes;

[0034] 2. Add pure water to the above beaker to prepare a solution diluted to 1 g / L;

[0035] 3. Place the solution obtained in step 2 into an ultrasonic disperser and ultrasonically disperse for 10-15 minutes;

[0036] 4. Slowly inject the slurry obtained in step 3 into the Ω electrode using a syringe, ensuring that the liquid level is flush with the electrode metal sheet;

[0037] 5. Place the Ω electrode from step 4 into the zeta potential detector, select appropriate parameters, and detect the zeta potential value of the slurry.

[0038] Example 2

[0039] The method for detecting the zeta potential of hydrophobic titanium dioxide according to the present invention includes the following steps:

[0040] 1. Take 0.1g of hydrophobic titanium dioxide No. 2 into a beaker, add 0.2g of propylene glycol, shake manually for 1 minute and let stand for 2 minutes;

[0041] 2. Add pure water to the above beaker to prepare a solution diluted to 1 g / L;

[0042] 3. Place the solution obtained in step 2 into an ultrasonic disperser and ultrasonically disperse for 10-15 minutes;

[0043] 4. Slowly inject the slurry obtained in step 3 into the Ω electrode using a syringe, ensuring that the liquid level is flush with the electrode metal sheet;

[0044] 5. Place the Ω electrode from step 4 into the zeta potential detector, select appropriate parameters, and detect the zeta potential value of the slurry.

[0045] Example 3

[0046] The method for detecting the zeta potential of hydrophobic titanium dioxide according to the present invention includes the following steps:

[0047] 1. Take 0.1g of hydrophobic titanium dioxide 3# into a beaker, add 0.2g of propylene glycol, shake manually for 1 minute and let stand for 2 minutes;

[0048] 2. Add pure water to the above beaker to prepare a solution diluted to 1 g / L;

[0049] 3. Place the solution obtained in step 2 into an ultrasonic disperser and ultrasonically disperse for 10-15 minutes;

[0050] 4. Slowly inject the slurry obtained in step 3 into the Ω electrode using a syringe, ensuring that the liquid level is flush with the electrode metal sheet;

[0051] 5. Place the Ω electrode from step 4 into the zeta potential detector, select appropriate parameters, and detect the zeta potential value of the slurry.

[0052] Example 4

[0053] The method for detecting the zeta potential of hydrophobic titanium dioxide according to the present invention includes the following steps:

[0054] 1. Take 0.2g of hydrophobic titanium dioxide #4 into a beaker, add 0.8g of ethanol, shake manually for 1.5min and let stand for 2min;

[0055] 2. Add pure water to the above beaker to prepare a solution diluted to 1 g / L;

[0056] 3. Place the solution obtained in step 2 into an ultrasonic disperser and ultrasonically disperse for 10-15 minutes;

[0057] 4. Slowly inject the slurry obtained in step 3 into the Ω electrode using a syringe, ensuring that the liquid level is flush with the electrode metal sheet;

[0058] 5. Place the Ω electrode from step 4 into the zeta potential detector, select appropriate parameters, and detect the zeta potential value of the slurry.

[0059] Example 5

[0060] The method for detecting the zeta potential of hydrophobic titanium dioxide according to the present invention includes the following steps:

[0061] 1. Take 0.15g of hydrophobic titanium dioxide No. 5 into a beaker, add 0.45g of ethylene glycol, shake manually for 1 minute and let stand for 2 minutes;

[0062] 2. Add pure water to the above beaker to prepare a solution diluted to 1 g / L;

[0063] 3. Place the solution obtained in step 2 into an ultrasonic disperser and ultrasonically disperse for 10-15 minutes;

[0064] 4. Slowly inject the slurry obtained in step 3 into the Ω electrode using a syringe, ensuring that the liquid level is flush with the electrode metal sheet;

[0065] 5. Place the Ω electrode from step 4 into the zeta potential detector, select appropriate parameters, and detect the zeta potential value of the slurry.

[0066] Comparative Example

[0067] Hydrophobic titanium dioxide products #1, #2, #3, #4, and #5 were tested for their filtration pressure values ​​in a PP resin system according to national standards.

[0068] Table 1 Comparison of Examples and Comparative Data

[0069]

[0070] A larger absolute value of the potential indicates better powder dispersion performance; a smaller filtration pressure value indicates better powder dispersibility. The results from both potential and filtration pressure values ​​show that this method of characterizing powder dispersion performance is consistent with the results obtained using filtration pressure values.

[0071] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. Any modifications or equivalent substitutions made to the present invention without departing from the spirit and scope thereof should be covered within the protection scope of the claims of the present invention.

Claims

1. A method for detecting the zeta potential of hydrophobic titanium dioxide, characterized in that, include: Step a: Take 0.1-0.2g of hydrophobic titanium dioxide, add 2-4 times the amount of slow-drying solvent to the titanium dioxide powder, shake by hand and let stand to fully wet the hydrophobic titanium dioxide; Step b: Add water to the fully moistened solution to prepare a solution with a concentration of 0.8 g / L to 1.2 g / L; Step c: Sonicate the diluted solution for a predetermined time, then slowly inject the dispersed solution into the Ω electrode of the zeta potential detector using a syringe, ensuring the liquid level is flush with the electrode metal plate, and then perform zeta potential detection.

2. The method for detecting the zeta potential of hydrophobic titanium dioxide according to claim 1, characterized in that, The slow-drying solvent includes one or more of ethanol, ethylene glycol, propanol, and propylene glycol.

3. The method for detecting the zeta potential of hydrophobic titanium dioxide according to claim 1, characterized in that, The predetermined time is 10-15 minutes.

Citation Information

Patent Citations

  • Method for detecting dispersion state of titanium dioxide

    CN110988037A

  • Method for detecting potential of titanium dioxide in organic system

    CN111474210A

  • Method for detecting pH value of hydrophobic titanium dioxide

    CN115453059A