Preparation method and use of a three-dimensional super-lithiophilic composite lithium metal negative electrode

By forming a biofilm on the surface of carbon materials and preparing a three-dimensional superlithophile framework through high-temperature calcination, the problem of lithium dendrite growth is solved, the safety and stability of lithium anodes are improved, and it is suitable for high-energy-density energy storage devices for lithium-ion batteries.

CN116885113BActive Publication Date: 2026-11-20XUZHOU NORMAL UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311045025.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-18
Publication Date
2026-11-20
Estimated Expiration
2043-08-18

AI Technical Summary

Technical Problem

When existing lithium-ion batteries use metallic lithium anodes, the growth of lithium dendrites and side reactions lead to low coulombic efficiency and short lifespan, making it difficult to meet the needs of high-energy-density energy storage devices.

Method used

A biofilm was formed on the surface of a carbon material using a bacterial solution, and a three-dimensional superlithiophilic framework was prepared by high-temperature calcination. The porous carbon material modified with heterocarbon elements in the biofilm was used to construct a conductive framework with a strong electric field, which induced uniform lithium-ion deposition and inhibited dendrite growth.

Benefits of technology

This method achieves uniform lithium-ion deposition, improves the safety and cycle stability of lithium anodes, and is a green and environmentally friendly approach suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116885113B_ABST
    Figure CN116885113B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a three-dimensional super-lithiophilic composite lithium metal negative electrode, and comprises the following steps: uniformly mixing a biological bacteria solution and a base carbon material, and culturing the mixture in a shaking incubator at room temperature for a period of time, so that a layer of biological biofilm is formed on the surface of the carbon material; centrifuging and freeze-drying to obtain a base carbon material-biofilm composite material; high-temperature calcining the base carbon material-biofilm composite material in an inert atmosphere to obtain a three-dimensional super-lithiophilic skeleton; and preparing the three-dimensional super-lithiophilic composite lithium metal negative electrode through a lithium intercalation method. The method is simple in steps, high in efficiency, green in environmental protection, free of pollution, and capable of realizing large-scale production, and the prepared three-dimensional super-lithiophilic composite lithium metal negative electrode can be applied to the field of energy storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion batteries, specifically to a method for preparing a three-dimensional superlithiophilic composite lithium metal anode and its applications. Background Technology

[0002] In recent years, with the rise of green and low-carbon concepts, the trend towards electrification has intensified. The demand for high-capacity rechargeable batteries is also constantly increasing. The energy density of current lithium-ion battery systems is nearing its limit, making it difficult to meet the high-energy-density energy storage requirements of various electronic devices and electric vehicles. Therefore, there is an urgent need to develop a new battery system to solve this problem.

[0003] Compared to traditional graphite or silicon-carbon anodes, the use of lithium metal anodes is key to achieving the high specific energy advantage of lithium-ion batteries. However, the unlimited volume expansion of lithium metal and the uncontrollable growth of lithium dendrites during charge and discharge severely restrict their application. The most prominent issue is the lithium dendrite problem caused by uneven lithium ion deposition on the anode during charge and discharge. The growth of lithium dendrites and the exacerbation of side reactions lead to the failure of lithium metal anodes during operation, seriously affecting the coulombic efficiency and lifespan of the battery. Therefore, designing a superlithophile composite lithium anode that induces homogeneous lithium ion deposition during charge and discharge, avoids lithium dendrite formation, and thus improves the safety of lithium anodes is a critical technical challenge that urgently needs to be solved. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing a three-dimensional superlithiophilic composite lithium anode and its application. This method is simple, efficient, green and environmentally friendly, pollution-free, and can be mass-produced. The prepared three-dimensional superlithiophilic composite lithium anode can be applied in the field of energy storage.

[0005] To achieve the above objectives, the technical solution adopted by this invention is: a method for preparing a three-dimensional superlithiophilic composite lithium metal anode, comprising the following steps:

[0006] (1) Preparation of substrate carbon materials@biofilm

[0007] A carbon substrate material was dispersed in a bacterial solution and incubated at room temperature in a shaking incubator for a period of time, resulting in the formation of a biofilm on the surface of the carbon material. Centrifugation and freeze-drying yielded the composite material of the carbon substrate material@biofilm.

[0008] (2) Preparation of three-dimensional superlithophile framework

[0009] A three-dimensional superlithiophilic framework was prepared by high-temperature calcination of a composite material of substrate carbon material@biofilm under an inert atmosphere;

[0010] (3) A three-dimensional superlithiophilic composite lithium metal anode was prepared by lithium intercalation.

[0011] Preferably, the biological bacterial solution is one or a mixture of Klebsiella pneumoniae solution, Bacillus subtilis solution, Clostridium klebsiella pneumoniae solution, Listeria monocytogenes solution, Ralstonia solanacearum solution, Candida albicans solution, Aspergillus niger solution, Vibrio desulfurization solution, Yersinia algae solution, Serratia marcescens solution, Staphylococcus aureus solution, Nocardia ciliata solution, and Klebsiella pneumoniae solution.

[0012] Preferably, the substrate carbon material is one or a mixture of multiple of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, MXene, carbon felt, carbon cloth, and conductive carbon black.

[0013] Furthermore, in step (2), when the substrate carbon material contains single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, Mxene or conductive carbon black, the composite material of substrate carbon material@biofilm is dispersed in an aqueous solution, filtered to form a film, dried, and then calcined at high temperature under an inert atmosphere to prepare a three-dimensional superlithophile framework.

[0014] Preferably, in step (1), the incubation time in the shaking incubator is 10-24 hours.

[0015] Preferably, in step (2), the calcination temperature is 200-1000℃ and the calcination time is 5-24h.

[0016] Preferably, in step (3), the lithium intercalation method is lithium deposition or molten lithium wetting.

[0017] The present invention also provides the application of the three-dimensional superlithiophilic composite lithium anode prepared by the above method in the field of energy storage.

[0018] This invention disperses a substrate carbon material in a bacterial solution. The bacteria spontaneously adhere to the carbon material surface during their metabolic activities, forming a biofilm. The resulting composite material is then filtered, calcined at high temperature, to obtain a heteroatom-modified three-dimensional superlithiophilic framework. The polysaccharides, peptides, and proteins secreted by the microorganisms can differentiate the types and contents of different carbon elements (oxygen, nitrogen, phosphorus, and sulfur), giving the porous carbon derived from the biofilm higher lithiophilicity. This not only significantly reduces the surface energy and viscosity of molten lithium, further improving its wettability, but more importantly, the three-dimensional conductive framework constructed by the biocarbon membrane combined with the substrate carbon material possesses a strong electric field strength. This effectively disperses the local current density on the electrode surface, inducing homogeneous lithium-ion deposition and thus inhibiting dendrite growth.

[0019] Compared with existing technical solutions, the present invention has the following advantages:

[0020] (1) The biological bacteria used in this invention are green and environmentally friendly, and are easy and convenient to obtain at low cost.

[0021] (2) The three-dimensional superlithophile framework prepared in this invention has a simple operation method and a concise process, and can be mass-produced.

[0022] (3) This invention utilizes the biofilm formed by the life metabolism of microorganisms, and modifies the lithiophilicity of the framework by the abundant heterocarbon elements in the biofilm, so that the preparation of three-dimensional superlithiophilic composite lithium metal anode has a wide application prospect in the field of energy storage. Attached Figure Description

[0023] Figure 1 Here is a SEM image of the surface of the three-dimensional superlithophile framework obtained in Example 1;

[0024] Figure 2 A photograph of the three-dimensional superlithiophilic composite lithium metal anode obtained in Example 1;

[0025] Figure 3 Cycle curves of lithium-to-lithium full cells assembled from the lithium metal anode obtained in Comparative Example 1 and the three-dimensional superlithiophilic composite lithium metal anode obtained in Example 1.

[0026] Figure 4 Here is a SEM image of the surface of the three-dimensional superlithophile framework obtained in Example 2;

[0027] Figure 5 A photograph of the three-dimensional superlithiophilic framework membrane obtained in Example 2;

[0028] Figure 6 Cycle curves of lithium-to-lithium full cells assembled from the lithium metal anode obtained in Comparative Example 2 and the three-dimensional superlithiophilic composite lithium metal anode obtained in Example 2. Detailed Implementation

[0029] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0030] Comparative Example 1

[0031] Weigh 20 mg of MXene, disperse it in 15 ml of water, filter it to form a film, dry it, and then calcine it to obtain blank control sample I.

[0032] Example 1

[0033] A method for preparing a three-dimensional superlithiophilic composite lithium metal anode includes the following steps:

[0034] (1) Preparation of MXene@biofilm

[0035] 10 ml of 25 mg / ml lysate solution was dispersed in a centrifuge tube, 1 ml of Klebsiella pneumoniae was added, 50 mg of MXene was weighed and added to the solution, and the mixture was mixed well. The resulting bacterial solution was transferred to a shaking incubator and cultured for 10 h at 30 °C. The bacteria formed a biofilm on the surface of the carbon material. The composite material of MXene@biofilm was obtained by centrifugation and freeze drying.

[0036] (2) Preparation of three-dimensional superlithophile framework

[0037] 20 mg of MXene@biofilm composite material was weighed and dispersed in 15 ml of water, filtered to form a film, dried, and then calcined at 500 °C for 6 h in an inert atmosphere to prepare a three-dimensional superlithophile framework.

[0038] (3) Cut the three-dimensional superlithiophilic framework prepared in step (2) into electrode discs with a diameter of 8 mm, and deposit lithium at a current of 20 mA for 4 h to obtain a three-dimensional superlithiophilic composite lithium metal anode.

[0039] See appendix Figure 1 The image shows a three-dimensional superlithiophilic framework surface SEM image obtained in step (2) of this embodiment. As shown in the figure, microorganisms are widely distributed on the membrane surface, indicating that the bacteria have been successfully deposited on the carbon membrane surface.

[0040] See appendix Figure 2 The image shown is a three-dimensional superlithiophilic framework lithium deposition image obtained in this example. As shown in the figure, it is clear that metallic lithium has been deposited on the film surface.

[0041] The blank control sample I obtained from Comparative Example 1 was cut into electrode discs with a diameter of 8 mm, and lithium deposition was performed at a current of 20 mA for 4 hours to obtain the lithium metal anode I of the control group. See Appendix Figure 3 The three-dimensional superlithiophilic composite lithium metal anode obtained in this embodiment and the comparative lithium metal anode I were respectively assembled into lithium-to-lithium full cells. At 0.5 mA / cm²... 2 Electrochemical performance tests of lithium-ion insertion and extraction were conducted at current densities, such as... Figure 3 As shown, the battery assembled in Comparative Example 1 has a much lower cycle performance than the battery assembled in Example 1, indicating that the three-dimensional superlithiophilic skeleton with fungal attachment exhibits better cycle stability.

[0042] Comparative Example 2

[0043] The carbon felt was cut into electrode discs with a diameter of 8 mm, which were used as blank control sample II.

[0044] Example 2

[0045] A method for preparing a three-dimensional superlithiophilic composite lithium metal anode includes the following steps:

[0046] (1) Preparation of carbon felt@biofilm

[0047] 20 ml of 30 mg / ml lysate solution was dispersed in a centrifuge tube, 2 ml of Bacillus subtilis solution was added, 40 mg of carbon felt was weighed and added to the above solution, and mixed evenly. The resulting bacterial solution was transferred to a shaking incubator and cultured for 15 h at a temperature of 35 °C. The bacteria formed a biofilm on the surface of the carbon material. The carbon felt@biofilm composite material was obtained by centrifugation and freeze drying.

[0048] (2) Preparation of three-dimensional superlithophile framework

[0049] A three-dimensional superlithophile framework was prepared by calcining the dried carbon felt@biofilm composite material at 500℃ for 8 hours in an inert atmosphere.

[0050] (3) The metallic lithium is heated at 300°C in an inert environment to obtain molten liquid lithium. The molten lithium is then drawn into the three-dimensional superlithophile framework by siphoning and cooled to obtain a three-dimensional superlithophile metal anode.

[0051] See appendix Figure 4 The image shows a three-dimensional superlithiophilic skeleton surface SEM image obtained in step (2) of this embodiment. As shown in the figure, a large number of fungi are attached to the columnar substrate material, indicating that the bacteria have been successfully deposited on the carbon felt surface.

[0052] Participate in the attached Figure 5 The image shows a photograph of the three-dimensional superlithiophilic skeleton membrane obtained in Example 2. As shown in the figure, the carbon fiber structure of the carbon felt is clearly visible in the photograph after high-temperature calcination.

[0053] Lithium metal was heated to 300°C in an inert environment to obtain molten liquid lithium. This molten lithium was then drawn into the blank control sample II obtained in Comparative Example 2 via siphoning. After cooling, the lithium metal anode II of the control group was obtained. (See appendix) Figure 6 The three-dimensional superlithiophilic composite lithium metal anode obtained in this embodiment and the comparative lithium metal anode II were respectively assembled into lithium-to-lithium full cells. At 1 mA / cm²... 2 Electrochemical tests of lithium-ion insertion and extraction were performed at current densities, such as... Figure 6 As shown, the battery assembled in Comparative Example 2 has a much lower cycle performance than the battery assembled in Example 2, indicating that the three-dimensional superlithiophilic skeleton with fungal attachment exhibits better cycle stability.

Claims

1. A method for preparing a three-dimensional superlithiophilic composite lithium metal anode, characterized in that, Includes the following steps: (1) Preparation of substrate carbon material@biofilm The substrate carbon material is dispersed in a biological bacterial solution and cultured in a shaking incubator at room temperature for a period of time. The biological bacteria form a biofilm on the surface of the carbon material. The composite material of substrate carbon material@biofilm is obtained by centrifugation and freeze-drying. The biological bacterial solution is one or a mixture of Klebsiella pneumoniae, Bacillus subtilis, Clostridium klebsiella pneumoniae, Listeria monocytogenes, Ralstonia solanacearum, Candida albicans, Aspergillus niger, Vibrio desulfurans, Yersinia spp., Serratia marcescens, Staphylococcus aureus, and Nocardia citrate. (2) Preparation of three-dimensional superlithophile framework When the substrate carbon material is carbon felt or carbon cloth, a three-dimensional superlithiophilic framework is prepared by high-temperature calcination of the substrate carbon material@biofilm under an inert atmosphere; when the substrate carbon material contains single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, Mxene or conductive carbon black, the substrate carbon material@biofilm composite material is dispersed in an aqueous solution, filtered to form a film, dried, and then calcined at high temperature under an inert atmosphere to prepare a three-dimensional superlithiophilic framework. (3) The three-dimensional superlithiophilic framework obtained in step (2) is used to prepare a three-dimensional superlithiophilic composite lithium metal anode by lithium intercalation.

2. The method for preparing a three-dimensional superlithiophilic composite lithium metal anode according to claim 1, characterized in that, In step (1), the incubation time in the shaking incubator is 10-24 hours.

3. The method for preparing a three-dimensional superlithiophilic composite lithium metal anode according to claim 1, characterized in that, In step (2), the calcination temperature is 200-1000 ℃ and the calcination time is 5-24h.

4. The method for preparing a three-dimensional superlithiophilic composite lithium metal anode according to claim 1, characterized in that, In step (3), the lithium insertion method is lithium deposition or molten lithium wetting.

5. The use of the three-dimensional superlithiophilic composite lithium metal anode prepared by the method of any one of claims 1-4 in the field of energy storage.

Citation Information

Patent Citations

  • Composite lithium metal negative electrode containing buffer interface, and preparation method thereof

    CN113594422A

  • Method for preparing carbon skeleton from wood hypha symbiotic material and sulfur-loaded energy storage application

    CN114388786A