Rechargeable high-performance chlorine-based battery based on lithium-silicon alloy negative electrode, electrolyte therefor, and method of preparation

By using a lithium-silicon alloy anode and a specific electrolyte ratio, the safety and cost issues of chlorine-based batteries have been resolved, and high-performance chlorine-based batteries have achieved excellent electrochemical performance under low-temperature conditions.

CN116885262BActive Publication Date: 2026-11-20SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310867838.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-16
Publication Date
2026-11-20
Estimated Expiration
2043-07-16

AI Technical Summary

Technical Problem

Existing chlorine-based batteries have safety and cost issues in terms of anode chemistry, especially the high cost and safety hazards caused by the use of lithium metal anodes, and the parasitic reaction between lithium and chlorine-based electrolytes leads to performance degradation.

Method used

A rechargeable high-performance chlorine-based battery based on a lithium silicon alloy anode was prepared by using an electrolyte solution composed of a lithium thionyl chloride electrolyte solution and 1,2-dichloroethane in a specific ratio, through electrolyte dilution and anode passivation.

Benefits of technology

It maintains excellent electrochemical performance under low-temperature conditions, significantly reduces material costs, and improves the safety and practicality of chlorine-based batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116885262B_ABST
    Figure CN116885262B_ABST
Patent Text Reader

Abstract

The application discloses a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy negative electrode, an electrolyte and a preparation method thereof. The chlorine-based battery adopts a conventional carbon-based positive electrode material, and a lithium-silicon alloy material coated by a polymer is used as the negative electrode. The electrolyte mainly comprises the following components in percentage by volume: a lithium sulfinyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%. The lithium sulfinyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and sulfinyl chloride. The technical scheme provided by the application realizes and prepares a rechargeable high-performance chlorine-based battery based on reversible oxidation and reduction of silicon through electrolyte dilution and negative electrode passivation. Compared with traditional chlorine-based batteries, the chlorine-based battery provided by the application has superior performance, especially under low-temperature (-60 DEG C) conditions, and the material cost of the chlorine-based battery is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chlorine-based battery and electrolyte technology, specifically relating to a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy negative electrode, its electrolyte, and preparation method. Background Technology

[0002] For half a century, chlorine (Cl)-based batteries, composed of chlorine-based active materials and electrolytes, have been actively explored. They exhibit various advantages, including low cost, high sustainability, and high safety, making them promising candidates for high-performance energy storage technologies.

[0003] For example, the lithium thionyl chloride (Li / SOCl2) primary battery, invented in the 1970s, can provide approximately 590 Wh / kg. -1 The ultra-high energy density. More importantly, the emerging rechargeable Li / Cl2 battery, based on reversible LiCl / Cl2 redox and SOCl2-based electrolytes, exhibits impressive electrochemical performance, opening up a new avenue for Cl-based batteries.

[0004] Despite the excellent performance achieved by chlorine-based batteries in the past, practical chlorine-based batteries have always suffered from serious limitations in anode chemistry. For example, the use of lithium metal anodes easily leads to widespread problems in the safety of use, cost, and production safety of chlorine-based batteries, which is now widely acknowledged in the battery industry (F. Shen, S. Wang, Y. Gao, Joule 2021, 5, 2766-2767.). More importantly, the currently accepted severe parasitic reaction between lithium metal and chlorine-based electrolytes necessitates the use of large amounts of excess lithium metal (e.g., for rechargeable Li / Cl2 batteries, the actual amount of lithium metal added exceeds 30 times its theoretical charge-discharge requirement) (T. Liu, H. Li, J. Yue, J. Feng, M. Mao, X. Zhu, Y.-s. Hu, H. Li, X. Huang, L. Chen, L. Suo, Angew. Chem. Int. Ed. 2021, 60, 17547-17555.) (G. Zhu, P. Liang, C.-L. Hua (ng, C.-C. Huang, Y.-Y. Li, S.-C. Wu, J. Li, F. Wang, X. Tian, ​​W.-H. Huang, S.-K. Jiang, W.-H. Hung, H. Chen, M.-C. Lin, B.-J. Hwang, H. Dai, J. Am. Chem. Soc. 2022, 144, 22505-22513.), which inevitably reduces the actual electrochemical and safety performance of chlorine-based batteries and brings high production and usage costs, significantly limiting the development and market position of chlorine-based batteries (MAZabara, H.). A. Karabatak, B. Ulgut, J. Electrochem. Soc. 2021, 168, 050529.) (GH Boyle, F. Goebel, Journal of Power Sources 1995, 54, 186-191.).

[0005] Therefore, if a new type of negative electrode other than lithium metal can be invented and its usage reduced, the cost-effectiveness, safety and practicality of chlorine-based batteries will be significantly improved. Summary of the Invention

[0006] In view of the shortcomings of the prior art described above, the present invention provides a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode, its electrolyte, and its preparation method. The technical solution provided by the present invention, through electrolyte dilution and anode passivation, achieves and prepares for the first time a rechargeable, high-performance chlorine-based battery based on silicon reversible redox. Compared with traditional chlorine-based batteries, the chlorine-based battery provided by the present invention has superior performance, especially in maintaining excellent electrochemical performance under low temperature (-60℃) conditions, and significantly reduces the material cost of chlorine-based batteries.

[0007] To achieve the above objectives, the present invention first provides an electrolyte for chlorine-based batteries and a method for preparing the same, which is achieved by adopting a technical solution consisting of the following technical measures.

[0008] An electrolyte for chlorine-based batteries, comprising, by volume percentage, the following components:

[0009] Lithium thionyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%;

[0010] The lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride.

[0011] In this document, the lithium thionyl chloride electrolyte solution is a lithium thionyl chloride electrolyte solution known in the art, namely, a lithium electrolyte solution composed of aluminum chloride and lithium salt mixed and dissolved in thionyl chloride (SOCl2); wherein the lithium salt used is a type of lithium salt conventionally selected in the electrolyte of lithium batteries / chlorine-based batteries in the prior art, such as at least one of lithium chloride (LiCl), lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(oxalate-borate) (LiBOB), lithium di(oxalate-borate) (LiDFOB), lithium trifluoromethanesulfonate (CF3SO3Li), lithium bis(trifluoromethanesulfonylimide) (LiTFSI), and lithium bis(fluorosulfonylimide) (LiFSI).

[0012] In this document, the lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride. Generally speaking, the ratio between the above components can be in accordance with the conventional ratio of lithium thionyl chloride electrolyte solutions in the art, or the conventional ratio of electrolyte solutions applicable to lithium batteries / chlorine-based batteries as described in the prior art.

[0013] In one technical solution, experiments have confirmed that the ratio of aluminum chloride, lithium salt, and thionyl chloride in the lithium thionyl chloride electrolyte solution has almost negligible impact on the characterization of the various functions of the final prepared chlorine-based battery, especially the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode described below. Therefore, using thionyl chloride as the solvent, the concentration of aluminum chloride can be arbitrarily selected within the range of 1–12 mol / L, and the concentration of lithium salt should not exceed the concentration of aluminum chloride and be ≥1 mol / L. However, comparative experiments have found that the ratio of aluminum chloride, lithium salt, and thionyl chloride significantly affects the various electrochemical performances of the final prepared chlorine-based battery, especially the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode described below. Therefore, using thionyl chloride as the solvent, the concentration of aluminum chloride is preferably arbitrarily selected within the range of 2–6 mol / L, and the concentration of lithium salt should not exceed the concentration of aluminum chloride and be ≥2 mol / L.

[0014] To better illustrate the present invention and provide a preferred technical solution for reference, the lithium thionyl chloride electrolyte solution is prepared by dissolving lithium chloride (LiCl) and aluminum chloride (AlCl3) in thionyl chloride (SOCl2). Under laboratory conditions, a specific preparation method can be as follows: add 8 mmol of AlCl3 and 8 mmol of LiCl to 2 ml of SOCl2 and stir for 8 hours. The resulting product is referred to as ALS electrolyte solution. It should be noted that the specific preparation method of the lithium thionyl chloride electrolyte solution described above is only for illustrating this application and should not be considered as limiting the scope of this application. This preparation method is a conventional preparation method in the technical field of this invention, and other preparation methods of lithium thionyl chloride electrolyte solutions based on existing technologies can also be applied to this invention.

[0015] In one technical solution, when the lithium thionyl chloride electrolyte solution is prepared by adding lithium chloride (LiCl) and aluminum chloride (AlCl3) to thionyl chloride (SOCl2) and dissolving them together, lithium tetrachloroaluminate (LiAlCl4) can also be added directly as an alternative.

[0016] The electrolyte for chlorine-based batteries in the above technical solution mainly consists of lithium thionyl chloride electrolyte solution and 1,2-dichloroethane. It should be noted that other conventional electrolyte additives / auxiliaries, especially functional additives, can also be added. Those skilled in the art can choose to add them according to the required functional needs. It is important to emphasize that the electrolyte for chlorine-based batteries in this invention may or may not contain other conventional electrolyte additives / auxiliaries.

[0017] In one of the technical solutions, the electrolyte for the chlorine-based battery is prepared by mixing a lithium thionyl chloride electrolyte solution with 1,2-dichloroethane.

[0018] In one preferred embodiment, in order to further improve the electrochemical performance of the chlorine-based battery and further reduce the production cost, the volume percentage of the 1,2-dichloroethane is 60-90%.

[0019] In one more preferred embodiment, in order to further improve the electrochemical performance of the chlorine-based battery and further reduce the production cost, the volume percentage of the 1,2-dichloroethane is 89-90%.

[0020] Secondly, based on the electrolyte for chlorine-based batteries provided above, this invention provides a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy negative electrode and its preparation method, which is achieved by adopting a technical solution consisting of the following technical measures.

[0021] A rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode, wherein the cathode uses a conventional carbon-based cathode material and the anode uses a polymer-coated lithium-silicon alloy material.

[0022] Its electrolyte, by volume percentage, mainly comprises the following components:

[0023] Lithium thionyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%;

[0024] The lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride;

[0025] The polymer-coated lithium-silicon alloy material, wherein the polymer is selected from any one of polyacrylonitrile, dopamine, polyvinylpyrrolidone, glucose, sucrose, and tannic acid; the lithium-silicon alloy is Li 15 Si4.

[0026] In this document, the cathode material used is a conventional carbon-based cathode material, which is the cathode material commonly used in lithium batteries / chlorine-based batteries. Those skilled in the art can select a suitable carbon-based cathode material based on existing technology or existing lithium battery / chlorine-based battery production processes.

[0027] In one technical solution, the cathode material is selected from at least one of Ketjen black, acetylene black, graphite, graphene, and carbon nanotubes.

[0028] To better illustrate the present invention and provide a preferred technical solution for reference, the positive electrode is prepared using polytetrafluoroethylene (PTFE) / Ketjen black material according to conventional lithium battery / chlorine-based battery processes. Under laboratory conditions, the specific preparation method can be as follows: Ketjen black (KJ) and PTFE are mixed at a mass ratio of 9:1, and then dispersed in ethanol via ultrasonic treatment to form a positive electrode slurry; the resulting positive electrode slurry is immersed in a nickel foam sheet with a diameter of 14 mm for positive electrodes and dried at 100°C to remove the ethanol; except for the addition of other third components, the Ketjen black (KJ) loading of the positive electrode is 1.28–1.32 mg / cm³. -2 .

[0029] In this document, the polymer-coated lithium-silicon alloy material includes any one of polyacrylonitrile, dopamine, polyvinylpyrrolidone, glucose, sucrose, and tannic acid. It should be noted that the polymer used should be able to coat the lithium-silicon alloy particles and possess a certain degree of conductivity. Due to the limited time available for conducting experiments related to this invention, the conductivity requirements of such polymers have not yet been systematically summarized. However, those skilled in the art can select polymers with similar or even better conductivity based on the polymer selections listed in this invention, achieving the same effect / function / purpose as the polymers listed in this invention. Furthermore, it should be additionally noted that polyacrylonitrile requires cyclization treatment before coating. The specific process for this cyclization treatment can refer to conventional cyclization treatment methods described in the prior art.

[0030] To better illustrate the present invention and provide a preferred technical solution for reference, when the polymer is polyacrylonitrile (PAN), it is prepared by coating silicon powder with polyacrylonitrile and then cyclizing it to obtain cyclized polyacrylonitrile-coated silicon (Si-PAN). The obtained Si-PAN is then pre-lithiated to prepare a lithium-silicon alloy material coated with cyclized polyacrylonitrile. Under laboratory conditions, the specific preparation method of the negative electrode can be as follows: 60 mg PAN and 140 mg silicon powder are mixed and stirred in 1.48 mL of N,N-dimethylformamide (DMF) for at least 12 h to obtain a negative electrode slurry; the obtained negative electrode slurry is dried at 80 °C for 3 h, and then annealed in an argon atmosphere at 300 °C for 12 h to obtain Si-PAN; the obtained Si-PAN is punched into a circular electrode sheet with a diameter of 12 mm; then, using a conventional lithium battery electrolyte, the circular electrode sheet and lithium metal are used to form a Li / Si-PAN half-cell for pre-lithiation treatment: the Li / Si-PAN half-cell is pre-lithiated at 150 mAg. -1The current density is discharged to 0.01V, and after washing with dimethyl carbonate (DMC) to remove residual electrolyte, the electrode is immediately disassembled to obtain a pre-lithiated circular negative electrode, referred to as LSC alloy negative electrode. The conventional lithium battery electrolyte used in the pre-lithiating treatment can be a commercially available lithium battery electrolyte, or a lithium battery electrolyte described in existing technology, such as 1M lithium hexafluorophosphate (LiPF6) commercial electrolyte (volume ratio EC:DMC:EMC = 1:1:1, LiPF6 concentration 1 mol / L) and 1M lithium bisfluorosulfonylimide (LiFSI) electrolyte (volume ratio EC:DMC = 1:1, LiFSI concentration 1 mol / L).

[0031] In this document, based on common knowledge of chlorine-based batteries in the prior art, the rechargeable high-performance chlorine-based battery based on the lithium-silicon alloy anode also includes conventional battery separators, conventional battery casings, and other conventional structures / components / parts. Those skilled in the art can select appropriate processes based on the conventional manufacturing processes of chlorine-based batteries or the required chlorine-based battery model to prepare the rechargeable high-performance chlorine-based battery product based on the lithium-silicon alloy anode.

[0032] To better illustrate the present invention and provide a preferred technical solution for reference, when the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy anode is a 2032 coin cell, the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy anode further includes a glass fiber battery separator and a stainless steel battery casing.

[0033] In this paper, based on common knowledge of chlorine-based batteries in the prior art, the mass ratio of the negative electrode, positive electrode and electrolyte in the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy negative electrode follows the conventional chlorine-based battery process. Those skilled in the art can select a suitable process based on the existing technology to prepare the rechargeable high-performance chlorine-based battery product based on the conventional preparation process of chlorine-based batteries or the required chlorine-based battery model. Attached Figure Description

[0034] Figure 1 This diagram illustrates the structural principle of the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode prepared in Example 1 of this invention, and compares its cost and performance with that of a conventional chlorine-based battery. In the diagram, a is a schematic diagram of the structural principle of the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode prepared in Example 1; b is a cost comparison diagram between a conventional chlorine-based battery (Li / SOCl2) (Comparative Example 3) and the product prepared in Example 1; c is a diagram showing the capacity of a battery with the same anode area of ​​2.5 mAh cm⁻¹. -2In the case of conventional chlorine-based batteries (Li / SOCl2) (Comparative Example 3) and the product prepared in Example 1, the following schematic diagram compares their performance in terms of safety, cost-effectiveness, rate performance, energy density, and discharge voltage. The energy density and rate performance are evaluated based on the total mass of the positive and negative electrode materials, while the comparison of safety is non-quantitative.

[0035] Figure 2 The figures show the initial discharge performance and shelf life comparison curves of the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode prepared in Example 1 of this invention, and the chlorine-based batteries prepared in Comparative Examples 1 and 2. In the figures, a is the initial discharge performance comparison curve of the chlorine-based battery prepared in Example 1 (ALS-90% DCE) and Comparative Example 1 (ALS); b is the initial discharge performance comparison curve of the chlorine-based battery prepared in Example 1 (LSC anode) and Comparative Example 2 (Li anode) after shelf life of 0h, 120h, and 300h; c is the initial discharge capacity comparison curve of the chlorine-based battery prepared in Example 1 (LSC anode: ALS-90% DCE), Comparative Example 2 (Li anode: ALS-90% DCE), and Comparative Example 3 (Li anode, ALS) after shelf life of different times.

[0036] Figure 3 This figure shows the electrochemical performance of the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode prepared in Example 1 of this invention. In the figure, a is the constant current charge-discharge curve of the chlorine-based battery prepared in Example 1 at different specific capacities; b is a comparison of the battery cycle performance of the chlorine-based batteries prepared in Example 1 (LSC anode) and Comparative Example 2 (Li anode), with a charge specific capacity of 500 mAh g. -1 The current density is 500 mAg -1 c shows the rate performance of the chlorine-based battery prepared in Example 1, with a charge specific capacity of 500 mAh g. -1 ;d is a comparison graph of the energy density and power density of the chlorine-based battery prepared in Example 1 (This work) and the conventional chlorine-based battery (Li / SOCl2 battery);e is a constant current charge-discharge curve of the chlorine-based battery prepared in Example 1 at 25℃, -20℃, -40℃ and -60℃, with a current density of 500mAg in all cases. -1 f is a demonstration photo showing the application of the chlorine-based battery prepared in Example 1 lighting a commercial light bulb with a rated power of 3W at -32℃; g is a low-temperature cycling performance graph of the chlorine-based battery prepared in Example 1 at -20℃ and -40℃, with a current density of 500mA in both cases. -1h is a comparison graph of the low-temperature energy density retention rate of the chlorine-based battery prepared in Example 1 (This work) and other types of batteries.

[0037] Figure 4 The images show the Raman spectrum, solvation structure diagram, radial distribution function diagram, atomic charge difference, and molecular electrostatic potential energy diagram of the ALS-60%DCE electrolyte used in Example 2 of this invention, as well as the 1H NMR spectrum of the ALS-90%DCE electrolyte used in Example 1. In the figure, a is the Raman spectrum of the ALS-60% DCE electrolyte used in Example 2 with thionyl chloride (SOCl2), ALS electrolyte solution (ALS), and 1,2-dichloroethane (DCE); b is the MD simulation photograph of the ALS electrolyte solution (ALS) and the ALS-60% DCE electrolyte used in Example 2 at 298 K and the corresponding solvation structure schematic diagram; c is the radial distribution function (RDFs) diagram between different atoms in the ALS electrolyte solution (ALS); d is the radial distribution function (RDFs) diagram between different atoms in the ALS-60% DCE electrolyte used in Example 2; e is the atomic charge difference of the S=O bond in the DCE-SOCl2 complex at different molecular ratios obtained by DFT simulation and the molecular electrostatic potential energy diagram of DCE-SOCl2; f is the 1H NMR spectrum of the ALS-90% DCE electrolyte used in Example 1 with 1,2-dichloroethane (DCE).

[0038] Figure 5 This is a schematic diagram illustrating the passivation effect of cyclized polyacrylonitrile used in Example 1 of the present invention. In the figures, a and b are the three-dimensional and depth distribution maps of secondary ion fragments obtained by time-of-flight secondary ion mass spectrometry (TOF-SIMS) on the cycled LSC alloy anode, respectively; c and d are the three-dimensional and depth distribution maps of secondary ion fragments obtained by time-of-flight secondary ion mass spectrometry (TOF-SIMS) on the cycled lithium metal anode, respectively; both the LSC alloy anode and the lithium metal anode used ALS-90% DCE electrolyte (corresponding to Example 1 and Comparative Example 2, respectively); e is the Nyquist plot of the chlorine-based battery prepared in Example 1 under different charge-discharge cycles; f is the Nyquist plot of the chlorine-based battery prepared in Comparative Example 2 under different charge-discharge cycles; g is the high-resolution XPS spectrum of the F1s, N1s, and Cl2p orbitals of the amino battery prepared in Example 1 after pre-lithiation, initial discharge, and 20 cycles on the LSC alloy anode; h is the lithium metal anode (Li metal) and LSC alloy anode (Li-Si) of the amino batteries prepared in Comparative Example 2 and Example 1 after charge-discharge cycles, respectively. A schematic diagram of the passivation layer formed on the alloy.

[0039] Figure 6The figures show the first-cycle discharge comparison curves of the rechargeable high-performance chlorine-based batteries based on lithium-silicon alloy anodes prepared in Examples 1-3. In the figures, the chlorine-based battery prepared in Example 1 corresponds to ALS-90% DCE, the chlorine-based battery prepared in Example 2 corresponds to ALS-60% DCE, the chlorine-based battery prepared in Example 3 corresponds to ALS-30% DCE, and the chlorine-based battery prepared in Comparative Example 1 corresponds to ALS without DCE. Detailed Implementation

[0040] To further understand the present invention, preferred embodiments are described below with reference to examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and not for limiting the scope of the claims. Those skilled in the art can refer to the content of this document to appropriately improve the process parameters. In particular, it should be noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included within the scope of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and those skilled in the art can obviously make modifications or appropriate changes and combinations to the methods and applications described herein without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention. Although it is believed that those skilled in the art will fully understand the following terms, the following definitions are set forth to help illustrate the subject matter disclosed in the present invention.

[0041] An electrolyte for chlorine-based batteries, comprising, by volume percentage, the following components:

[0042] Lithium thionyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%;

[0043] The lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride.

[0044] In this document, the lithium thionyl chloride electrolyte solution is a lithium thionyl chloride electrolyte solution known in the art, namely, a lithium electrolyte solution composed of aluminum chloride and lithium salt mixed and dissolved in thionyl chloride (SOCl2). The lithium salt used is a type of lithium salt conventionally selected for electrolytes in lithium-ion / chlorine-based batteries in the prior art. In one embodiment, the lithium salt is selected from at least one of lithium chloride (LiCl), lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium di(oxalato)borate (LiDFOB), lithium trifluoromethanesulfonate (CF3SO3Li), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI).

[0045] In this document, the lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride. Generally speaking, the ratio between the above components can be in accordance with the conventional ratio of lithium thionyl chloride electrolyte solutions in the art, or the conventional ratio of electrolyte solutions applicable to lithium batteries / chlorine-based batteries as described in the prior art.

[0046] In one embodiment, experiments have confirmed that the ratio of aluminum chloride, lithium salt, and thionyl chloride in the lithium thionyl chloride electrolyte solution has almost negligible impact on the characterization of the various functions of the final prepared chlorine-based battery, especially the rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode described below. Therefore, using thionyl chloride as the solvent, the concentration of aluminum chloride can be arbitrarily selected within the range of 1–12 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, etc. The concentrations of the lithium salt are 1 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, or any range or value between them; the concentration of the lithium salt should not exceed the concentration of the aluminum chloride and should be ≥1 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, or any range or value between them. However, comparative experiments have shown that the ratio of aluminum chloride, lithium salt, and thionyl chloride significantly affects the electrochemical performance of the final prepared chlorine-based battery, especially the rechargeable high-performance chlorine-based battery based on the lithium-silicon alloy anode described below. Therefore, in one preferred embodiment, the thionyl chloride is used as the solvent, the concentration of the aluminum chloride is preferably arbitrarily selected within the range of 2 to 6 mol / L, and the concentration of the lithium salt should not exceed the concentration of the aluminum chloride and should be ≥2 mol / L.

[0047] To better illustrate the present invention and provide a preferred embodiment, the lithium thionyl chloride electrolyte solution is prepared by dissolving lithium chloride (LiCl) and aluminum chloride (AlCl3) in thionyl chloride (SOCl2). Under laboratory conditions, a specific preparation method can be as follows: add 8 mmol of AlCl3 and 8 mmol of LiCl to 2 ml of SOCl2 and stir for 8 hours. The resulting product is referred to as the ALS electrolyte solution. It should be noted that the specific preparation method of the lithium thionyl chloride electrolyte solution described above is only for illustrating this application and should not be considered as limiting the scope of this application. This preparation method is a conventional preparation method in the technical field of this invention, and other preparation methods of lithium thionyl chloride electrolyte solutions based on existing technologies can also be applied to this invention.

[0048] In one embodiment, when the lithium thionyl chloride electrolyte solution is prepared by adding lithium chloride (LiCl) and aluminum chloride (AlCl3) to thionyl chloride (SOCl2) and dissolving them together, lithium tetrachloroaluminate (LiAlCl4) can also be added directly as an alternative.

[0049] In one embodiment, the electrolyte for chlorine-based batteries described above is mainly composed of lithium thionyl chloride electrolyte solution and 1,2-dichloroethane. It should be noted that other conventional electrolyte additives / auxiliaries, especially functional additives, may also be added. Those skilled in the art can choose to add them according to the required functional needs. It is important to emphasize that the electrolyte for chlorine-based batteries in this invention may or may not contain other conventional electrolyte additives / auxiliaries.

[0050] In one embodiment, the electrolyte for the chlorine-based battery is prepared by mixing a lithium thionyl chloride electrolyte solution with 1,2-dichloroethane.

[0051] In one embodiment, the 1,2-dichloroethane has a volume percentage of 30-90%, for example, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%. %, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, or any range or point value between them.

[0052] In one preferred embodiment, in order to further improve the electrochemical performance of the chlorine-based battery and further reduce the production cost, the volume percentage of the 1,2-dichloroethane is 60-90%.

[0053] In one more preferred embodiment, in order to further improve the electrochemical performance of the chlorine-based battery and further reduce the production cost, the volume percentage of the 1,2-dichloroethane is 89-90%.

[0054] Secondly, based on the electrolyte for chlorine-based batteries provided above, this invention provides a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy negative electrode and its preparation method, which is achieved by adopting a technical solution consisting of the following technical measures.

[0055] A rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode, wherein the cathode uses a conventional carbon-based cathode material and the anode uses a polymer-coated lithium-silicon alloy material.

[0056] Its electrolyte, by volume percentage, mainly comprises the following components:

[0057] Lithium thionyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%;

[0058] The lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride;

[0059] The polymer-coated lithium-silicon alloy material, wherein the polymer is selected from any one of polyacrylonitrile, dopamine, polyvinylpyrrolidone, glucose, sucrose, and tannic acid; the lithium-silicon alloy is Li 15 Si4.

[0060] In this document, the cathode material used is a conventional carbon-based cathode material, which is the cathode material commonly used in lithium batteries / chlorine-based batteries. Those skilled in the art can select a suitable carbon-based cathode material based on existing technology or existing lithium battery / chlorine-based battery production processes.

[0061] In one embodiment, the cathode material is selected from at least one of Ketjen black, acetylene black, graphite, graphene, and carbon nanotubes.

[0062] To better illustrate the present invention and provide a preferred embodiment for reference, the positive electrode is prepared using polytetrafluoroethylene (PTFE) / Ketjen black material according to conventional lithium battery / chlorine-based battery processes. Under laboratory conditions, the specific preparation method may be as follows: Ketjen black (KJ) and PTFE are mixed at a mass ratio of 9:1, and then dispersed in ethanol via ultrasonic treatment to form a positive electrode slurry; the resulting positive electrode slurry is immersed in a nickel foam sheet with a diameter of 14 mm for positive electrodes and dried at 100°C to remove the ethanol; except for the addition of other third components, the Ketjen black (KJ) loading of the positive electrode is 1.28–1.32 mg / cm³. -2 .

[0063] In this document, the polymer-coated lithium-silicon alloy material includes any one of polyacrylonitrile, dopamine, polyvinylpyrrolidone, glucose, sucrose, and tannic acid. It should be noted that the polymer used should be able to coat the lithium-silicon alloy particles and possess a certain degree of conductivity. Due to the limited time available for conducting experiments related to this invention, the conductivity requirements of such polymers have not yet been systematically summarized. However, those skilled in the art can select polymers with similar or even better conductivity based on the polymer selections listed in this invention, achieving the same effect / function / purpose as the polymers listed in this invention. Furthermore, it should be additionally noted that polyacrylonitrile requires cyclization treatment before coating. The specific process for this cyclization treatment can refer to conventional cyclization treatment methods described in the prior art.

[0064] To better illustrate the present invention and provide a preferred embodiment for reference, when the polymer is polyacrylonitrile (PAN), it is prepared by coating silicon powder with polyacrylonitrile and then cyclizing it to obtain cyclized polyacrylonitrile-coated silicon (Si-PAN). The obtained Si-PAN is then pre-lithiated to prepare a lithium-silicon alloy material coated with cyclized polyacrylonitrile. Under laboratory conditions, the specific preparation method of the negative electrode can be as follows: 60 mg PAN and 140 mg silicon powder are mixed and stirred in 1.48 mL N,N-dimethylformamide (DMF) for at least 12 h to obtain a negative electrode slurry; the obtained negative electrode slurry is dried at 80 °C for 3 h, and then annealed in an argon atmosphere at 300 °C for 12 h to obtain Si-PAN; the obtained Si-PAN is punched into a circular electrode sheet with a diameter of 12 mm; then, using a conventional lithium battery electrolyte, the circular electrode sheet and lithium metal are used to form a Li / Si-PAN half-cell for pre-lithiation treatment: the Li / Si-PAN half-cell is pre-lithiated at 150 mAg. -1 The current density is discharged to 0.01V, and after washing with dimethyl carbonate (DMC) to remove residual electrolyte, the electrode is immediately disassembled to obtain a pre-lithiated circular negative electrode, referred to as LSC alloy negative electrode. The conventional lithium battery electrolyte used in the pre-lithiating treatment can be a commercially available lithium battery electrolyte, or a lithium battery electrolyte described in existing technology, such as 1M lithium hexafluorophosphate (LiPF6) commercial electrolyte (volume ratio EC:DMC:EMC = 1:1:1, LiPF6 concentration 1 mol / L) and 1M lithium bisfluorosulfonylimide (LiFSI) electrolyte (volume ratio EC:DMC = 1:1, LiFSI concentration 1 mol / L).

[0065] In this document, based on common knowledge of chlorine-based batteries in the prior art, the rechargeable high-performance chlorine-based battery based on the lithium-silicon alloy anode also includes conventional battery separators, conventional battery casings, and other conventional structures / components / parts. Those skilled in the art can select appropriate processes based on the conventional manufacturing processes of chlorine-based batteries or the required chlorine-based battery model to prepare the rechargeable high-performance chlorine-based battery product based on the lithium-silicon alloy anode.

[0066] To better illustrate the present invention and provide a preferred embodiment for reference, when the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy anode is a 2032 coin cell, the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy anode further includes a glass fiber battery separator and a stainless steel battery casing.

[0067] In this paper, based on common knowledge of chlorine-based batteries in the prior art, the mass ratio of the negative electrode, positive electrode and electrolyte in the rechargeable high-performance chlorine-based battery based on the lithium silicon alloy negative electrode follows the conventional chlorine-based battery process. Those skilled in the art can select a suitable process based on the existing technology to prepare the rechargeable high-performance chlorine-based battery product based on the conventional preparation process of chlorine-based batteries or the required chlorine-based battery model.

[0068] The present application will be further explained in detail below with reference to embodiments. However, those skilled in the art should understand that these embodiments are provided for illustrative purposes only and are not intended to limit the present application.

[0069] Example

[0070] The embodiments of this application will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be construed as limiting the scope of this application. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Where the manufacturers of reagents or instruments are not specified, they are all commercially available conventional products. This application should not be construed as being limited to the specific embodiments described.

[0071] 1. Raw materials

[0072] SOCl2 (99%, Aladdin), DCE (Water≤50ppm, 99.5%, Adamas), AlCl3

[0073] (98.0%, TCI), LiCl (water content less than 10 ppm, 99.99%, Adamas), N,N-dimethylformamide (DMF, water content less than 50 ppm, Adamas), DMC (water ≤ 50 ppm, 99.5%, Adamas);

[0074] PAN (99%, Mw = 150,000);

[0075] Nanoscale Si powder (99.99%, 80-100nm) was purchased from Guangdong Kangde New Energy Technology Co., Ltd.

[0076] The polytetrafluoroethylene (PTFE) emulsion binder (60%, D-210C) and Ketjen Black KJ (epc-600jd) were purchased from Cyber ​​Electrochemical Materials.

[0077] 2. Preparation method

[0078] (1) Preparation of positive electrode

[0079] Ketjen black (KJ) and polytetrafluoroethylene (PTFE) were mixed at a mass ratio of 9:1 and then ultrasonically dispersed in ethanol to form a positive electrode slurry. The resulting positive electrode slurry was immersed in a 14 mm diameter nickel foam sheet for positive electrodes and dried at 100 °C to remove the ethanol. The mass loading of Ketjen black (KJ) in the positive electrode was 1.28–1.32 mg·cm³. -2 .

[0080] (2) Preparation of LSC alloy anode

[0081] 60 mg of polyacrylonitrile (PAN) and 140 mg of silicon powder were mixed and stirred in 1.48 mL of N,N-dimethylformamide (DMF) for at least 12 h to obtain a negative electrode slurry. The resulting negative electrode slurry was dried at 80 °C for 3 h and then annealed at 300 °C in an argon atmosphere for 12 h to obtain Si-PAN. The obtained Si-PAN was punched into a negative electrode circular sheet with a diameter of 12 mm. Then, using a conventional lithium battery electrolyte, the negative electrode circular sheet and a lithium metal positive electrode were used to form a Li / Si-PAN half cell for pre-lithiation treatment. The Li / Si-PAN half cell was subjected to a 150 mA g-load test. -1 Discharge to 0.01V at a current density, wash with dimethyl carbonate (DMC) to remove residual electrolyte, and immediately disassemble to obtain a pre-lithiated circular negative electrode, referred to as LSC alloy negative electrode;

[0082] The conventional lithium battery electrolyte is a 1M lithium hexafluorophosphate (LiPF6) commercial electrolyte (volume ratio EC:DMC:EMC = 1:1:1, LiPF6 concentration is 1mol / L).

[0083] (3) Preparation of ALS-DCE electrolyte

[0084] Add 8 mmol AlCl3 and 8 mmol LiCl to 2 ml SOCl2 and stir for 8 hours. The resulting product is referred to as ALS electrolyte solution. Mix 10-70% of the ALS electrolyte solution with 30-90% of 1,2-dichloroethane (DCE) by volume to prepare ALS-DCE electrolyte.

[0085] (4) Fabrication of a rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode

[0086] 2032 type coin cell was prepared as a test sample: 150 μL of ALS-DCE electrolyte was added to a glass fiber separator (GF / D, Whatman) and formed an LSC / SOCl2 cell with the prepared LSC alloy negative and positive electrodes.

[0087] The battery casing is made of 316 stainless steel. For pouch batteries, a glass fiber membrane is used as a separator. The amount of electrolyte is increased according to the weight of Si (approximately 100 μL / mg). The positive electrode area is kept slightly larger than the negative electrode area to ensure that all capacity is effectively utilized.

[0088] 3. Testing Methods

[0089] The Raman spectrum of the electrolyte was obtained using Renishaw inVia Qontor confocal Raman microscopy at an excitation laser wavelength of 532 nm.

[0090] SEM images were obtained using a Zeiss Gemini 300 field emission scanning electron microscope. TOF-SIMS data were obtained from an ION-TOF 5-100 instrument using a Cs+ sputtering beam with a sputtering area of ​​250 × 250 μm. 2 .

[0091] XPS spectra were obtained using a Thermo Fisher Scientific K-Alpha+ X-ray photoelectron spectrometer. NMR spectra of the electrolyte were measured using a Bruker Avance III 500MHz liquid nuclear magnetic resonance spectrometer.

[0092] Unless otherwise stated, all electrochemical measurements were performed in a constant temperature test chamber at 25°C.

[0093] The battery electrochemical performance was tested using the Neware battery testing system.

[0094] Specific capacity and current density are calculated based on the mass of silicon, while energy / power density is calculated based on the total mass of the positive / negative electrode materials.

[0095] Examples 1-3

[0096] Examples 1-3 are test samples of rechargeable high-performance chlorine-based batteries (2032 coin cells) based on lithium silicon alloy anodes prepared according to the above preparation methods (1)-(4).

[0097] In Example 1, the ALS-90%DCE electrolyte was prepared by mixing 10% ALS electrolyte solution with 90% 1,2-dichloroethane (DCE) by volume percentage.

[0098] In Example 2, by volume percentage, an ALS-60%DCE electrolyte was prepared by mixing 40% ALS electrolyte solution with 60% 1,2-dichloroethane (DCE).

[0099] In Example 3, the ALS-30%DCE electrolyte was prepared by mixing 70% ALS electrolyte solution with 30% 1,2-dichloroethane (DCE) by volume percentage.

[0100] Comparative Example 1

[0101] In Comparative Example 1, no 1,2-dichloroethane (DCE) was added during the preparation of ALS-DCE electrolyte as described in the above preparation method (3), and 100% ALS electrolyte solution was used by volume percentage.

[0102] The remaining parts were prepared according to the above preparation methods (1) to (4) to obtain chlorine-based batteries (2032 type button batteries) as test samples.

[0103] Comparative Example 2

[0104] Comparative Example 2 uses a traditional lithium metal anode and the remaining parts are prepared according to the above preparation methods (1), (3), and (4) to obtain a chlorine-based battery (2032 coin cell) as a test sample.

[0105] Comparative Example 3

[0106] Comparative Example 3 uses a conventional lithium metal anode. In the preparation of ALS-DCE electrolyte as described in the above preparation method (3), no 1,2-dichloroethane (DCE) was added. The ALS electrolyte solution was 100% by volume.

[0107] The remaining parts were prepared according to the above preparation methods (1), (3), and (4) to obtain chlorine-based batteries (2032 type button cells) as test samples.

[0108] 4. Test Conclusion

[0109] like Figure 1As shown, the synergistic design of electrolyte dilution and negative electrode / electrolyte interface passivation is key to achieving reversible Li-Si alloying / dealloying reactions in chlorine-based electrolytes. 1,2-Dichloroethane (DCE), as an effective diluent, can mitigate the corrosiveness of thionyl chloride (SOCl2)-based electrolytes. Cyclic polyacrylonitrile, as a robust passivation layer, can suppress parasitic reactions between the lithium-silicon alloy and thionyl chloride (SOCl2). Together, they achieve, for the first time, reversible silicon redox in chlorine-based electrolytes. Compared to conventional chlorine-based batteries (Li / SOCl2) (Comparative Example 3), the use of inexpensive silicon-based negative electrodes and a large amount of 1,2-dichloroethane (DCE) reduces costs by up to 84%.

[0110] like Figure 2 As shown, batteries using ALS electrolyte cannot provide any usable discharge capacity due to severe parasitic reactions between the lithium-silicon alloy and the corrosive chlorine-based electrolyte. In contrast, adding 90% 1,2-dichloroethane (DCE) to ALS provides 2,720 mAh g⁻¹. -1 High specific capacity (based on Si quality), and a distinct discharge plateau at ~3V. Figure 2 a) A Li / SOCl2 battery prepared using ALS-90% DCE electrolyte (Comparative Example 2) provided 2,991 mAh g. -1 It has a high discharge capacity, but due to the severe corrosion of lithium metal of the same capacity in SOCl2-based electrolytes, it cannot discharge after being left to stand for 120 hours. Figure 2 b). In contrast, the LSC / SOCl2 battery (Example 1) retained 98.7% of its original capacity after being left to stand for 300 hours. Figure 2 b); Even after 600 hours of retention, it retains 95.3% of its original capacity. Figure 2 c) This indicates that our LSC metal anode exhibits good electrochemical stability. The stable open-circuit voltage (OCV) of our LSC / SOCl2 cell (Example 1) during a 1,000-hour shelf life further confirms its excellent shelf performance. Figure 2 d). In stark contrast, conventional Li / SOCl2 batteries (Comparative Example 3) using a corrosive ALS electrolyte without 1,2-dichloroethane (DCE) dilution showed a rapid decrease in OCV within just 10 hours. Figure 2 d) This indicates that our Si-based anode has a shelf life 100 times longer than that of a lithium anode battery of the same capacity.

[0111] like Figure 3As shown, our rechargeable LSC / SOCl2 battery (Example 1) using ALS-90% DCE electrolyte exhibited high reversibility at different rated charge capacities based on Si mass. Figure 3 a) At 500mA g -1 At a current density of 500 mAh g, the LSC / SOCl2 battery... -1 At a fixed charge capacity, the average coulombic efficiency (CE) is approximately 98% over more than 250 cycles. In stark contrast, a conventional Li / SOCl2 battery (Comparative Example 2) completely fails after only 25 cycles under the same conditions using the same anode capacity. The rapid kinetics of our silicon anode chemistry also provide excellent rate capability for the LSC / SOCl2 battery; for example, a maximum current density of up to 5 Ag based on the ALS-90% DCE electrolyte. -1 ( Figure 3 c). Based on the total mass of the positive / negative electrode materials, our LSC / SOCl2 battery achieved a power and energy density of 4,277 W kg. -1 and 809Wh kg -1 This significantly exceeds the ~279W kg of state-of-the-art Li / Cl2 batteries. –1 and ~418Wh kg -1 value ( Figure 3 d). Traditional lithium-ion batteries exhibit poor electrochemical performance at low temperatures, posing a long-standing challenge for practical applications. The rapid kinetics of our LSC / SOCl2 battery enable the battery using the ALS-90% DCE electrolyte (Example 1) to demonstrate excellent electrochemical performance at -20°C and -40°C. Figure 3 e, g). Our battery exhibits good reversibility, with only a slight increase in overpotential even at -60°C using the ALS-60% DCE electrolyte (Example 2), retaining approximately 95% of the room temperature energy density. Figure 3 e). It is also highly competitive compared to state-of-the-art lithium-ion and Li / Na / K metal batteries that operate at low temperatures. Figure 3 h).

[0112] like Figure 4 As shown, in Raman spectra ( Figure 4 a) SOCl2 at 342 and 490 cm⁻¹ -1 The characteristic peaks at 361 and 503 cm⁻¹ represent the symmetrical Cl-S-Cl deformation vibration and the symmetrical S-Cl tensile vibration, respectively. After the addition of AlCl₃ and LiCl, these peaks are observed at 361 and 503 cm⁻¹, respectively. -1 The formation of a new peak indicates that Li +The formation of the -SOCl2 complex; the addition of DCE caused a significant blue shift in the complex peaks, and the obvious splitting of the symmetrical Cl-S-Cl deformation vibration and symmetrical S-Cl tensile vibration peaks indicated that Li + The enhanced interaction between DCE and SOCl2 indicates that DCE molecules squeeze and shield Li + -SOCl2 complex, rather than coordinated with Li ions. We also observed a slight blue shift in the Cl-SO symmetric deformation vibration and S-Cl asymmetric stretching vibration peaks, as well as a red shift in the S=O stretching vibration peak, indicating that DCE enhances the non-uniformity of the electron cloud density on the SOCl2 molecule, which ensures normal battery reactivity at high DCE levels. Further molecular dynamics (MD) simulations were performed to provide a deeper understanding of electrolyte dissolution. Figure 4 (be)MD simulation snapshots show that SOCl2 molecules coordinated around lithium ions are surrounded by DCE ( Figure 4 b). According to the radial distribution functions (RDFs), the lithium-ion solvent sheath is mainly composed of Li-O (SOCl2) and Li-Al (AlCl4). - Composed of ) respectively in 2.3 and ( Figure 4 c). The presence of 60% DCE slightly shortens the Li-O(SOCl2) and Li-Al(AlCl4) bonding time. - The distance, and in A new Li-C(DCE) peak was formed at this location. Figure 4 d). This indicates that DCE molecules participate in the first dissolved sheath structure around lithium ions, thus enabling them to act as an effective diluent and effectively inhibit corrosion of SOCl2-based electrolytes. The interaction between SOCl2 and DCE molecules was further investigated by density functional theory (DFT) simulations and nuclear magnetic resonance (NMR). Electrostatic potential (ESP) analysis from DFT simulations showed that intermolecular hydrogen bonds (S=O—H-Cl) formed between SOCl2 and DCE. Figure 4 e). Furthermore, the increase in DCE content enhances the polarization of the S=O bond ( Figure 4 e). NMR results showed that in the ALS electrolyte, the chemical shift of hydrogen in the DCE shifted to a higher field ( Figure 4 f) confirmed the intermolecular interaction between DCE and SOCl2, which ensures that the DCE molecule supports Li + The tight encapsulation of the SOCl2 complex greatly reduces the corrosiveness of the electrolyte to the electrodes and the battery.

[0113] like Figure 5As shown, we investigated the chemical composition of the solid-electrolyte interface (SEI) phase using time-of-flight secondary ion mass spectrometry (TOF-SIMS). After 30 charge-discharge cycles, a thin lithium chloride layer was observed on the surface of the LSC metal anode. Figure 5 (a, 5b). Similarly, the detected S signal was much weaker, indicating that corrosion of the LSC metal anode was suppressed. In stark contrast, a thicker passivation layer, mainly composed of LiCl and S, was detected on the surface of the cycled lithium metal anode, exhibiting poor uniformity. Figure 5 c, 5d), indicating severe corrosion of metallic lithium during battery cycling. Electrochemical impedance spectroscopy (EIS) further showed that the charge transfer resistance (Rct) of the Li / SOCl2 battery (Comparative Example 2) increased significantly, increasing by 104.1% after 20 cycles. Figure 5 f), while our LSC / SOCl2 battery only increased by 24.7% after 50 cycles (f). Figure 5 e). This confirms the passivation effect of cyclized PAN, which suppresses parasitic reactions between the lithium-silicon alloy and the electrolyte, thus providing high electrochemical reversibility. We further performed X-ray photoelectron spectroscopy (XPS) to elucidate the evolution of the SEI under different charge-discharge states. We found that PAN and LiF coexist in the SEI during battery cycling. The strength of lithium chloride did not increase significantly during cycling (e). Figure 5 g), indicating effective passivation of the PAN and the derived SEI layer. Therefore, our LSC anode exhibits significant stability in SOCl2-based electrolytes, further suppressing corrosion of the Li-Si alloy anode by the ALS-DCE electrolyte through the construction of an effective interphase layer at the anode / electrolyte interface. Figure 5 h).

[0114] like Figure 6 As shown, compared with the battery performance without DCE, adding different amounts of DCE can achieve a certain initial discharge capacity, indicating that the presence of DCE plays a key role in reducing the corrosiveness of the electrolyte.

[0115] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A rechargeable high-performance chlorine-based battery based on a lithium-silicon alloy anode, characterized in that... The positive electrode uses carbon-based positive electrode material, and the negative electrode uses polymer-coated lithium-silicon alloy material; Its electrolyte, by volume percentage, mainly comprises the following components: Lithium thionyl chloride electrolyte solution 10-70%, 1,2-dichloroethane 30-90%; The lithium thionyl chloride electrolyte solution is composed of aluminum chloride, lithium salt and thionyl chloride; The carbon-based cathode material is selected from at least one of Ketjen black, acetylene black, graphite, graphene, and carbon nanotubes. The polymer-coated lithium-silicon alloy material, wherein the polymer is selected from any one of polyacrylonitrile, dopamine, polyvinylpyrrolidone, glucose, sucrose, and tannic acid; the lithium-silicon alloy is Li 15 Si4.

2. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: The lithium salt is selected from at least one of lithium chloride, lithium hexafluorophosphate, lithium difluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium di(oxalate)borate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide.

3. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: The thionyl chloride is used as a solvent, the concentration of aluminum chloride is 1~12 mol / L, and the concentration of lithium salt is not greater than the concentration of aluminum chloride and is ≥1 mol / L.

4. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: The thionyl chloride is used as a solvent, the concentration of aluminum chloride is 2~6 mol / L, and the concentration of lithium salt is not greater than the concentration of aluminum chloride and is ≥2 mol / L.

5. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: The volume percentage of the 1,2-dichloroethane is 60-90%.

6. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: The volume percentage of the 1,2-dichloroethane is 89-90%.

7. The rechargeable high-performance chlorine-based battery according to claim 1, characterized in that: When the polymer is polyacrylonitrile, the polyacrylonitrile is coated with silicon powder and then cyclized to obtain cyclized polyacrylonitrile-coated silicon. The cyclized polyacrylonitrile-coated silicon is then pre-lithiated to prepare a lithium-silicon alloy material coated with cyclized polyacrylonitrile.

Citation Information

Patent Citations

  • Electrolyte for chemical source of energy

    RU1688757C

  • Additive to zinc-plating electrolytes

    SU1177399A1