Method of manufacturing electrode assembly and electrode assembly manufacturing apparatus
By applying heat and pressure during the manufacturing process of electrode assemblies through a combination of primary and secondary hot pressing, along with fixtures and pressing units, the problems of positional deformation and damage of electrode assemblies during manufacturing are solved, resulting in higher manufacturing uniformity and energy density.
Patent Information
- Application Number
- CN202280013323.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-09
- Filing Date
- 2022-07-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-07-08
AI Technical Summary
During the manufacturing of electrode assemblies, issues such as electrode position deformation and mechanical component damage arise, especially in stacked-folded electrode assemblies where the Z-shaped folding of the electrodes leads to position deformation and warping.
The electrode stacking position is fixed by a clamp using a method of primary hot pressing and secondary hot pressing, and heat and pressure are applied at 50°C to 90°C and 1 MPa to 6 MPa. The pressing unit heats and presses the electrodes and diaphragm to prevent electrode deformation.
It effectively prevents damage and deformation of electrode components, improves manufacturing uniformity, reduces differences in adhesion and permeability between electrodes and diaphragms, and enhances the energy density of electrode components.
Smart Images

Figure CN116888784B_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2021-0090596, filed July 9, 2021; Korean Patent Application No. 10-2021-0090592, filed July 9, 2021; Korean Patent Application No. 10-2021-0090597, filed July 9, 2021; and Korean Patent Application No. 10-2021-0090598, filed July 9, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a method and apparatus for manufacturing electrode assemblies. Background Technology
[0003] Unlike primary batteries, rechargeable batteries are rechargeable and have been extensively researched and developed in recent years due to their small size and large capacity. With technological advancements and increasing demand for mobile devices, the need for rechargeable batteries as an energy source is rapidly growing.
[0004] Based on the shape of the battery casing, secondary batteries can be classified into button batteries, cylindrical batteries, prismatic batteries, and pouch batteries. In secondary batteries, the electrode assembly installed inside the battery casing is a rechargeable / dischargeable power generation element, which has a stacked structure including electrodes and a separator.
[0005] Electrode assemblies can generally be classified into wound type, stacked type, and stack-folded type. In the wound type, a separator is inserted between sheet-shaped positive and negative electrodes, both coated with active material, and the entire arrangement is wound up. In the stacked type, multiple positive and negative electrodes are stacked sequentially with separators inserted between them. In the stack-folded type, stacked cell units are wound together with long separators.
[0006] In stacked-folded electrode assemblies, the problem is that the position of the electrodes is deformed from the diaphragm folded in a zigzag manner and the electrodes are positioned in between.
[0007] [Existing Technical Documents]
[0008] [Patent Literature]
[0009] Korean Patent Application Publication No. 10-2013-0132230 Summary of the Invention
[0010] Technical issues
[0011] The present invention particularly provides a method and apparatus for manufacturing electrode assemblies, which prevents battery damage and deformation of mechanical components during the manufacturing process of electrode assemblies (involving stacking electrodes with a separator).
[0012] The present invention also provides an apparatus for manufacturing electrode assemblies, which can prevent the electrodes from deforming during the manufacturing process.
[0013] Technical solutions to the problem
[0014] An exemplary aspect of the present invention provides a method for manufacturing an electrode assembly. The method according to this aspect of the invention preferably includes the following steps: assembling an electrode stack; then performing a first hot-pressing operation on the electrode stack; and then performing a second hot-pressing operation on the electrode stack. The electrode stack assembled in the assembly step preferably comprises a plurality of electrodes stacked along a stack axis, wherein a corresponding diaphragm portion is positioned between each electrode. In the first hot-pressing operation, the electrode stack may be engaged with a jig to fix the position of the electrode stack. Then, as part of the first hot-pressing operation, heat and pressure may be applied to the electrode stack while the jig is engaged with the electrode stack. In the second hot-pressing operation, the jig may be disengaged from the electrode stack, and then, as part of the second hot-pressing operation, heat and pressure may be applied to the electrode stack. The second hot-pressing operation preferably also includes applying heat and pressure to the electrode stack for a period of 5 to 60 seconds at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa.
[0015] According to some aspects of the invention, the diaphragm portion may be part of an elongated diaphragm sheet. In these aspects of the invention, the step of assembling the electrode stack may include alternately stacking a first electrode and a second electrode on the elongated diaphragm sheet. Furthermore, the elongated diaphragm sheet is sequentially folded over previously stacked electrodes of the first and second electrodes, and then subsequent electrodes of the first and second electrodes are stacked.
[0016] Another exemplary aspect of the invention provides an apparatus for manufacturing an electrode assembly. Such an electrode assembly may include an electrode stack having a plurality of first and second electrodes stacked along a stack axis, with a corresponding diaphragm positioned between each of the first and second electrodes. The apparatus according to this aspect of the invention preferably includes a pressing unit and a clamp. The pressing unit binds the electrodes and the diaphragm portions within the electrode stack together by applying heat and pressure to the electrode stack. The clamp engages the electrode stack to fix its position when heat and pressure are applied to it by the pressing unit. The clamp and the pressing unit are ideally configured such that the pressing unit can apply heat and pressure to the electrode stack when the clamp is engaged with the electrode stack and when the clamp is disengaged from the electrode stack.
[0017] According to some aspects of the invention, the device may further include: a stacking platform for supporting the electrode stack; a diaphragm supply unit for supplying the diaphragm to the stacking platform; a first electrode supply unit for supplying the first electrode to the stacking platform; a second electrode supply unit for supplying the second electrode to the stacking platform; a first electrode stacking unit for moving the first electrode supplied from the first electrode supply unit to the stacking platform; and a second electrode stacking unit for moving the second electrode supplied from the second electrode supply unit to the stacking platform.
[0018] According to other aspects of the invention, the device may further include a rotating unit for rotating the stacking platform between a first position and a second position. The first position may be oriented toward the first electrode stacking unit for receiving the first electrode from the first electrode stacking unit, and the second position may be oriented toward the second electrode stacking unit for receiving the second electrode from the second electrode stacking unit.
[0019] Beneficial effects of the invention
[0020] According to the invention, by heating and pressing the entire stack with a pressing unit, electrodes can be bonded to diaphragms without individually heating and / or pressing each level of the electrode assembly (i.e., heating and / or pressing each electrode and diaphragm pair at each step of the process). The electrodes and diaphragms are then heated and stacked. Therefore, it is advantageous to avoid harmful accumulation of heat and / or pressure in the lower diaphragm of the stack, thereby reducing the likelihood of damage and deformation to the components of the electrode assembly.
[0021] The present invention can also advantageously reduce the adhesion between the electrode and the diaphragm, the air permeability of the diaphragm, and the thickness deviation of the manufactured electrode assembly, thereby increasing uniformity.
[0022] By pressing the entire stacked assembly with a pressing unit, the present invention also ideally reduces any deformation or displacement of the electrode positions within the electrode stack. Advantageously, this reduces manufacturing time and increases the energy density of the manufactured electrode assemblies. Attached Figure Description
[0023] Figure 1 This is a diagram schematically illustrating a method for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0024] Figure 2 This is a top plan view illustrating an embodiment of an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0025] Figure 3 This is a conceptual front view illustrating an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0026] Figure 4 This is a cross-sectional view showing an electrode assembly manufactured by an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0027] Figure 5 This is a perspective view illustrating a pressing unit in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0028] Figure 6 This is a perspective view showing an embodiment of a pressing unit in a state of pressing and stacking in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0029] Figure 7 This is a perspective view showing a stacking platform in an apparatus for manufacturing electrode assemblies according to an exemplary embodiment of the present invention.
[0030] Figure 8 This is a perspective view showing a first electrode mounting stage in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0031] Figure 9 This is a perspective view showing a second electrode mounting stage in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0032] Figure 10 This is a perspective view showing a first suction head in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0033] Figure 11 This illustrates an exemplary embodiment of the present invention. Figure 10 A bottom view of the first suction head.
[0034] Figure 12 This is a top plan view illustrating the holding mechanism and stacking stage in an apparatus for manufacturing electrode assemblies according to an exemplary embodiment of the present invention.
[0035] Figure 13 This is a conceptual front view illustrating an apparatus for manufacturing an electrode assembly according to another exemplary embodiment of the present invention.
[0036] Figure 14 This is a perspective view of the diaphragm heating unit of a diaphragm supply unit according to an exemplary embodiment of the present invention.
[0037] Figure 15 A is a perspective view illustrating a first pressing unit according to an exemplary embodiment of the present invention, and Figure 15 B is a perspective view illustrating a second pressing unit according to an exemplary embodiment of the present invention.
[0038] <Figure Labels>
[0039] 10: Assembled electrode assembly
[0040] 11: First electrode
[0041] 11a: First electrode connector
[0042] 12: Second electrode
[0043] 12a: Second electrode connector
[0044] 14: Diaphragm
[0045] 50: First pressing unit
[0046] 50a, 50b: First pressing block
[0047] 51: Fixture
[0048] 51a: Main body
[0049] 51b: Fixing part
[0050] 52: Clamping slot
[0051] 60: Second pressing unit
[0052] 60a, 60b: Second pressing blocks
[0053] 100, 200: Equipment used for manufacturing electrode assemblies
[0054] 110: Stacking Platform
[0055] 111: Main body of Taiwan
[0056] 112: Stacking Platform Heater
[0057] 120: Diaphragm Supply Unit
[0058] 121: Diaphragm heating unit
[0059] 121a: Ontology
[0060] 121b: Diaphragm heater
[0061] 122: Diaphragm roller
[0062] 130: First electrode supply unit
[0063] 131: First electrode sealing stage
[0064] 133: First electrode roller
[0065] 134: First Cutter
[0066] 135: First Conveyor Belt
[0067] 136: First electrode supply head
[0068] 140: Second electrode supply unit
[0069] 141: Second electrode mounting platform
[0070] 143: Second electrode roller
[0071] 144: Second cutter
[0072] 145: Second Conveyor Belt
[0073] 146: Second electrode supply head
[0074] 150: First electrode stacking unit
[0075] 151: First suction head
[0076] 151a: Vacuum suction port
[0077] 151b: Bottom surface
[0078] 153: First moving unit
[0079] 160: Second electrode stacking unit
[0080] 161: Second suction head
[0081] 163: Second moving unit
[0082] 170: Maintaining the organization
[0083] 171: First Holder
[0084] 172: Second Holder
[0085] 180: Pressing unit
[0086] 181, 182: Pressing blocks
[0087] 183, 184: Press the heater
[0088] 290: Visual Device
[0089] 291: The First Camera
[0090] 292: Second Camera
[0091] R: Rotation unit
[0092] S: Stacking Detailed Implementation
[0093] The objects, specific advantages, and novel features of the present invention will become more apparent from the following detailed description taken in conjunction with the accompanying drawings and exemplary embodiments. In this specification, when adding reference numerals to the constituent elements of each figure, it should be noted that even if the same constituent elements are indicated in different figures, these same constituent elements are given the same reference numerals. Furthermore, the present invention can be embodied in several different forms and is not limited to the exemplary embodiments described herein. Moreover, in describing the present invention, detailed descriptions of related known technologies that may unnecessarily obscure the essential points of the invention will be omitted.
[0094] According to an exemplary embodiment of the present invention, a method for manufacturing an electrode assembly can be provided. The method may include: supplying a first electrode to a stacking stage; supplying a second electrode to the stacking stage; supplying a diaphragm to the stacking stage; and assembling a stack on the stacking stage by alternately stacking the first and second electrodes on the diaphragm, wherein the diaphragm is sequentially folded over previously stacked electrodes of the first and second electrodes, and then subsequent electrodes of the first and second electrodes are stacked. After assembling the stack, the method may include performing a first hot-pressing operation, which includes clamping the stack with a jig, and then heating and pressing the stack. After performing the first hot-pressing operation, the method may further include performing a second hot-pressing operation, which includes removing the jig, and then heating and pressing the stack. The second hot-pressing operation may include pressing the stack for a period of 5 to 60 seconds at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa.
[0095] In an exemplary embodiment of the present invention, a hot pressing operation may include: securing the stack by pressing the upper surface of the stack with a clamp; heating the stacking platform and / or a pair of pressing blocks; and pressing the stack between the pair of heated pressing blocks or between the pressing blocks and the stacking platform (either or both of the pressing blocks and the stacking platform may be heated).
[0096] In an exemplary embodiment of the invention, each of the first electrode, the second electrode, and the diaphragm can be supplied to the stacking platform while being heated. This means that the first electrode, the second electrode, and the diaphragm can be heated by conventional methods before being supplied to the stacking platform, provided that the first electrode, the second electrode, and the diaphragm are not damaged by such heating.
[0097] In an exemplary embodiment of the present invention, a single hot-pressing operation may include heating and pressing the stack for 10 to 30 seconds at a temperature of 65°C to 90°C and a pressure of 1 MPa to 3 MPa. More preferably, a single hot-pressing operation may include heating and pressing the stack for 10 to 20 seconds at a temperature of 65°C to 75°C and a pressure of 1.5 MPa to 2 MPa.
[0098] In an exemplary embodiment of the present invention, the secondary hot pressing operation may include: stopping the heating of the stacking platform and / or a pair of pressing blocks; stopping the pressing of the stack; removing the fixture from the stack; heating the stacking platform and / or a pair of pressing blocks to transfer heat to the stack; and pressing the stack between a pair of pressing blocks, or pressing the stack between a pressing block and a stacking platform (one or both of the pressing block and the stacking platform may be heated).
[0099] In an exemplary embodiment of the invention, a pair of pressing blocks may include a pressing heater for heating the pair of pressing blocks, such that the pair of pressing blocks can be heated and stacked. That is, in an exemplary embodiment of the invention, the operation of heating and pressing the stack may include heating and pressing the stack with a pair of pressing blocks. In some exemplary embodiments of the invention, the stacking platform may also include a stacking platform heater for heating the body of the stacking platform to transfer heat to the stack.
[0100] In an alternative embodiment of the invention, one or both of the hot-pressing operations may occur on the stacking table. In this case, only one of the pressing blocks may be used to press the top of the stack downwards against the stacking table. In this case, the clamp may be a holding mechanism of the stacking table, which can stabilize the stack by fixing the position of the stack relative to the stacking table. Furthermore, the holding mechanism may be configured to fix the stack in this manner at least during one hot-pressing operation.
[0101] In this instruction manual, Figure 1 This is a diagram schematically illustrating a method for manufacturing an electrode assembly according to an exemplary embodiment of the present invention. That is, referring to... Figure 1 The method may first include a stacking process on a stacking table to assemble a stack (a stacked battery) by alternately stacking a first electrode and a second electrode on a separator, wherein the separator is sequentially folded over previously stacked electrodes in the first and second electrodes, and then subsequent electrodes in the first and second electrodes are stacked. After this stacking process, the stack can be removed from the stacking table. During this process, the separator is pulled, and after being pulled to a predetermined length, the separator is cut. Subsequently, the predetermined length of the cut end of the separator is wound around the stacked battery. The movement of the stack away from the stacking table can be achieved by means of a clamp, ideally a movable component capable of holding the stack on the stacking table and then moving the stack to a pressing unit for a thermo-pressing operation. Then, a thermo-pressing operation is performed while the wound stacked battery is held by the clamp. After the first thermo-pressing operation is completed, the clamp is released from the stacked battery, and a second thermo-pressing operation is performed after the clamp is removed. When the second thermo-pressing operation is completed, the finished electrode assembly can be completed.
[0102] In an exemplary embodiment of the present invention, the temperature conditions for the secondary hot pressing operation can be 50°C or higher, preferably 65°C or higher.
[0103] In an exemplary embodiment of the present invention, the temperature conditions for the secondary hot pressing operation can be below 90°C, preferably below 85°C.
[0104] In an exemplary embodiment of the present invention, the temperature conditions for the secondary hot pressing operation can be 50°C to 90°C, preferably 65°C to 90°C, more preferably 65°C to 85°C. Most preferably, the temperature conditions for the secondary hot pressing operation can be 70°C.
[0105] In an exemplary embodiment of the present invention, the pressure condition for the secondary hot pressing operation can be 1 MPa or more, preferably 1.5 MPa or more, and more preferably 3 MPa or more.
[0106] In an exemplary embodiment of the present invention, the pressure conditions for the secondary hot pressing operation can be below 6 MPa, preferably below 5.5 MPa.
[0107] In an exemplary embodiment of the present invention, the pressure conditions for the secondary hot pressing operation can be 1 MPa to 6 MPa, preferably 1.5 MPa to 6 MPa, and more preferably 3 MPa to 5.5 MPa.
[0108] In an exemplary embodiment of the present invention, the heating and pressing in the secondary hot pressing operation can be performed for more than 5 seconds, preferably more than 7 seconds.
[0109] In an exemplary embodiment of the present invention, the heating and pressing in the secondary hot pressing operation can be performed for 60 seconds or less, preferably 30 seconds or less, and more preferably 25 seconds or less.
[0110] In an exemplary embodiment of the present invention, the heating and pressing in the secondary hot pressing operation can last for a period of 5 to 60 seconds, preferably 5 to 30 seconds, and more preferably 7 to 25 seconds.
[0111] In an exemplary embodiment of the present invention, the secondary hot-pressing operation may involve heating and pressing the stacks at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa for 5 to 60 seconds, preferably at a temperature of 65°C to 90°C and a pressure of 1.5 MPa to 6 MPa for 5 to 30 seconds. More preferably, the secondary hot-pressing operation may involve heating and pressing the stacks at a temperature of 65°C to 85°C and a pressure of 3 MPa to 5.5 MPa for 7 to 25 seconds. Here, a temperature of 70°C is most preferred.
[0112] Here, the pressure conditions for the primary and secondary hot-pressing operations refer to the pressure applied by a pair of pressure blocks (or by means of pressure blocks against the stacking table), and the temperature conditions refer to the temperature of the heat applied by the stacking table and / or the pair of pressing blocks. Furthermore, the pair of pressing blocks used for the primary and secondary hot-pressing operations can be the same or different. That is, during the primary hot-pressing operation, after the stack is pressed and heated with a pair of pressing blocks while held in a clamp, in the secondary hot-pressing operation after releasing the clamp, the stack can later be pressed and heated with the same pair of pressing blocks or with a different pair of pressing blocks.
[0113] In an alternative embodiment where at least one hot-pressing operation occurs on the stacking platform, as described above, a single hot-pressing operation may involve a pressing block applying pressure to a stack disposed on the stacking platform, wherein the stack is heated by one or both of a heater in the stacking platform and / or the pressing block. During such a single hot-pressing operation, the stack may be secured to the stacking platform by means of a clamp in the form of a holding mechanism of the stacking platform. After the single hot-pressing operation, the clamp may be released from the stack, and a second hot-pressing operation may then be performed with the clamp detached from the stack. This second hot-pressing operation may be performed on the stacking platform using pressure applied by the same or different pressing blocks. Alternatively, the stack may be moved to a separate pressing unit, where a second hot-pressing operation may be performed by applying heat and pressure to the stack by a pair of pressing blocks of the pressing unit.
[0114] When the temperature, pressure, and time conditions disclosed herein are not met, the components of the electrode assembly may fail to adhere properly together, which could cause the electrode assembly to fall apart or its components to deviate from their positions within the assembly, especially if the electrode assembly is moved before being inserted into the battery housing. Excessive permeability of the separator may also occur.
[0115] On the other hand, when performing the hot-pressing operation disclosed herein (including meeting the corresponding pressure, temperature, and time conditions), the electrode assembly can be manufactured to bond the components together without individually heating and / or pressing each level of the electrode assembly (i.e., heating and / or pressing each electrode and diaphragm pair at each step of the process). Since the already stacked layers will experience heat and / or pressure in each application, such individual hot-pressing at each level can adversely cause the effects of heat and / or pressure to accumulate in the lower diaphragm of the stack. This can adversely affect this portion of the diaphragm by, for example, reducing porosity (and permeability). In contrast, the present invention allows the entire electrode assembly to bond simultaneously, which in particular improves uniformity. Therefore, it is possible to simultaneously achieve an appropriate level of adhesive force between the electrodes and also achieve a diaphragm with an appropriate amount of permeability while minimizing damage to the unit electrodes.
[0116] In an exemplary embodiment of the present invention, the operation of creating a stack by stacking a first electrode, a diaphragm, and a second electrode on a stacking platform includes: stacking the diaphragm on the stacking platform (S1); stacking the first electrode on the upper surface of the diaphragm (S2); supplying the diaphragm to cover the upper surface of the first electrode while rotating the stacking platform (S3); and stacking the second electrode on the portion of the diaphragm covering the upper surface of the first electrode (S4); and the operations of S1 to S4 can be repeated once or multiple times. By repeating the above operations once or multiple times, the diaphragm is positioned between each of the first and second electrodes in such a way that a Z-shaped fold is possible.
[0117] In an exemplary embodiment of the invention, the stack including at least one of the first electrode and the second electrode and the diaphragm can be held by a holding mechanism, thereby securing it to the stacking stage. The holding mechanism may also be referred to as a clamp.
[0118] In an exemplary embodiment of the invention, the method may further include using a holding mechanism to hold the first electrode or the second electrode, and securing the first electrode or the second electrode to the stacking platform when the first electrode or the second electrode is stacked on the stacking platform. By doing so, it is possible to prevent the electrode from shifting its position within the electrode assembly.
[0119] In this case, when stacked on a stacking table, the retaining mechanism can press and secure the upper surface of the stack (i.e., the upper surface of the first or second electrode or diaphragm stacked on the top side of the stack).
[0120] In an exemplary embodiment of the invention, the operation of supplying the diaphragm to the stack may include continuously supplying (by unwinding) the diaphragm as it passes through the channel of the diaphragm supply unit.
[0121] In an exemplary embodiment of the present invention, the method may further include checking the stacking quality of the first electrode or the second electrode using image information obtained by a camera before stacking the first electrode or the second electrode.
[0122] In an exemplary embodiment of the present invention, an electrode assembly manufactured by the above-described manufacturing method can be provided. The electrode assembly has uniform adhesion and permeability across all layers of the assembly, and the thickness of each electrode is uniform. That is, any deviations in adhesion, permeability, and electrode thickness on the electrode assembly are minimized.
[0123] In an exemplary embodiment of the present invention, an apparatus for manufacturing an electrode assembly using the manufacturing method described above can be provided. Such an apparatus includes: a stacking platform, wherein a first electrode, a diaphragm, and a second electrode are stacked as disclosed herein; a diaphragm supply unit for supplying a diaphragm to the stacking platform; a first electrode supply unit for supplying a first electrode; a second electrode supply unit for supplying a second electrode; a first electrode stacking unit for stacking the first electrode supplied from the first electrode supply unit onto the stacking platform; a second electrode stacking unit for stacking the second electrode supplied from the second electrode supply unit onto the stacking platform; a pressing unit for bonding the first electrode, diaphragm, and second electrode by heating and pressing the stack; and a clamp for clamping the stack to secure it while it is heated and pressed by the pressing unit, wherein the pressing unit performs a first hot-pressing operation by heating and pressing the stack while it is clamped by the clamp, and wherein, while the stack is not clamped by the clamp, the pressing unit performs a second hot-pressing operation by pressing the stack for 5 to 60 seconds at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa.
[0124] In an exemplary embodiment of the invention, the pressing unit may further include a pair of pressing blocks and a pressing heater for heating the pressing blocks, the pair of pressing blocks being configured to move toward each other to heat and press the stacked blocks. The foregoing description can be applied to the pressing blocks and pressing heater constituting the pressing unit in a method of manufacturing an electrode assembly.
[0125] In an exemplary embodiment of the present invention, the first electrode supply unit includes a first electrode placement stage, wherein the first electrode is placed on the first electrode placement stage before being stacked on the stacking stage by the first electrode stacking unit, and the second electrode supply unit may include a second electrode placement stage, wherein the second electrode is placed on the second electrode placement stage before being stacked on the stacking stage by the second electrode stacking unit.
[0126] In addition, the first electrode stacking unit may include a first suction head for picking up a first electrode placed on a first electrode mounting stage using vacuum suction, and the second electrode stacking unit may similarly include a second suction head for picking up a second electrode placed on a second electrode mounting stage using vacuum suction.
[0127] In an exemplary embodiment of the present invention, the first electrode supply unit and the second electrode supply unit may include a heater. Each of the first electrode and the second electrode may be supplied while being heated by the heater.
[0128] More specifically, in an exemplary embodiment of the invention, the first electrode mounting stage may include a heater that can heat the first electrode mounting stage to transfer heat to heat the first electrode.
[0129] Furthermore, in an exemplary embodiment of the present invention, the second electrode mounting stage may include a heater that can heat the second electrode mounting stage in order to transfer heat to heat the second electrode.
[0130] In an exemplary embodiment of the present invention, the first suction head may include a heater to heat the first electrode by using the heater.
[0131] In an exemplary embodiment of the present invention, the second suction head may include a heater to heat the second electrode by using the heater.
[0132] In an exemplary embodiment of the invention, the apparatus for manufacturing electrode assemblies may further include a rotating unit for rotating a stacking stage, wherein a first electrode stacking unit is disposed on one side of the rotating unit and a second electrode stacking unit is disposed on the other side of the rotating unit. In this manner, a Z-shaped fold can be performed by positioning a diaphragm between the first and second electrodes, and by the rotating unit alternately rotating the stacking stage to the side facing a first suction head of the first electrode stacking unit during the first electrode stacking, and then rotating the stacking stage to the side facing a second suction head of the second electrode stacking unit during the second electrode stacking.
[0133] In an exemplary embodiment of the invention, the retaining mechanism may apply some pressure to fix the upper surface of the electrode or diaphragm positioned on the top side of the stack on the stacking platform.
[0134] In this invention, there are no particular limitations on the method for measuring the adhesive force of the diaphragm. In the method further utilized and discussed herein, the lower, middle, and upper portions of the electrode assembly are separated along the stacking direction of the electrode assembly, and a sample is prepared from each of the positive, middle, and negative electrode terminals in the width direction of the electrode assembly. The sample has a width of 55 mm and a length of 20 mm, and each sample may include either a positive electrode and a diaphragm or a negative electrode and a diaphragm. The sample is adhered to a glass slide, while the electrodes are positioned on the adhesion surface of the glass slide.
[0135] More specifically, a glass slide with the sample attached is mounted to an adhesive force measuring device, and the force (in grams per millimeter) is measured per sample width when the diaphragm is peeled from the electrode according to the standard test method described in ASTM-D6862. Specifically, the edge of the diaphragm is pulled upward at a 90° angle relative to the glass slide at a speed of 100 mm / min to peel the diaphragm from the electrode along the width of the sample (i.e., from 0 mm to 55 mm).
[0136] In this invention, there are no particular limitations on the method used to measure the air permeability of the diaphragm. In the method further utilized and discussed herein, the air permeability is measured using a method commonly used in the art, namely, using a Gurley type densitometer (No. 158) manufactured by Toyo Seiki, according to the JIS Gurley measurement method of the Japanese Industrial Standard. That is, the air permeability of the diaphragm is obtained by measuring the time it takes for 100 ml (or 100 cc) of air to pass through a 1 square inch diaphragm at room temperature and a pressure of 0.05 MPa.
[0137] Figure 2 This is a top plan view illustrating an embodiment of an apparatus for manufacturing electrode assemblies according to an exemplary embodiment of the present invention, and Figure 3 This is a conceptual front view illustrating an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention. Here, for convenience, Figure 2 In the middle, the following was omitted. Figure 3 The diaphragm supply unit 120 shown, and in Figure 3 In the middle, the following was omitted. Figure 2 The retaining mechanism 170 is shown, and the pressing unit 180 located on the rear side in the top plan view is shown in dashed lines.
[0138] refer to Figure 2 and Figure 3 An apparatus 100 for manufacturing an electrode assembly according to an exemplary embodiment of the present invention includes a stacking platform 110; a diaphragm supply unit 120 for supplying a diaphragm 14; a first electrode supply unit 130 for supplying a first electrode 11; a second electrode supply unit 140 for supplying a second electrode 12; a first electrode stacking unit 150 for stacking the first electrode 11 on the stacking platform 110; a second electrode stacking unit 160 for stacking the second electrode 12 on the stacking platform 110; and a pressing unit 180 for bonding the first electrode 11, the diaphragm 14, and the second electrode 12 to each other. The pressing unit 180 can be used for the aforementioned primary hot pressing operation and secondary hot pressing operation. Alternatively, after a primary hot pressing operation is completed using the pressing unit 180, a secondary hot pressing operation can be performed by another pressing unit (not shown), which would involve transfer between the pressing units.
[0139] Furthermore, the apparatus 100 for manufacturing an electrode assembly according to an exemplary embodiment of the present invention may further include a holding mechanism 170 for securing the first electrode 11 and the second electrode 12 to the stacking stage 110 when the first electrode 11 and the second electrode 12 are stacked on the stacking stage 110. Additionally, the holding mechanism 170 can secure the stacking of the first electrode 11, the diaphragm 14, and the second electrode 12.
[0140] The following text will refer to Figures 2 to 12An apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention will be described in more detail.
[0141] Figure 4 This is a cross-sectional view showing an electrode assembly manufactured by an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0142] refer to Figures 2 to 4 According to an exemplary embodiment of the present invention, the apparatus 100 for manufacturing an electrode assembly is an apparatus for manufacturing an electrode assembly 10 by stacking a first electrode 11, a diaphragm 14, and a second electrode 12.
[0143] The electrode assembly 10 is a rechargeable / dischargeable power generation element and can be formed in the form of alternating stacking and aggregation of a first electrode 11, a diaphragm 14, and a second electrode 12.
[0144] Here, in the electrode assembly 10, for example, the diaphragm 14 can be folded into a Z-shape, and the first electrode 11 and the second electrode 12 can be alternately disposed between the folded diaphragm 14. In this case, the electrode assembly 10 can be provided in the form where the outermost part is surrounded by the diaphragm 14 (e.g., an electrode assembly 10 assembled by winding the diaphragm together), such as Figure 4 As shown in the image.
[0145] Figure 5 This is a perspective view illustrating a pressing unit in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention, and Figure 6 This is a perspective view illustrating an embodiment of a pressing unit in a device for manufacturing electrode assemblies according to an exemplary embodiment of the present invention, showing a state in which pressing units are stacked. More specifically, Figure 6 The above-mentioned secondary hot pressing operation is shown.
[0146] refer to Figures 4 to 6 The pressing unit 180 presses the stacked first electrode 11, diaphragm 14 and second electrode 12 to combine the first electrode 11, diaphragm 14 and second electrode 12 with each other.
[0147] In addition, the pressing unit 180 includes a pair of pressing blocks 181 and 182, and the pair of pressing blocks 181 and 182 move toward each other to press the stack S including the stacked first electrode 11, the diaphragm 14 and the second electrode 12.
[0148] In this configuration, when the diaphragm 14 surrounds the outer surface of the stack S, the space between the outer portion of the diaphragm 14 positioned along the side of the stack S and the outer-facing portions of the first electrode 11 and the second electrode 12, as well as the outer-facing folds of the diaphragm 14, can be engaged with each other. Therefore, it is possible to more effectively prevent displacement of the first electrode 11 and the second electrode 12 and the diaphragm 14, and / or separation of the stacked components from each other.
[0149] Furthermore, the pressing unit 180 also includes pressing heaters 183 and 184 for heating a pair of pressing blocks 181 and 182, and the pair of pressing blocks 181 and 182 can be heated and pressed against the stack S. Therefore, when the stack S is pressed using the pressing unit 180, thermal fusion between the first electrode 11, the diaphragm 14, and the second electrode 12 is better achieved, resulting in stronger adhesion.
[0150] A pair of pressing blocks 181 and 182 have flat pressing surfaces, and the width and length dimensions of the pressing surfaces may be longer than the width and length dimensions of the facing stack S.
[0151] In addition, the pair of pressing blocks 181 and 182 includes a first pressing block 181 and a second pressing block 182, and the first pressing block 181 and the second pressing block 182 each define a quadrilateral block having a cuboid shape.
[0152] Figure 7 This is a perspective view showing a stacking platform in an apparatus for manufacturing electrode assemblies according to an exemplary embodiment of the present invention.
[0153] refer to Figure 3 and Figure 7 The stacking stage 110 may include: a stage body 111 on which a first electrode 11, a diaphragm 14, and a second electrode 12 are stacked; and a stacking stage heater 112 that heats the stage body 111 to transfer heat to the stacked stacks S.
[0154] The first electrode 11 can be configured as a positive electrode and the second electrode 12 can be configured as a negative electrode, but the present invention is not limited thereto. For example, the first electrode 11 can be configured as a negative electrode and the second electrode 12 can be configured as a positive electrode.
[0155] refer to Figure 3 The diaphragm supply unit 120 can supply the diaphragm 14 to the stacking platform 110.
[0156] The diaphragm supply unit 120 may have a channel through which the diaphragm 14 passes toward the stacking platform 110. Specifically, the diaphragm supply unit 120 may include a diaphragm heating unit 121, which defines the channel through which the diaphragm 14 passes toward the stacking platform 110. Figure 14As shown, the diaphragm heating unit 121 may include a pair of bodies 121a, each of which may be in the form of a square block, and the bodies 121a may be spaced apart by a distance that defines one of the dimensions of the channel through which the diaphragm 14 passes. At least one or both bodies 121a may also include a diaphragm heater 121b for heating the respective body 121a, thereby transferring heat to the diaphragm 14.
[0157] The diaphragm supply unit 120 may also include a diaphragm roller 122 on which the diaphragm 14 is wound. Thus, the diaphragm 14 wound on the diaphragm roller 122 can be gradually unwound and pass through the formed channel to be supplied to the stacking table 110.
[0158] Figure 8 This is a perspective view showing a first electrode mounting stage in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0159] refer to Figure 3 and Figure 8 The first electrode supply unit 130 can supply the first electrode 11 to the first electrode stacking unit 150. In addition, the first electrode supply unit 130 may include a first electrode mounting stage 131, on which the first electrode 11 is mounted before being stacked on the stacking stage 110 by means of the first electrode stacking unit 150.
[0160] The first electrode supply unit 130 may further include: a first electrode roller 133 on which the first electrode 11 is wound in sheet form; a first cutter 134 for cutting the first electrode 11 at regular intervals to form a first electrode 11 of a predetermined size when the first electrode 11 is unwound and supplied from the first electrode roller 133; a first conveyor belt 135 for moving the first electrode 11 cut by the first cutter 134; and a first electrode supply head 136 for picking up (e.g., via vacuum suction) the first electrode 11 transferred by the first conveyor belt 135 and placing the first electrode on the first electrode mounting table 131. Here, the first cutter 134 may cut the sheet-like first electrode 11 in a manner that defines a first electrode connector 11a protruding from its end.
[0161] Figure 9 This is a perspective view showing a second electrode mounting stage in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0162] refer to Figure 3 and Figure 9The second electrode supply unit 140 can supply the second electrode 12 to the second electrode stacking unit 160. In addition, the second electrode supply unit 140 may include a second electrode mounting stage 141, on which the second electrode 12 is mounted before being stacked on the stacking stage 110 by means of the second electrode stacking unit 160.
[0163] The second electrode supply unit 140 may further include: a second electrode roller 143 on which the second electrode 12 is wound in sheet form; a second cutter 144 for cutting the second electrode 12 at regular intervals to form a second electrode 12 of a predetermined size when the second electrode 12 is unwound and supplied from the second electrode roller 143; a second conveyor belt 145 for moving the second electrode 12 cut by the second cutter 144; and a second electrode supply head 146 for picking up (e.g., via vacuum suction) the second electrode 12 transferred by the second conveyor belt 145 and placing the second electrode on the second electrode mounting table 141. Here, the second cutter 144 may cut the sheet-like second electrode 12 in a manner that defines a second electrode connector 12a protruding from its end.
[0164] Figure 10 This is a perspective view illustrating a first suction head in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention, and Figure 11 This is a bottom view showing a first suction head in an apparatus for manufacturing an electrode assembly according to an exemplary embodiment of the present invention.
[0165] refer to Figure 3 , Figure 10 and Figure 11 The first electrode stacking unit 150 can stack the first electrode 11 on the stacking platform 110. The first electrode stacking unit 150 may include a first suction head 151 and a first moving unit 153. The first suction head 151 can pick up the first electrode 11 placed on the first electrode mounting platform 131 via vacuum suction. In this case, the first suction head 151 may be formed with one or more vacuum suction ports 151a formed on the bottom surface 151b of the first suction head 151 to apply suction to the first electrode 11, thereby fixing the first electrode 11 to the bottom surface 151b of the first suction head 151. In the first suction head 151, a channel connecting the vacuum suction port 151a and a device (not shown) for generating vacuum suction may be formed.
[0166] The first moving unit 153 can move the first suction head 151 to the stacking platform 110 to allow the first suction head 151 to stack the first electrode 11 on the stacking platform 110.
[0167] At the same time, refer to Figure 3The second electrode stacking unit 160 can stack the second electrode 12 on the stacking platform 110. The second electrode stacking unit 160 may have the same structure as the aforementioned first electrode stacking unit 150. In this case, the second electrode stacking unit 160 may include a second suction head 161 and a second moving unit 163. The second suction head 161 can pick up the second electrode 12 placed on the second electrode placement stage 141 via vacuum suction. Then, the second moving unit 163 can move the second suction head 161 to the stacking platform 110 to allow the second suction head 161 to stack the second electrode 12 on the stacking platform 110.
[0168] Figure 12 This is a top plan view illustrating the holding mechanism and stacking stage in an apparatus for manufacturing electrode assemblies according to an exemplary embodiment of the present invention.
[0169] refer to Figure 2 and Figure 12 When the first electrode 11 or the second electrode 12 is stacked on the stacking platform 110, the holding mechanism 170 can hold the first electrode 11 or the second electrode 12 and secure it to the stacking platform 110. In doing so, the holding mechanism 170 can apply pressure to the upper surface of the stack S (i.e., the first electrode 11, the second electrode 12, or the diaphragm 14 stacked at the top of the stack S). Specifically, when the first electrode 11 and the second electrode 12 are positioned in the stack S between the layers of the diaphragm 14, the holding mechanism 170 can hold the uppermost surface of the stack by pressing the stack towards the stacking platform 110 to prevent movement of the stack S relative to the stacking platform 110. The holding mechanism 170 may include, for example, a first retainer 171 and a second retainer 172 to secure opposite sides of the first electrode 11 or the second electrode 12. The retainers 171 and 172 may each be in the form of one or more clamps or other clamping mechanisms.
[0170] As the stacking platform 110 rotates, while the holding mechanism 170 maintains its hold on the first electrode 11 or the second electrode 12, the diaphragm 14 can be supplied to the stacking platform 110 simultaneously from the diaphragm roller 122, proportional to the amount of rotation of the stacking platform 110. The holding mechanism 170 and the stacking platform 110 can be connected to or combined with a rotating device (not shown) that enables the rotation of the stacking platform 110. Such a rotating device may include, for example, a spindle or other form of rotating shaft or pivot shaft. Thus, when the holding mechanism 170 holds the first electrode 11 or the second electrode 12, the rotating device can cause the holding mechanism 170 to rotate together with the stacking platform 110.
[0171] The operation of an apparatus 100 for manufacturing electrode assemblies according to an exemplary embodiment of the present invention will be described below.
[0172] refer to Figures 2 to 4 The diaphragm 14, wound on the diaphragm roller 122, is supplied as it passes through a channel formed so that the diaphragm can be stacked on the stacking platform 110.
[0173] In addition, the first electrode 11 is supplied from the first electrode supply unit 130 to the first electrode stacking unit 150, which stacks the first electrode 11 on the upper surface of the diaphragm 14 stacked on the stacking platform 110.
[0174] Then, the holding mechanism 170 presses down on the upper surface of the first electrode 11 to fix the position of the first electrode 11 on the stacking platform 110.
[0175] Subsequently, as the stacking stage 110 rotates in the direction of the second electrode stacking unit 160, the diaphragm 14 is continuously supplied to cover the upper surface of the first electrode 11.
[0176] The second electrode 12 is supplied from the second electrode supply unit 140 and then stacked by the second electrode stacking unit 160 on the portion of the diaphragm 14 that covers the upper surface of the first electrode 11. Then, the holding mechanism 170 releases the upper surface of the first electrode 11 and presses down on the upper surface of the second electrode 12 to fix the position of the stack being constructed relative to the stacking stage 110.
[0177] Subsequently, by repeating the process of stacking the first electrode 11 and the second electrode 12, a stack S can be formed, wherein the diaphragm 14 is zig-folded and positioned between each successive first electrode 11 and second electrode 12.
[0178] Then, the stack S is moved to the pressing unit 180, and the pressing unit 180 heats and presses the stack S, thereby thermally bonding the stacked components (i.e., the heated first electrode 11, diaphragm 14 and second electrode 12) together to manufacture the electrode assembly 10.
[0179] The stack S can be moved to the pressing unit by means of a clamp 51, which is configured to hold the stack on the stacking table 110, and then the stack is moved to the pressing unit 180 for hot pressing. In addition, the pressing unit 180 can be divided into a first pressing unit 50 and a second pressing unit 60, wherein the first pressing unit 50 can be used for a single hot pressing operation (or preheating), and the second pressing unit 60 can be used for a second hot pressing operation.
[0180] refer to Figure 15A and 15B, the first pressing unit 50 can heat and press the stack S simultaneously in a fixed state. The first pressing unit 50 includes a pair of first pressing blocks 50a and 50b, and may also include a clamp 51 configured to fix the stack S. When fixing the stack S, the clamp 51 can hold the stack S by pressing the upper and lower surfaces of the stack S toward each other along the stacking direction (along the y-axis) to fix the relative positions of the first electrode 11, the second electrode 12, and the diaphragm 14. As in the illustrated embodiment, in order to maintain these relative positions, the clamp 51 can press the upper and lower surfaces of the stack S.
[0181] A pair of first pressing blocks 50a and 50b of the first pressing unit 50 can move toward and away from each other. When moving toward each other, the pair of first pressing blocks 50a and 50b can compress one or both of the stack S and the clamp 51.
[0182] In this way, the first pressing unit 50 can heat and compress the stack S to reduce or eliminate any space between the first electrode 11, the diaphragm 14 and the second electrode 12 included in the stack S, thereby bringing these components of the stack S together.
[0183] As shown, each pressing surface of a pair of first pressing blocks 50a and 50b configured to contact and compress the stack S can define a plane. At least one of the pair of first pressing blocks 50a and 50b may include a clamping groove 52 having a shape corresponding to the fixing portion 51b of the clamp 51 further described herein. Figure 15 In the embodiment shown in A, each of the pair of first pressing blocks 50a and 50b includes four clamping slots 52 to correspond to four fixing portions 51b. However, the number of clamping slots 52 may be more or less. Preferably, the number of clamping slots 52 should match the number of fixing portions to be used.
[0184] The clamp 51 may include a body 51a and a plurality of fixing portions 51b. As in the illustrated arrangement, the body 51a may have a length along the x-axis and a height along the y-axis that are the same as or substantially the same as the length and height of the stack S along those corresponding axes. In some other arrangements, the body may be longer than the stack S along the x-axis and taller than the stack S along the y-axis. The fixing portions 51b may preferably be in the form of rods, posts, or plates, extending along the width direction (z-axis) of the stack S. Here, the length of the stack S along the x-axis may refer to the stack portion having the longest distance from one end of the stack S to the other, the height along the y-axis may refer to the distance in the stacking direction of the stack S, and the width along the z-axis may refer to the distance in a direction perpendicular to both the x and y axes.
[0185] The fixing portions 51b can be arranged in two rows, one row adjacent to the pressing surface of the pressing block 50a, and the other row adjacent to the pressing surface of the pressing block 50b. The position of each fixing portion 51b can be adjusted in the height direction of the main body 51a. In this way, each fixing portion 51b can be placed in contact with the upper and lower surfaces of the stack S (preferably along the width of the fixing portion) to fix the position of the stack S and the relative position of the first electrode 11 and the second electrode 12 within the stack S.
[0186] In some arrangements, the second pressing unit 60 can heat and compress the stack S that was previously heated and compressed by the first pressing unit 50, thereby performing a secondary compression of the stack S that has already been compressed once.
[0187] like Figure 15 As shown in Figure B, the second pressing unit 60 includes a pair of second pressing blocks 60a and 60b. These pressing blocks 60a and 60b are movable in directions toward and away from each other. When moving toward each other, these pressing blocks 60a and 60b can press against the upper and lower surfaces of the stack S to compress the stack.
[0188] As shown, each pressing surface of the pair of second pressing blocks 60a and 60b configured to contact and compress the stack S can define a plane. In some arrangements, as shown in the embodiment, slots for securing portion 51b can be excluded from the second pressing blocks 60a and 60b. In other arrangements, at least one of the pair of second pressing blocks 60a and 60b may include one or more slots having a shape corresponding to the securing portion 51b of the clamp 51.
[0189] In some arrangements, each of a pair of first pressing blocks 50a and 50b of the first pressing unit 50 includes a clamping groove 52 having a shape corresponding to the fixing portion 51b of the clamp 51, and each of a pair of second pressing blocks 60a and 60b of the second pressing unit 60 has a flat pressing surface without any clamping groove.
[0190] In some arrangements, the second pressing unit 60 may heat and press only the portion of the stack S where the clamp 51 is located (or previously located), which was not heated and pressed by the first pressing unit 50. In other arrangements, the second pressing unit 60 may heat and press the entire upper and lower surfaces of the stack.
[0191] In some arrangements, the first pressing unit 50 can initially compress the heated stack S while the upper and lower surfaces of the stack S are fixed by clamps 51, in order to reduce or eliminate the space between the first electrode 11, diaphragm 14 and second electrode 12 included in the stack S, while combining the first electrode 11, diaphragm 14 and second electrode 12 so as to combine these components of the stack S together in the area of the stack S without clamps 51.
[0192] In some such arrangements, the second pressing unit 60 can compress and heat the stack S (which has been initially bonded by the first pressing unit 50) and remove the clamp 51 from the stack. Therefore, the second pressing unit 60 can reduce or eliminate any space between the first electrode 11, the diaphragm 14, and the second electrode 12 included in the stack S, to bond these components of the stack S together in a specific area of the stack S, which is the area where the clamp 51 previously pressed the stack S during the initial pressing operation of the first pressing unit 50. In some such arrangements, each of a pair of second pressing blocks 60a and 60b can be a quadrilateral block in the form of a parallelogram. In such arrangements, the pair of second pressing blocks 60a and 60b can have the flat pressing surfaces described earlier herein.
[0193] In some arrangements, each of the pair of first pressing blocks 50a and 50b of the first pressing unit 50 may have a flat pressing surface. In some such arrangements, each of the pair of second pressing blocks 60a and 60b of the second pressing unit 60 may have a groove whose shape corresponds to the shape of the fixing portion 51b of the clamp 51.
[0194] In some arrangements, the fixing portion 51b may include a thermally conductive material, such as a thermally conductive metal material selected from the group consisting of aluminum and iron. By conducting heat to the stack S, the electrodes 11, 12 and the diaphragm 14 can be joined together when the first pressing unit 50 compresses the stack S fixed by the clamp 51, as the space between them is reduced or eliminated.
[0195] In some arrangements, the second pressing unit 60 may not compress the area on the stack S where the previous clamp 51 was located, but only the area on the stack S that was previously without clamps and was not pressed by the first pressing unit 50 during the initial pressing.
[0196] Furthermore, each of the pair of first pressing blocks 50a and 50b can be a quadrangular block in the form of a parallelogram. In such an arrangement, the pair of first pressing blocks 50a and 50b can have the flat pressing surface described earlier herein.
[0197] Either or both of the first pressing unit 50 and the second pressing unit 60 preferably include a pressing heater (not shown) configured to heat each pair of first pressing blocks 50a, 60a and second pressing blocks 50b, 60b so that the blocks can heat the stack S when the stack is pressed. In this way, thermal fusion between the first electrode 11, the diaphragm 14 and the second electrode 12 can be better achieved when the stack S is pressed with the first pressing unit 50 and the second pressing unit 60, thereby forming a stronger bond between these layers.
[0198] In any one or more pairs of the first pressing blocks 50a, 60a and the second pressing blocks 50b, 60b, the length and width of each pressing surface can both be greater than the corresponding length and width of the stack S (on the x-axis and z-axis, respectively).
[0199] The apparatus 100 for manufacturing an electrode assembly according to an exemplary embodiment of the present invention, configured as described above, can ideally prevent the stack S from falling apart or the components of the stack S from shifting their positions within the stack S by thermally bonding the components of the stack S to each other.
[0200] The following will describe an apparatus for manufacturing an electrode assembly according to another embodiment of the invention.
[0201] Figure 13 This is a conceptual front view illustrating an apparatus for manufacturing an electrode assembly according to another exemplary embodiment of the present invention. Figure 13 For convenience, the holding mechanism is omitted, and the pressing unit 180 located at the rear in the top plan view is shown in dashed lines.
[0202] refer to Figure 13 According to another exemplary embodiment of the present invention, an apparatus 200 for manufacturing an electrode assembly includes: a stacking platform 110; a diaphragm supply unit 120 for supplying a diaphragm 14; a first electrode supply unit 130 for supplying a first electrode 11; a second electrode supply unit 140 for supplying a second electrode 12; a first electrode stacking unit 150 for stacking the first electrode 11 on the stacking platform 110; a second electrode stacking unit 160 for stacking the second electrode 12 on the stacking platform 110; a pressing unit 180 for joining the first electrode 11, the diaphragm 14, and the second electrode 12 together; and a holding mechanism 170 for fixing the position of the stack on the stacking platform 110 (see [link to previous description]). Figure 12 ).
[0203] According to another embodiment, the device 200 may also include a rotating unit R for rotating the stacking stage 110 and a vision device 290 for inspecting the first electrode 11 and the second electrode 12.
[0204] Therefore, in this exemplary embodiment, the content that overlaps with the previous embodiment will be briefly described, while the differences from the previous embodiment will be mainly described.
[0205] More specifically, the vision device 290 of the device 200 may include a first camera 291 and a second camera 292. The first camera 291 can capture images of the first electrode 11 mounted on the first electrode mounting stage 131 in the first electrode supply unit 130, and the second camera 292 can capture images of the second electrode 12 mounted on the second electrode mounting stage 141 in the second electrode supply unit 140. Thus, the stacking quality of the first electrode 11 and the second electrode 12 can be inspected using the image information obtained by the first camera 291 and the second camera 292. For example, the placement position, size, and stacking state of the first electrode 11 and the second electrode 12 can be inspected.
[0206] The rotating unit R can rotate the stacking stage 110 in one direction r1 and another direction r2. The first electrode stacking unit 150 can be disposed on one side of the rotating unit R, and the second electrode stacking unit 160 can be disposed on the other side of the rotating unit R. Therefore, the rotating unit R can rotate the stacking stage 110 to one side to face the first suction head 151 when stacking the first electrode 11, and can rotate the stacking stage 110 to the other side to face the second suction head 161 when stacking the second electrode 12. Thus, by alternately rotating the stacking stage 110 between orientations facing the first electrode stacking unit 150 and the second electrode stacking unit 160, it is possible to achieve the desired result. Figure 4 The diagram shows the diaphragm 14 being folded in a Z-shape between each successive electrode in the first electrode 11 and the second electrode 12.
[0207] Unless otherwise stated, the device 200 and all its sub-components in this embodiment operate in the same manner as the device 100 of the aforementioned embodiments. For example, when the first electrode 11 is supplied and placed on the first electrode mounting stage 131 of the first electrode supply unit 130, the stacking quality of the first electrode 11 can be inspected via the vision device 290. Similarly, when the second electrode 12 is supplied and placed on the second electrode mounting stage 141 of the second electrode supply unit 140, the stacking quality of the second electrode 12 can be inspected via the vision device 290.
[0208] In some arrangements of the present invention, the positive electrode can be manufactured by, for example, coating a positive electrode current collector with a positive electrode coating mixture comprising a positive electrode active material, a conductive material, and a binder, and then drying the coating mixture. If necessary, fillers can be added to the mixture. These materials can be any suitable materials used in the relevant art, particularly those commonly used in specific applications.
[0209] For example, positive electrode active materials may include: layered compounds, such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or compounds substituted with one or more transition metals; compounds derived from the chemical formula Li 1+x Mn 2-x Lithium manganese oxides represented by O4 (where x is 0 to 0.33), such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, LiFe3O4, V2O5, and Cu2V2O7; and those derived from the chemical formula LiNi. 1-x M x Nickel (Ni)-position lithium nickel oxides represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, x = 0.01 to 0.3); LiMn 2-x M x Lithium manganese composite oxides represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta, x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); LiMn2O4, wherein a portion of the Li in the chemical formula is replaced by an alkaline earth metal ion; disulfides; and Fe2(MoO4)3, but the invention is not limited to such materials.
[0210] The materials used for the positive electrode current collector are not particularly limited. Preferably, the positive electrode current collector has relatively high conductivity and will not cause chemical changes when used in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or materials whose surfaces are treated with carbon, nickel, titanium, silver, etc., can be used. Preferably, the positive electrode current collector can be aluminum. It is preferable to increase the adhesion between the current collector and the positive electrode coating mixture by including fine irregularities on the surface where the current collector and the coating mixture come into contact. Furthermore, various structural configurations of the positive electrode current collector can be used, such as films, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics. The thickness of the positive electrode current collector can generally range from 3 micrometers to 500 micrometers.
[0211] The amount of conductive material in the positive electrode coating mixture can typically be from 1 wt% to 50 wt% of the total weight of the mixture including the positive electrode active material. There are no particular limitations on the conductive material, but it is preferred to have conductivity that does not cause chemical changes when used in the battery. Examples of conductive materials include graphite, such as natural and artificial graphite; carbon black, such as carbon black, acetylene black, Kirschner black, channel black, furnace black, lamp black, and summer black; conductive fibers, such as carbon fibers and metal fibers; carbon and metal powders, such as fluorinated carbon, aluminum, and nickel powders; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and polystyrene derivatives.
[0212] The binder in the positive electrode coating mixture facilitates the bonding between the active material and the conductive material, and helps adhere the coating mixture to the current collector. Such a binder is generally included in an amount of 1 to 50% by weight of the total weight of the mixture (including the positive electrode active material). Examples of the binder may include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, and various copolymers.
[0213] The filler optionally added to the positive electrode coating mixture can act as a component that suppresses expansion of the positive electrode. Such a filler is not particularly limited, and may include fibrous materials that do not cause chemical changes when used in a battery. For example, olefin polymers (such as polyethylene and polypropylene) as well as fibrous materials (such as glass fibers and carbon fibers) can be used.
[0214] In some arrangements, the negative electrode can be manufactured by coating, drying and pressing a negative electrode active material on a negative electrode current collector, and if necessary, may optionally additionally include the conductive material, binder, filler and the like discussed above. In any case, any appropriate material used in the relevant field may be used, particularly those commonly used for specific applications. For example, as the negative electrode active material, carbon such as non-graphitized carbon and graphitized carbon can also be used; represented by the chemical formula Li x Fe2O3 (0≤x≤1), Li x WO2 (0≤x≤1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups 1, 2 and 3 of the periodic table, and halogens; 0<x≤1; 1≤y≤3; 1≤z≤8); metallic lithium; lithium alloys; silicon-based alloys; tin-based alloys; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; and lithium-cobalt-nickel-based materials.
[0215] The material that can be used for the negative electrode current collector is not particularly limited. The negative electrode current collector preferably has high electrical conductivity and does not cause chemical changes in the battery. For example, copper; stainless steel; aluminum; nickel; titanium; calcined carbon; materials with copper or stainless steel surfaces subjected to surface treatment with carbon, nickel, titanium, silver and the like; and aluminum-cadmium alloys can be used.
[0216] Furthermore, similar to the positive electrode current collector, the bonding between the negative electrode current collector and the negative electrode active material can be strengthened by forming fine irregularities on the surface of the positive electrode current collector. Various structural configurations of the negative electrode current collector can be used, such as membranes, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics. In addition, the thickness of the negative electrode current collector can generally range from 3 micrometers to 500 micrometers.
[0217] In some arrangements, the diaphragm can be an organic / inorganic composite porous SRS (safety-reinforced diaphragm). The SRS may have a structure that includes an inorganic particle and a coating component of a binder polymer coated on a polyolefin-based diaphragm substrate.
[0218] Because SRS does not experience high-temperature thermal shrinkage due to the heat resistance of its inorganic particles, it can maintain the elongated length of the safety diaphragm even if the electrode assembly is penetrated by a needle-shaped conductor.
[0219] In addition to the porous structure of the separator substrate itself, SRS can have a uniform porous structure formed by the interstitial volume between inorganic particles that serve as coating components. The pores not only significantly reduce any external impacts applied to the electrode assembly, but also facilitate the movement of lithium ions through the pores and allow a large amount of electrolyte to be impregnated into the separator, thereby improving battery performance.
[0220] In some arrangements, the diaphragm may be dimensioned with respect to its width dimension (orthogonal to the longitudinal dimension of the diaphragm as it unfolds), such that portions of the diaphragm extend outward on both sides beyond the corresponding edges of the adjacent positive and negative electrodes (hereinafter, "excess portions"). Furthermore, this outwardly extending portion of the diaphragm may have a structure comprising a coating thicker than the diaphragm itself, formed on one or both sides of the diaphragm, to prevent diaphragm shrinkage. For more information regarding the thicker coating of the excess portions of the outwardly extending diaphragm, see Korean Patent Application Publication No. 10-2016-0054219, the entire contents of which are incorporated herein by reference. In some arrangements, the size of each excess portion of the diaphragm may be 5% to 12% of the diaphragm width. Furthermore, in some arrangements, the coating may be applied to both surfaces of the diaphragm, with a coating width of 50% to 90% of the width of each excess portion. Furthermore, the width of the coating on each surface of the diaphragm may be the same or different. In some arrangements, the coating may comprise inorganic particles and a binder polymer as components.
[0221] In an exemplary embodiment of the present invention, examples of membrane components based on polyolefins may include high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene, polypropylene, or derivatives thereof.
[0222] In some arrangements, the coating thickness may be less than the thickness of the first or second electrode. In some such arrangements, the coating thickness may be 30% to 99% of the thickness of the first or second electrode.
[0223] In some arrangements, the coating can be formed by wet or dry coating.
[0224] In some arrangements, the polyolefin-based diaphragm substrate and coating can exist in such a way that the pores on the surfaces of the substrate and coating are anchored to each other, thereby allowing the diaphragm substrate and coating to be firmly bonded together.
[0225] The substrate and coating of the diaphragm can have a thickness ratio of 9:1 to 1:9. A preferred thickness ratio is 5:5.
[0226] In some arrangements, the inorganic particles can be those commonly used in the art. The inorganic particles can interact to form micropores in the form of empty spaces between them, while structurally helping to maintain the physical shape of the coating. Furthermore, since inorganic particles typically possess the property of not altering their physical properties even at temperatures of 200°C or higher, the resulting organic / inorganic composite porous membranes generally preferably exhibit good heat resistance.
[0227] Furthermore, there are no particular limitations on the materials that can be used for inorganic particles, but electrochemical stability is preferred. That is, the inorganic particles are preferably selected such that oxidation and / or reduction reactions do not occur within the operating voltage range of the applied battery (e.g., 0 to 5V based on Li / Li+). In particular, using inorganic particles with ion-transporting capabilities can improve performance by increasing the ionic conductivity in the electrochemical device. Therefore, using inorganic particles with the highest possible ionic conductivity is preferred. Furthermore, when the inorganic particles have a high density, it is difficult to disperse them during the coating process, and it also undesirably increases the weight of the battery. Therefore, using inorganic particles with the lowest possible density is preferred. In addition, inorganic materials with high dielectric constants help to increase the degree of dissociation of electrolyte salts (such as lithium salts) in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte.
[0228] For the reasons mentioned above, inorganic particles can be selected from at least one class of inorganic particles with piezoelectricity and inorganic particles with lithium-ion transport capability.
[0229] The piezoelectric inorganic particles refer to materials that are non-conductors under normal pressure, but exhibit conductive properties due to changes in their internal structure when a certain pressure is applied. They are also materials that show high permittivity characteristics, with a dielectric constant of 100 or higher. When tension or compression is applied to an object composed of the inorganic particles (such as a separator), the piezoelectric inorganic particles can also generate a potential difference between two opposite surfaces of the object by making, for example, one of the two opposite surfaces of the separator positively charged and the other surface negatively charged, or vice versa.
[0230] When the inorganic particles with the above characteristics are used as a coating component, in the case where an internal short circuit occurs between two electrodes due to an external impact (such as impact by a needle-shaped conductor), since the inorganic particles are coated on the separator, the positive electrode and the negative electrode may not be in direct contact with each other. In addition, due to the piezoelectricity of the inorganic particles, a potential difference may appear inside the particles, which can desirably lead to electron migration (i.e., the flow of a tiny current) between the two electrodes, so that the voltage of the battery can be gently reduced, thereby improving safety.
[0231] Examples of the piezoelectric inorganic particle material may be one or more selected from the group consisting of: BaTiO3, Pb(Zr,Ti)O3 (PZT); those represented by the chemical formula Pb 1-x La x Zr 1-y Ti y O3 (PLZT), the substance represented by Pb(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT); and hafnium dioxide (HfO2), but are not limited to these materials.
[0232] The inorganic particles with lithium ion transport capability refer to inorganic particles that contain lithium element but do not store lithium, and have the function of moving lithium ions. The inorganic particles with lithium ion transport capability can transport and move lithium ions due to a certain defect in the particle structure. Therefore, the lithium ion conductivity in the battery can be improved, thereby enhancing the battery performance.
[0233] Examples of the inorganic particle material with lithium ion transport capability may be one or more selected from the group consisting of: lithium phosphate (Li3PO4); lithium titanium phosphate (represented by the chemical formula Li x Ti y (PO4)3, where 0<x<2, 0<y<3); lithium aluminum titanium phosphate (represented by the chemical formula Li x Al y Ti z (PO4)3, where 0<x<2, 0<y<1, 0<z<3); represented by the chemical formula (LiAlTiP) x O ya series of glasses represented by (0<x<4, 0<y<13); lithium titanate (represented by the chemical formula Li x La y TiO3, where 0<x<2, 0<y<3); lithium thiogermanophosphate (represented by the chemical formula Li x Ge y P z S w , where 0<x<4, 0<y<1, 0<z<1, 0<w<5); lithium nitride (represented by the chemical formula Li x N y , where 0<x<4, 0<y<2); SiS2 series glasses (represented by the chemical formula Li x Si y S z , where 0<x<3, 0<y<2, 0<z<4); and P2S5 series glasses (represented by the chemical formula Li x P y S z , where 0<x<3, 0<y<3, 0<z<7), but are not limited to these materials.
[0234] The composition ratio of the inorganic particles and the binder polymer as components of the separator coating is not particularly limited, but can be adjusted in the range of 10:90 to 99:1 (weight percentage), preferably in the range of 80:20 to 99:1 (weight percentage). When the composition ratio is less than 10:90 (weight percentage), the polymer content may become excessively large, and since the voids formed between the inorganic particles are reduced, the pore diameter and porosity may decrease, eventually leading to deterioration of battery performance. On the other hand, when the composition ratio exceeds 99:1 (weight percentage), the polymer content may be too small, and the adhesion between the inorganic materials is weakened, so that the mechanical properties of the final organic / inorganic composite porous separator may deteriorate.
[0235] In some arrangements, binder polymers commonly used in the art can be used as the binder polymer.
[0236] The coating of the organic / inorganic composite porous separator may further include other conventionally known additives in addition to the above-mentioned inorganic particles and binder polymer.
[0237] In some arrangements, the coating may be referred to as an active layer.
[0238] Embodiments of the Invention
[0239] Although the present invention has been described in detail through specific exemplary embodiments, the electrode assembly according to the present invention is not limited thereto. Within the technical spirit of the present invention, those of ordinary skill in the art can make various different implementations.
[0240] 1) Example 1
[0241] Nineteen positive electrode plates, twenty negative electrode plates, and a thin separator are supplied to the stacking stage from the corresponding positive electrode supply unit, negative electrode supply unit, and separator supply unit.
[0242] More specifically, the positive and negative electrodes are supplied after being cut from the positive and negative electrode plates, respectively, and the separator is supplied in the form of an elongated separator sheet. Subsequently, while the stacking stage is rotated and the positive and negative electrodes are stacked as described above, the supplied separator is folded. A holding mechanism is used to press down on the stack on the stacking stage and stabilize the stack, thereby producing a stack comprising 39 electrodes.
[0243] After the stack is manufactured, a hot-pressing operation is performed by heating the stack at a temperature of 70°C and a pressure of 1.91 MPa while clamping and pressing the stack for 15 seconds.
[0244] After a first hot pressing operation, a second hot pressing operation is performed, wherein the pressing block is heated to a temperature of 70°C (temperature condition), and a pressure of 2.71 MPa is applied to the stack with the heated pressing block for 10 seconds (pressing time), thereby producing the electrode assembly of Example 1.
[0245] The above-disclosed content of this invention can be applied in the process of manufacturing electrode assemblies.
[0246] 2) Examples 2 to 12
[0247] The electrode assemblies of Examples 2 to 12 are manufactured in the same manner as those of Example 1, except that the secondary hot pressing operation is performed under the temperature conditions, pressure conditions, and pressing time shown in Table 1 of Example 1 below. That is, the primary hot pressing conditions of Examples 1 to 12 are the same.
[0248] [Table 1]
[0249] 3) Comparative Examples 1 to 7
[0250] The electrode assemblies of Comparative Examples 1 to 7 were manufactured in the same manner as in Example 1, except that the first hot pressing operation was performed under the temperature conditions, pressure conditions, and pressing time shown in Table 2 below, and no second hot pressing operation was performed.
[0251] [Table 2]
[0252] All electrode assemblies of Examples 1 to 12 and Comparative Examples 1 to 5, manufactured under the conditions described in Tables 1 and 2, were tested by picking up each electrode assembly using a vacuum suction mechanism under the same conditions as the electrode supply unit discussed above, with the vacuum suction mechanism attempting to hold the electrode assembly for 60 seconds. In all electrode assemblies of Comparative Examples 1 to 5, it was observed that the electrode and diaphragm separated before 60 seconds. This indicates poor adhesion between the electrode and diaphragm in the electrode assemblies of Comparative Examples 1 to 5, while the electrode assemblies according to this application (which underwent one and two pressing operations) exhibited good adhesion, thus providing an excellent effect in preventing any unfolding and separation of the electrode assembly.
[0253] In Comparative Examples 6 and 7, although no separation of the electrode and diaphragm was observed before 60 seconds, damage to the electrode assembly was confirmed. This was attributed to the initial press being performed under a pressure of 2.54 MPa (i.e., high pressure).
[0254] 4) Experimental Example 1 – Evaluation of Adhesive Strength
[0255] The electrode assemblies of Examples 1 to 12 and Comparative Examples 6 and 7 were disassembled (i.e., their layers were separated) (where no separation of the electrode and separator was observed before 60 seconds in previous tests), and the separated layers were analyzed to measure the adhesive force between the surfaces at the top, bottom, and middle of the stack S. Specifically, the adhesive force between the negative electrode and the separator at the bottom of the stack was measured. Additionally, the adhesive force between the negative electrode and the separator at the top of the stack was measured. Finally, the adhesive force between the negative electrode and the separator at the middle position along the stacking direction was measured.
[0256] In each separate electrode assembly, the sampled negative electrode and diaphragm were 55 mm wide and 20 mm long. The sampled specimen was adhered to a glass slide, with the electrode positioned on the adhesive surface of the slide. The slide containing the specimen was then mounted to an adhesive force measuring device, and a 90° peel test was performed at a speed of 100 mm / min according to the test method specified in ASTM-D6862 discussed above. Ignoring any significant initial fluctuations, the force applied to each sample width (in g / mm) was measured when peeling the diaphragm from the electrode.
[0257] The results are shown in Table 3 below.
[0258] [Table 3]
[0259] In Comparative Examples 6 and 7, as described above, vacuum suction was performed at a pressure of 2.54 MPa, thus confirming that the electrode assembly may have been damaged. Furthermore, referring to the results in Table 3, the deviation in adhesion force was significantly greater than 15 gf / 20 mm. This indicates that the performance of the electrode assembly may be uneven depending on the location.
[0260] On the other hand, in the cases of Examples 1 to 12, it was confirmed that the deviation in adhesive force was less than 15 gf / 20 mm, which was not significant. That is, it was confirmed that the electrode assemblies of Examples 1 to 12 have uniform performance.
[0261] 5) Experiment Example 2 – Evaluation of Air Permeability
[0262] In Examples 1 to 12, the air permeability of the electrode assemblies of Examples 1, 6 and 12 was evaluated, wherein these electrode assemblies differed only in the temperature conditions of the second press.
[0263] Specifically, after collecting the diaphragms from the electrode assemblies of Examples 1, 6, and 12, the diaphragms were cut to prepare diaphragm samples with dimensions of 5 cm × 5 cm (width × length). The diaphragm samples were then washed with acetone.
[0264] According to the JIS Gurley measurement method of Japanese Industrial Standard, the air permeability of Examples 1, 6 and 12 was measured by measuring the time required for 100 ml (or 100 cc) of air to pass through a 1 square inch diaphragm under the conditions of room temperature and 0.05 MPa pressure, using a Gurley type densitometer (No. 158) manufactured by Toyo Seiki.
[0265] The results are shown in Table 4.
[0266] [Table 4]
[0267] As shown in Table 4, when the conditions for the secondary hot-pressing operation according to the present invention are met, it is confirmed that the permeability corresponding to each position is less than 120 seconds / 100 ml, but they have an appropriate permeability level for use as electrode assemblies. Furthermore, it is confirmed that the permeability deviation between each position is also less than 20 seconds / 100 ml, which is considered substantially uniform. That is, it is once again confirmed that the electrode assemblies manufactured by the manufacturing method according to the present invention have uniform performance.
[0268] Note that the air permeability deviation of Example 1 is minimal when the temperature condition is 70°C.
[0269] The above experimental examples confirm that the electrode assembly according to the present invention has appropriate and uniform air permeability and adhesion.
Claims
1. A method for manufacturing an electrode assembly, the method comprising the following steps: Assemble an electrode stack comprising a plurality of electrodes stacked along a stacking axis, with a corresponding diaphragm portion positioned between each electrode; After assembling the electrode stack, a thermo-pressing operation is performed on the electrode stack. The thermo-pressing operation includes engaging the electrode stack with a fixture to fix the position of the electrode stack, and then applying heat and pressure to the electrode stack while the fixture is engaged with the electrode stack. as well as Following the first hot-pressing operation, a second hot-pressing operation is performed on the electrode stack. This second hot-pressing operation involves detaching the clamp from the electrode stack and then applying heat and pressure to the electrode stack. The hot-pressing operation includes applying heat and pressure to the electrode stack for a period of 10 to 20 seconds at a temperature of 65°C to 75°C and a pressure of 1.5 MPa to 2 MPa. The secondary hot-pressing operation includes applying heat and pressure to the electrode stack for a period of 5 to 60 seconds at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa.
2. The method according to claim 1, wherein, The diaphragm portion is part of an elongated diaphragm sheet, and the step of assembling the electrode stack includes alternately stacking a first electrode and a second electrode of the plurality of electrodes on the elongated diaphragm sheet, wherein the elongated diaphragm sheet is sequentially folded over previously stacked electrodes of the first and second electrodes, and then subsequent electrodes of the first and second electrodes are stacked.
3. The method according to claim 2, wherein, The steps for assembling the electrode stack include the following: (1) Position the elongated diaphragm sheet on the stacking platform; (2) One of the first electrodes is stacked on the upper surface of the elongated diaphragm; (3) Rotate the stacking platform while covering the upper surface of one of the first electrodes with the elongated diaphragm; and (4) One of the second electrodes is stacked on the portion of the elongated diaphragm covering the upper surface of the first electrode. Among them, repeat steps (1) to (4) once or more.
4. The method according to claim 3, wherein, The electrode stack is secured to the stacking platform by means of a retaining mechanism.
5. The method of claim 2, further comprising using a camera to inspect the stacking of the first electrodes and / or using a camera to inspect the stacking of the second electrodes.
6. The method according to claim 1, wherein, The step of applying pressure to the electrode stack in both the primary hot pressing operation and the secondary hot pressing operation includes: The pressing block is advanced along the stack axis and engages with the electrode stack.
7. The method according to claim 6, wherein, The pressing block is heated to transfer heat to the electrode stack.
8. The method according to claim 1, wherein, The step of assembling the electrode stack includes winding an elongated diaphragm around the outer periphery of the electrode stack.
9. The method according to claim 1, further comprising the following steps: Prior to the step of assembling the electrode stack, at least one of the electrodes and the diaphragm portion is heated.
10. An apparatus for manufacturing an electrode assembly, the electrode assembly comprising an electrode stack having a plurality of first electrodes and second electrodes stacked along a stack axis, wherein a corresponding diaphragm portion is positioned between each of the first electrodes and the second electrodes, the apparatus comprising: A pressing unit is used to bond the electrodes and the diaphragm portion within the electrode stack together by applying heat and pressure to the electrode stack; as well as A clamp for engaging the electrode stack to fix its position when heat and pressure are applied to it by the pressing unit. The clamp and the pressing unit are configured such that when the clamp engages with the electrode stack, the pressing unit applies heat and pressure to the electrode stack at a temperature of 65°C to 75°C and a pressure of 1.5 MPa to 2 MPa for a period of 10 to 20 seconds; and when the clamp disengages from the electrode stack, the pressing unit applies heat and pressure to the electrode stack at a temperature of 50°C to 90°C and a pressure of 1 MPa to 6 MPa for a period of 5 to 60 seconds.
11. The device according to claim 10, further comprising: A stacking platform for supporting the electrode stack; A diaphragm supply unit for supplying an elongated diaphragm sheet to the stacking platform, wherein the diaphragm portion is a part of the elongated diaphragm sheet; A first electrode supply unit is configured to supply the first electrode to the stacking platform; A second electrode supply unit is used to supply the second electrode to the stacking platform; A first electrode stacking unit, configured to move a first electrode supplied from a first electrode supply unit to the stacking platform; and A second electrode stacking unit is used to move the second electrode supplied from the second electrode supply unit to the stacking platform.
12. The device according to claim 11, wherein, The first electrode supply unit includes a first electrode placement stage, on which the first electrode is placed before being stacked by means of the first electrode stacking unit. The second electrode supply unit includes a second electrode mounting platform, on which the second electrode is mounted before being stacked by means of the second electrode stacking unit.
13. The device according to claim 11, wherein, The first electrode stack unit includes a first suction head for picking up the first electrode by vacuum suction, and The second electrode stack unit includes a second suction head for picking up the second electrode by vacuum suction.
14. The device according to claim 11, further comprising: A rotating unit is configured to rotate the stacking platform between a first position and a second position, the first position being toward the first electrode stacking unit for receiving the first electrode from the first electrode stacking unit, and the second position being toward the second electrode stacking unit for receiving the second electrode from the second electrode stacking unit.
15. The device according to claim 10, wherein, The clamp is configured to apply downward pressure along the stack axis to the upper surface of the electrode stack in order to fix the position of the electrode stack relative to the pressing unit.
16. The device according to claim 10, wherein, The pressing unit further includes a pressing block and a pressing heater for heating the pressing block, and The pressing block is configured to advance along the stack axis of the electrode stack to apply heat and pressure to the electrode stack.
17. The device according to claim 10, wherein, The clamp includes a main body and multiple fixing parts. The pressing unit includes a first pressing unit for a single hot pressing operation and a second pressing unit for a secondary hot pressing operation, and The first pressing unit includes a pressing block having a clamping groove whose shape corresponds to the fixing portion of the clamp.
Citation Information
Patent Citations
Electrode assembly with SRS coated separator
KR1020160054219A
Optical Imaging System
KR1020210090592A
Measuring unit for measuring the forwarding of a workpiece in a bending machine
KR1020210090596A
A magazine-shaped apparatus for supplying powder papers and system for managing medication using the same
KR1020210090597A
Beverage compositioin
KR1020210090598A