High-temperature-resistant and easy-to-collapse precoated sand for casting and preparation method thereof
By combining modified silica sand and high-temperature resistant resin, a high-temperature resistant ceramic phase is formed, which solves the problem of easy cracking and fracture of coated sand at high temperatures, and achieves stability and quality assurance of castings at high temperatures.
Patent Information
- Application Number
- CN202310874028.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-07-17
AI Technical Summary
Existing coated sand is prone to cracking, fracture, deformation and internal stress at high temperatures, resulting in low casting quality and short service life. In particular, it is prone to core penetration when casting special steels, and cannot meet the high-temperature process requirements above 1500℃.
The process involves using modified silica sand, high-temperature resistant resin, glass powder, curing agent, and other components to form a high-temperature resistant coating through spraying and mixing. Combined with composite fibers and carbothermal reduction reaction, a high-temperature resistant ceramic phase is formed, which enhances the high-temperature resistance of the resin and makes it easy to collapse at high temperatures to prevent casting deformation.
It improves the high-temperature resistance of coated sand, extends its service life at high temperatures, reduces the risk of deformation and fracture of castings, ensures casting quality and service life, and prevents casting defects.
Smart Images

Figure BDA0004342180880000111
Abstract
Description
Technical Field
[0001] This invention relates to the field of coated sand processing technology, specifically to a high-temperature resistant, easily collapsible coated sand for casting and its preparation method. Background Technology
[0002] When ordinary coated sand is used as a sand core in the production of cast steel parts and some special cast iron parts (thick-walled, thin-core castings), cracks are often found in the sand core after casting, sometimes even causing the sand core to break and resulting in an orange-peel-like defect on the surface of the casting. This is because after the sand core comes into contact with the high-temperature molten metal, the benzoxazine resin carbonizes, burns, and decomposes at high temperatures, reducing its strength. Meanwhile, the silica sand undergoes a phase transformation and expands significantly, causing the sand core to break under the effect of rapid thermal expansion. When the pouring temperature is too high and the molten iron mass is relatively large, the sand mold may even experience core penetration, causing the casting to be scrapped. In one case, when the sand core is completely surrounded by molten iron, the sand core may soften and deform under the buoyancy of the molten iron, causing changes in the dimensions of the casting and seriously leading to scrapping. Another technical problem that is currently difficult to solve is that during the preparation of coated sand, due to the influence of ambient temperature and the lack of appropriate preheating or cooling, the coated sand castings have large internal stress (i.e., large expansion rate), resulting in low molding quality, easy deformation and breakage, and short service life.
[0003] For example, the invention patent with announcement number CN103521676A discloses a high-temperature resistant, easily collapsible coated sand for casting. The coated sand contains 97-98 parts of raw sand, 2-2.5 parts of phenolic resin, 0.3-0.4 parts of hexamethylenetetramine, 0.15-0.2 parts of calcium stearate, and 0.1-0.3 parts of anhydrous copper sulfate. Although this coated sand also has good high-temperature resistance and can meet the requirements of casting iron processes with pouring temperatures in the range of 800-1400℃, some special steels used in special fields can reach a molten steel temperature of over 1500℃ during casting. Such high-temperature molten steel will cause the conventional high-temperature resistant coated sand to penetrate the core during pouring, thus causing the casting to be scrapped. Summary of the Invention
[0004] To address the problems existing in the prior art, the purpose of this invention is to provide a high-temperature resistant, easily collapsible coated sand for casting and its preparation method.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A high-temperature resistant, easily collapsible coated sand for casting, the coated sand comprising the following components by weight: 800-1000 parts modified silica sand, 30-50 parts high-temperature resistant resin, 10-20 parts clay, 1-3 parts calcium stearate, 1-3 parts anhydrous copper sulfate, 5-8 parts glass powder, and 3-6 parts curing agent.
[0007] The particle size of the glass powder is not less than 10,000 mesh;
[0008] The glass powder is composed of two or more of Na2SiO3, CaSiO3, B2O3 and SiO2.
[0009] The curing agent is a 25-35 wt% aqueous solution of hexamethylenetetramine.
[0010] As a further preferred embodiment of the present invention, the method for preparing the modified silica sand is as follows:
[0011] 1) Add organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water to a mixer in sequence, stir at 100-200 r / min for 1-2 h, and then stir at 350-500 r / min for 30-50 min to form a coating agent.
[0012] 2) Place the silica sand in a sealed container with a stirrer and stir at a high speed of 1000-2000 r / min. Then spray the coating agent into the sealed container. After taking out the product, transfer it to an oven and pre-bake at 80-90℃ for 30-50 min, and then bake at 200-210℃ for 1-2 h to obtain modified silica sand.
[0013] As a further preferred embodiment of the present invention, the mass ratio of organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water in the coating agent is (40-50):(0.5-1.0):(1-3):(12-18):(8-15):(3-7):(15-25):(0.5-1.5):(15-23).
[0014] As a further preferred embodiment of the present invention, the mass ratio of the silica sand to the coating agent is (2-5):1;
[0015] The coating agent is sprayed at a rate of 300-400 mL / min and sprayed continuously for 3-6 minutes.
[0016] As a further preferred embodiment of the present invention, the method for preparing the high-temperature resistant resin is as follows:
[0017] 1) Phenol is preheated and melted at 70-75℃, and then added to a container in sequence with paraformaldehyde and sodium hydroxide. The mixture is stirred evenly at 40-45℃, and then heated to 60-65℃ and reacted for 2-5 hours. After the reaction is completed, the temperature is further increased to 80-85℃ and reacted for 80-120 minutes. The reaction product is then distilled under reduced pressure at 82-87℃ for 10-20 minutes to obtain the prepolymer.
[0018] 2) Add zirconium oxychloride to a container containing methanol. After complete dissolution, add the mixture formed by thoroughly mixing acetylacetone and triethylamine dropwise through a constant pressure dropping funnel under an ice-water bath. After the addition is complete, stir the reaction at room temperature for 6-10 hours. Rotate the reaction product at 50-56℃ until a solid product precipitates. Then add tetrahydrofuran and stir rapidly for 30-50 minutes. After filtration, rotate and concentrate the solution at 50-56℃ to obtain the zirconium source solution.
[0019] 3) Weigh an appropriate amount of prepolymer and place it in a container. Add the composite fiber to the container and mix thoroughly to form a mixture. Then dissolve boric acid in methanol to obtain a boric acid solution. Then, at 32-38℃, add the boric acid solution and zirconium source solution dropwise to the mixture. React at 50-60℃ for 8-12 hours. After rotary evaporation at 50-56℃, a viscous liquid high-temperature resistant resin can be obtained.
[0020] As a further preferred embodiment of the present invention, the mass ratio of phenol, paraformaldehyde, and sodium hydroxide is (95-110):(55-63):(0.4-0.6);
[0021] The ratio of zirconium oxychloride, methanol, acetylacetone, triethylamine, and tetrahydrofuran is (32-36)g:(120-180)mL:(13-15)g:(20-25)g:(250-300)mL;
[0022] The drip rate of the mixture is 1-3 drops / s.
[0023] As a further preferred embodiment of the present invention, the ratio of the amount of the prepolymer, composite fiber, boric acid, methanol, and zirconium source solution is (50-70)g:(3-8)g:(12-16)g:(100-130)mL:(35-50)mL;
[0024] The dropping rate of the boric acid solution and the zirconium source solution is 2-5 drops / s.
[0025] As a further preferred embodiment of the present invention, the method for preparing the composite fiber is as follows:
[0026] Polyacrylonitrile is slowly added to N,N-dimethylformamide and stirred at room temperature for 12-15 hours. Then cobalt acetate is added and mixed evenly to form a spinning solution, which is then injected into a syringe. During electrospinning, the distance between the injection needle and the current collector is maintained at 12-16 cm, and the voltage is set at 12-15 kV. The resulting fiber is vacuum dried overnight at 60-70°C, and then heated to 700-750°C and held at that temperature for 2-5 hours under an argon atmosphere to obtain the desired composite fiber.
[0027] As a further preferred embodiment of the present invention, the ratio of polyacrylonitrile, N,N-dimethylformamide and cobalt acetate is (1-3)g:(10-20)mL:(1-3)g;
[0028] The heating rate is controlled at 1-3℃ / min.
[0029] A method for preparing high-temperature resistant, easily collapsible coated sand for casting, the specific operation steps are as follows:
[0030] Weigh each component according to the required weight proportions, preheat the modified silica sand to 145-160℃, add it to the sand mixer, add high-temperature resistant resin to the sand mixer and coat it fully, then add clay and glass powder, mix thoroughly, add curing agent, and after the moisture has evaporated, add calcium stearate and anhydrous copper sulfate, mix thoroughly, and after cooling, sieving, inspection and packaging, the required high-temperature resistant and easily collapsible coated sand can be obtained.
[0031] Compared with the prior art, the beneficial effects of the present invention are:
[0032] In this invention, organosilicon oligomers are used as high-temperature resistant resins. By selecting suitable functional fillers and additives, a coating agent is formulated and uniformly sprayed onto the surface of silica sand under high-speed stirring to obtain modified silica sand. The high-temperature resistant coating formed on the silica sand surface can withstand temperatures of around 600°C. When used in conjunction with anhydrous copper sulfate, it can decompose and generate gas at temperatures above 600°C, causing a gas impact on the coated sand, which makes the coated sand easily collapse. Moreover, because the high-temperature resistant coating has a very high temperature resistance, it will not collapse during casting, thus preventing the phenomenon of casting deformation or even scrap during the casting process, which helps to improve the quality of castings.
[0033] In this invention, phenol and paraformaldehyde are used as raw materials to synthesize a prepolymer under sodium hydroxide catalysis. Then, zirconium source solution is synthesized using zirconium oxychloride, acetylacetone, and triethylamine as raw materials. The prepolymer, boric acid, zirconium source solution, and prepared composite fibers are then reacted in a specific ratio to obtain a high-temperature resistant resin. This high-temperature resistant resin decomposes at high temperatures to form zirconium oxide and boron oxide crystals, which undergo carbothermic reduction with carbon in the system to form a zirconium boride ceramic phase. This significantly improves the high-temperature resistance of the resin. Furthermore, at high temperatures, the zirconium and boron sources contained in the high-temperature resistant resin decompose to form zirconium oxide and boron oxide, respectively, which cover the resin surface. The glassy oxide layer formed on the surface acts as a barrier between the resin interior and the external environment, providing excellent protection for the internal structure of the resin and effectively covering the internal atmosphere. The pores generated during the volatilization of the resin play a certain role in modifying the resin structure, allowing the high-temperature resistant resin to maintain its structural integrity for a long time at high temperatures. This results in the coated sand having a long heat resistance time and strong high-temperature resistance. At the same time, the introduction of composite fibers into the resin system—which are formed by electrospinning and high-temperature treatment with polyacrylonitrile as the carbon source and the addition of cobalt acetate—creates a fiber structure with a large number of nano-cobalt particles deposited on the surface of the carbon fiber matrix. The deposited nanoparticles effectively increase the surface roughness of the carbon fiber and can also fill and repair cracks on the surface of the carbon fiber, thereby improving the strength of the carbon fiber. Utilizing the high thermal conductivity of carbon fiber, the composite fibers can cross-link to form a thermally conductive network, accelerating heat transfer and further improving the high-temperature resistance of the resin material, giving it strong high-temperature resistance.
[0034] The high-temperature resistant and easily collapsible coated sand in this invention has a long heat resistance time at high temperatures, a low expansion rate, high molding quality of cast products, excellent performance, and long service life. In addition, it has little strength loss at high temperatures, good thermal stability, and is easily collapsible, which can effectively prevent casting defects such as sand adhesion, porosity, and veins in castings. Detailed Implementation
[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] In this embodiment of the invention, the glass powder has a particle size of not less than 10,000 mesh and its main components are Na2SiO3, CaSiO3 and SiO2;
[0037] The curing agent is a 30wt% aqueous solution of hexamethylenetetramine.
[0038] Example 1
[0039] A high-temperature resistant, easily collapsible coated sand for casting, comprising the following components by weight: 800 parts modified silica sand, 30 parts high-temperature resistant resin, 10 parts clay, 1 part calcium stearate, 1 part anhydrous copper sulfate, 5 parts glass powder, and 3 parts curing agent.
[0040] The specific steps for preparing this coated sand are as follows:
[0041] Weigh each component according to the required weight proportions, preheat the modified silica sand to 145℃, add it to the sand mixer, add high temperature resistant resin to the sand mixer and coat it fully, then add clay and glass powder, mix thoroughly, add curing agent, and after the moisture has evaporated, add calcium stearate and anhydrous copper sulfate, mix thoroughly, and after cooling, sieving, inspection and packaging, the required high temperature resistant and easily collapsible coated sand can be obtained.
[0042] The preparation method of modified silica sand is as follows:
[0043] 1) According to the mass ratio of 40:0.5:1:12:8:3:15:0.5:15, add organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water into a mixer in sequence, stir at 100 r / min for 1 h, and then stir at 350 r / min for 30 min to form a coating agent;
[0044] 2) Place the silica sand in a sealed container with a stirrer at a mass ratio of 2:1 and stir at a high speed of 1000 r / min. Then spray the coating agent into the sealed container and control the spraying speed of the coating agent to be 300 mL / min. Continue spraying for 3 min. After that, take out the product and transfer it to an oven. Pre-bake at 80℃ for 30 min and then bake at 200℃ for 1 h to obtain the modified silica sand.
[0045] The preparation method of the high-temperature resistant resin is as follows:
[0046] 1) Slowly add 1g of polyacrylonitrile to 10mL of N,N-dimethylformamide and stir at room temperature for 12h. Then add 1g of cobalt acetate and mix evenly to form a spinning solution. Then inject it into a syringe. During the electrospinning process, the distance between the injection needle and the current collector is kept at 12cm and the voltage is set at 12kV. The formed fiber is vacuum dried at 60℃ overnight. Then, under an argon atmosphere, it is heated to 700℃ at a rate of 1℃ / min and kept at that temperature for 2h to obtain the desired composite fiber.
[0047] 2) After preheating and melting 95g of phenol at 70℃, add it to a container in sequence with 55g of paraformaldehyde and 0.4g of sodium hydroxide. Mix them evenly at 40℃, then raise the temperature to 60℃ and react for 2 hours. After the reaction is completed, continue to raise the temperature to 80℃ and react for 80 minutes. Distill the reaction product under reduced pressure at 82℃ for 10 minutes to obtain the prepolymer.
[0048] 3) Add 32g of zirconium oxychloride to a container containing 120mL of methanol. After complete dissolution, add a mixture of 13g of acetylacetone and 20g of triethylamine to the container dropwise through a constant pressure dropping funnel under an ice-water bath. Control the dropping rate to 1 drop / s. After the addition is complete, stir the mixture at 50r / min at room temperature for 6h. Rotate the reaction product at 50℃ until a solid product precipitates. Then add 250mL of tetrahydrofuran and stir rapidly for 30min. After filtration, rotate the mixture at 50℃ and concentrate it to obtain the zirconium source solution.
[0049] 4) Weigh 50g of prepolymer and place it in a container. Add 3g of composite fiber to the container and mix thoroughly to form a mixture. Then, dissolve 12g of boric acid in 100mL of methanol to obtain a boric acid solution. Then, at 32℃, add the boric acid solution and 35mL of zirconium source solution dropwise to the mixture at a rate of 2 drops / s. React at 50℃ for 8 hours. After rotary evaporation at 50℃, a viscous liquid high-temperature resistant resin can be obtained.
[0050] Example 2
[0051] A high-temperature resistant, easily collapsible coated sand for casting, comprising the following components by weight: 900 parts modified silica sand, 40 parts high-temperature resistant resin, 15 parts clay, 2 parts calcium stearate, 2 parts anhydrous copper sulfate, 7 parts glass powder, and 5 parts curing agent.
[0052] The specific steps for preparing this coated sand are as follows:
[0053] Weigh each component according to the required weight proportions, preheat the modified silica sand to 155℃, add it to the sand mixer, add high temperature resistant resin to the sand mixer and coat it fully, then add clay and glass powder, mix thoroughly, add curing agent, and after the moisture has evaporated, add calcium stearate and anhydrous copper sulfate, mix thoroughly, and after cooling, sieving, inspection and packaging, the required high temperature resistant and easily collapsible coated sand can be obtained.
[0054] The preparation method of modified silica sand is as follows:
[0055] 1) According to the mass ratio of 45:0.8:2:15:13:5:20:1:20, add organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water into a mixer in sequence, stir at 150 r / min for 1.5 h, and then stir at 450 r / min for 40 min to form a coating agent;
[0056] 2) Place the silica sand in a sealed container with a stirrer at a mass ratio of 3:1 and stir at a high speed of 1500 r / min. Then spray the coating agent into the sealed container and control the spraying speed of the coating agent to be 350 mL / min. Continue spraying for 5 min. After that, take out the product and transfer it to an oven. Pre-bake at 85℃ for 40 min and then bake at 205℃ for 1.5 h to obtain the modified silica sand.
[0057] The preparation method of the high-temperature resistant resin is as follows:
[0058] 1) Slowly add 2g of polyacrylonitrile to 15mL of N,N-dimethylformamide and stir at room temperature for 13h. Then add 2g of cobalt acetate and mix evenly to form a spinning solution. Then inject it into a syringe. During the electrospinning process, the distance between the injection needle and the current collector is kept at 15cm and the voltage is set at 13kV. The formed fiber is vacuum dried at 65℃ overnight. Then, under an argon atmosphere, it is heated to 730℃ at a rate of 2℃ / min and kept at that temperature for 3h to obtain the desired composite fiber.
[0059] 2) After preheating and melting 105g of phenol at 72℃, add it to a container in sequence with 60g of paraformaldehyde and 0.5g of sodium hydroxide. Mix them evenly at 42℃, then raise the temperature to 62℃ and react for 3h. After the reaction is completed, continue to raise the temperature to 82℃ and react for 100min. Distill the reaction product under reduced pressure at 85℃ for 15min to obtain the prepolymer.
[0060] 3) Add 35g of zirconium oxychloride to a container containing 160mL of methanol. After complete dissolution, add a mixture of 14g of acetylacetone and 23g of triethylamine to the container dropwise through a constant pressure dropping funnel under an ice-water bath. Control the dropping rate at 2 drops / s. After the addition is complete, stir the mixture at 70r / min at room temperature for 8h. Rotate the reaction product at 53℃ until a solid product precipitates. Then add 280mL of tetrahydrofuran and stir rapidly for 40min. After filtration, rotate the mixture at 52℃ and concentrate it to obtain the zirconium source solution.
[0061] 4) Weigh 60g of prepolymer and place it in a container. Add 5g of composite fiber to the container and mix thoroughly to form a mixture. Then, dissolve 15g of boric acid in 120mL of methanol to obtain a boric acid solution. Then, at 35℃, add the boric acid solution and 42mL of zirconium source solution dropwise to the mixture at a rate of 3 drops / s. React at 55℃ for 10h. After rotary evaporation at 53℃, a viscous liquid high-temperature resistant resin can be obtained.
[0062] Example 3
[0063] A high-temperature resistant, easily collapsible coated sand for casting, comprising the following components by weight: 1000 parts modified silica sand, 50 parts high-temperature resistant resin, 20 parts clay, 3 parts calcium stearate, 3 parts anhydrous copper sulfate, 8 parts glass powder, and 6 parts curing agent.
[0064] The specific steps for preparing this coated sand are as follows:
[0065] Weigh each component according to the required weight proportions, preheat the modified silica sand to 160℃, add it to the sand mixer, add high temperature resistant resin to the sand mixer and coat it fully, then add clay and glass powder, mix thoroughly, add curing agent, and after the moisture has evaporated, add calcium stearate and anhydrous copper sulfate, mix thoroughly, and after cooling, sieving, inspection and packaging, the required high temperature resistant and easily collapsible coated sand can be obtained.
[0066] The preparation method of modified silica sand is as follows:
[0067] 1) According to the mass ratio of 50:1:3:18:15:7:25:1.5:23, add organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water into a mixer in sequence, stir at 200 r / min for 2 h, and then stir at 500 r / min for 50 min to form a coating agent;
[0068] 2) Place the silica sand in a sealed container with a stirrer at a mass ratio of 5:1 and stir at a high speed of 2000 r / min. Then spray the coating agent into the sealed container and control the spraying speed of the coating agent to 400 mL / min. Continue spraying for 6 min. After that, take out the product and transfer it to an oven. Pre-bake at 90℃ for 50 min and then bake at 210℃ for 2 h to obtain the modified silica sand.
[0069] The preparation method of the high-temperature resistant resin is as follows:
[0070] 1) Slowly add 3g of polyacrylonitrile to 20mL of N,N-dimethylformamide and stir at room temperature for 15h. Then add 3g of cobalt acetate and mix evenly to form a spinning solution. Then inject it into a syringe. During the electrospinning process, the distance between the injection needle and the current collector is kept at 16cm and the voltage is set at 15kV. The formed fiber is vacuum dried at 70℃ overnight. Then, under an argon atmosphere, it is heated to 750℃ at a rate of 3℃ / min and kept at that temperature for 5h to obtain the desired composite fiber.
[0071] 2) After preheating and melting 110g of phenol at 75℃, add it to a container in sequence with 63g of paraformaldehyde and 0.6g of sodium hydroxide. Mix them evenly at 45℃, then raise the temperature to 65℃ and react for 5h. After the reaction is completed, continue to raise the temperature to 85℃ and react for 120min. Distill the reaction product under reduced pressure at 87℃ for 20min to obtain the prepolymer.
[0072] 3) Add 36g of zirconium oxychloride to a container containing 180mL of methanol. After complete dissolution, add a mixture of 15g of acetylacetone and 25g of triethylamine to the container dropwise through a constant pressure dropping funnel under an ice-water bath. Control the dropping rate at 3 drops / s. After the addition is complete, stir the reaction at 80r / min at room temperature for 10h. Rotate the reaction product at 56℃ until a solid product precipitates. Then add 300mL of tetrahydrofuran and stir rapidly for 50min. After filtration, rotate the solution at 56℃ and concentrate to obtain the zirconium source solution.
[0073] 4) Weigh 70g of prepolymer and place it in a container. Add 8g of composite fiber to the container and mix thoroughly to form a mixture. Then, dissolve 16g of boric acid in 130mL of methanol to obtain a boric acid solution. Then, at 38℃, add the boric acid solution and 50mL of zirconium source solution dropwise to the mixture at a rate of 5 drops / s. React at 60℃ for 12h. After rotary evaporation at 56℃, a viscous liquid high-temperature resistant resin can be obtained.
[0074] Comparative Example 1: This comparative example is basically the same as Example 1, except that ordinary silica sand is used instead of modified silica sand.
[0075] Comparative Example 2: This comparative example is basically the same as Example 1, except that ordinary phenolic resin is used instead of high-temperature resistant resin.
[0076] Comparative Example 3: This comparative example is basically the same as Example 1, except that it does not contain high-temperature resistant resin.
[0077] Comparative Example 4: This comparative example is basically the same as Example 1, except that the high-temperature resistant resin does not contain composite fibers in its preparation.
[0078] Comparative Example 5: This comparative example is basically the same as Example 1, except that carbon fiber is used instead of composite fiber in the preparation of the high temperature resistant resin.
[0079] Test experiment:
[0080] The residual tensile strength at 700℃ was used to characterize low-temperature collapse resistance. The specific method was as follows: eight figure-eight shaped test blocks of tensile strength were prepared according to the national standard GB / T8583-2008, and then fired in a high-temperature furnace for 2 minutes at 700℃. After cooling to room temperature, the residual tensile strength was measured. A higher residual tensile strength indicated poorer low-temperature collapse resistance, while a lower residual strength indicated better low-temperature collapse resistance. In addition, the high-temperature resistance time and high-temperature deformation of the coated sand at 1500℃ were tested using an SHH-type resin sand high-temperature performance testing machine. The test results are shown in Table 1.
[0081] Table 1
[0082]
[0083] As shown in Table 1, the coated sand in this invention has high collapsibility and high temperature resistance, which can effectively prevent casting defects such as sand adhesion, porosity, and vein patterns, and help improve the quality of castings.
[0084] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high-temperature resistant, easily collapsible coated sand for casting, characterized in that, The coated sand comprises the following components by weight: 800-1000 parts modified silica sand, 30-50 parts high-temperature resistant resin, 10-20 parts clay, 1-3 parts calcium stearate, 1-3 parts anhydrous copper sulfate, 5-8 parts glass powder, and 3-6 parts curing agent. The particle size of the glass powder is not less than 10,000 mesh; The glass powder is composed of two or more of Na2SiO3, CaSiO3, B2O3 and SiO2. The curing agent is a 25-35 wt% aqueous solution of hexamethylenetetramine; The modified silica sand is prepared as follows: 1) Add organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water to a mixer in sequence, stir at 100-200 r / min for 1-2 h, and then stir at 350-500 r / min for 30-50 min to form a coating agent. 2) Place the silica sand in a sealed container with a stirrer and stir at a high speed of 1000-2000 r / min. Then spray the coating agent into the sealed container. After taking out the product, transfer it to an oven and pre-bake at 80-90℃ for 30-50 min, and then bake at 200-210℃ for 1-2 h to obtain modified silica sand. The preparation method of the high-temperature resistant resin is as follows: 1) Phenol is preheated and melted at 70-75℃, and then added to a container in sequence with paraformaldehyde and sodium hydroxide. The mixture is stirred evenly at 40-45℃, and then heated to 60-65℃ and reacted for 2-5 hours. After the reaction is completed, the temperature is further increased to 80-85℃ and reacted for 80-120 minutes. The reaction product is then distilled under reduced pressure at 82-87℃ for 10-20 minutes to obtain the prepolymer. 2) Zirconium oxychloride was added to a container containing methanol. After complete dissolution, a mixture of acetylacetone and triethylamine was added dropwise to the container through a constant pressure dropping funnel under an ice-water bath. After the addition was complete, the mixture was stirred at room temperature for 6-10 hours. The reaction product was then rotary evaporated at 50-56°C until a solid product precipitated. Tetrahydrofuran was then added and stirred rapidly for 30-50 minutes. After filtration, the product was rotary evaporated and concentrated at 50-56°C to obtain a zirconium source solution. 3) Weigh an appropriate amount of prepolymer and place it in a container. Add the composite fiber to the container and mix thoroughly to form a mixture. Then dissolve boric acid in the second methanol to obtain a boric acid solution. Then, at 32-38℃, add the boric acid solution and zirconium source solution dropwise to the mixture. React at 50-60℃ for 8-12 hours. After rotary evaporation at 50-56℃, a viscous liquid high-temperature resistant resin can be obtained. The method for preparing the composite fiber is as follows: Polyacrylonitrile is slowly added to N,N-dimethylformamide and stirred at room temperature for 12-15 hours. Then cobalt acetate is added and mixed evenly to form a spinning solution, which is then injected into a syringe. During electrospinning, the distance between the injection needle and the current collector is maintained at 12-16 cm, and the voltage is set at 12-15 kV. The resulting fiber is vacuum dried overnight at 60-70°C, and then heated to 700-750°C and held at that temperature for 2-5 hours under an argon atmosphere to obtain the desired composite fiber.
2. The high-temperature resistant, easily collapsible coated sand for casting according to claim 1, characterized in that, In the coating agent, the mass ratio of organosilicon oligomer, dispersant, anti-settling agent, aluminum powder, silica powder, mica powder, xylene, accelerator and water is (40-50): (0.5-1.0): (1-3): (12-18): (8-15): (3-7): (15-25): (0.5-1.5): (15-23).
3. The high-temperature resistant, easily collapsible coated sand for casting according to claim 1, characterized in that, The mass ratio of the silica sand to the coating agent is (2-5):1; The coating agent is sprayed at a rate of 300-400 mL / min and sprayed continuously for 3-6 minutes.
4. The high-temperature resistant, easily collapsible coated sand for casting according to claim 1, characterized in that, The mass ratio of phenol, paraformaldehyde, and sodium hydroxide is (95-110):(55-63):(0.4-0.6). The ratio of zirconium oxychloride, first methanol, acetylacetone, triethylamine, and tetrahydrofuran is (32-36) g: (120-180) mL: (13-15) g: (20-25) g: (250-300) mL; The drip rate of the mixture is 1-3 drops / s.
5. The high-temperature resistant, easily collapsible coated sand for casting according to claim 1, characterized in that, The ratio of the amount of prepolymer, composite fiber, boric acid, second methanol, and zirconium source solution is (50-70) g: (3-8) g: (12-16) g: (100-130) mL: (35-50) mL; The dropping rate of the boric acid solution and the zirconium source solution is 2-5 drops / s.
6. The high-temperature resistant, easily collapsible coated sand for casting according to claim 1, characterized in that, The ratio of polyacrylonitrile, N,N-dimethylformamide, and cobalt acetate is (1-3) g: (10-20) mL: (1-3) g; The heating rate is controlled at 1-3℃ / min.
7. A method for preparing high-temperature resistant, easily collapsible coated sand for casting according to any one of claims 1-6, characterized in that, The specific steps are as follows: Weigh each component according to the required weight proportions, preheat the modified silica sand to 145-160℃, add it to the sand mixer, add high-temperature resistant resin to the sand mixer and coat it fully, then add clay and glass powder, mix thoroughly, add curing agent, and after the moisture has evaporated, add calcium stearate and anhydrous copper sulfate, mix thoroughly, and after cooling, sieving, inspection and packaging, the required high-temperature resistant and easily collapsible coated sand can be obtained.
Citation Information
Patent Citations
High-temperature-resistant easy-collapsibility precoated sand for casting
CN103521676A
Super-high-temperature-resistant precoated sand
CN112692225A