Cu-ti-based copper alloy sheet, method for producing the same, power feeding member, and heat dissipating member

By controlling the formation of grain boundary reaction precipitates in Cu-Ti copper alloy plates through two solution treatments and intermediate cold rolling processes, the problem of density reduction in existing technologies is solved, achieving a balance between strength, conductivity and bending workability, with the density reduced to below 8.53 g/cm³.

CN116891960BActive Publication Date: 2026-11-20DOWA METALTECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211512057.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-08-01
Filing Date
2022-11-29
Publication Date
2026-11-20
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively reduce the density of Cu-Ti copper alloys while maintaining their strength, electrical conductivity, and good bending workability.

Method used

By employing a two-stage solution treatment and intermediate cold rolling process to control the formation of grain boundary reactive precipitates, and by adjusting the alloy composition and manufacturing process, Cu-Ti copper alloy plates with appropriate lattice strain are prepared.

Benefits of technology

A high level of balance was achieved in Cu-Ti copper alloy plates, which have excellent strength, conductivity, bending workability and stress relaxation characteristics, while the density was reduced to below 8.53 g/cm³.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116891960B_ABST
    Figure CN116891960B_ABST
Patent Text Reader

Abstract

This invention relates to Cu-Ti copper alloy sheets, their manufacturing methods, electrical components, and heat dissipation components. It provides Cu-Ti copper alloy sheets that achieve a high level of balanced strength, electrical conductivity, bendability, stress relaxation properties, and reduced density (specific gravity). The copper alloy sheets, by mass%, comprise Ti: 1.0–5.0%, Al: 0.5–3.0%, Ag: 0–0.3%, B: 0–0.3%, Be: 0–0.15%, Co: 0–1.0%, Cr: 0–1.0%, Fe: 0–1.0%, Mg: 0–0.5%, Mn: 0–1.5%, Nb: 0.0–0.5%, Ni: 0–1.0%, P: 0–0.2%, Si: 0–0.5%, Sn... : 0~1.5%, V: 0~1.0%, Zn: 0~2.0%, Zr: 0~1.0%, S: 0~0.2%, rare earth elements: 0~3.0%, balance is essentially composed of Cu, the maximum width of the region where grain boundary reaction precipitates exist is less than 1000nm, the KAM value of the grain boundary is less than 3.0°, which is defined as a crystal orientation difference of more than 15° based on EBSD measurement (step size 0.1μm), and the tensile strength in the rolling direction is more than 850MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to Cu-Ti copper alloy plates with reduced density (specific gravity), methods for manufacturing the same, and the use of the plates as electrically conductive components of materials. Background Technology

[0002] Cu-Ti copper alloys (titanium copper) boast high strength and excellent stress relaxation resistance among various copper alloys, making them widely used in connectors, relays, switches, and other electrical components, as well as spring components. In recent years, with the increasing functionality of portable terminals such as smartphones and automotive electronic devices, the demand for lightweight components has been rising. To meet this requirement, achieving lightweighting while maintaining the inherent good properties of copper alloys used in electrical components has become crucial.

[0003] Patent document 1 discloses the following technology: In Cu-Ti copper alloys, by combining a pre-aging treatment (pre-treatment) with an aging treatment in a lower temperature range, the formation of grain boundary reaction precipitates is suppressed, thereby improving strength, bending workability, stress relaxation resistance, and fatigue resistance.

[0004] Patent document 2 discloses the following technology: In Cu-Ti copper alloys, by adjusting the combination of hot rolling to obtain a reduction rate in a high temperature region, solution treatment at a relatively high temperature, and aging treatment controlled near the temperature at which the maximum hardness is obtained, to a specified microstructure, the bending workability after notching is improved.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-185370

[0008] Patent Document 2: Japanese Patent Application Publication No. 2010-126777 Summary of the Invention

[0009] The problem that the invention aims to solve

[0010] Based on the technologies disclosed in Patent Documents 1 and 2, Cu-Ti copper alloy sheets with improved desired properties for different applications are currently industrially available. However, an effective method for reducing the density (specific gravity) of the alloy has not yet been established. For example, in the technologies of Patent Documents 1 and 2, it is described that Al, which has a smaller atomic weight than Cu, can be added up to a maximum of 1.0% by mass, but the Al content of the materials shown in the examples is 0.08% (Patent Document 1, Invention Example 6) and 0.14% (Patent Document 2, Example 9). At this level of Al content, the density reduction effect is insufficient. Furthermore, when attempting to manufacture Cu-Ti alloy sheets with, for example, more than 0.5% Al added using the manufacturing process disclosed in Patent Documents 1 and 2, it is difficult to consistently maintain a high level of strength and bending workability.

[0011] The purpose of this invention is to provide Cu-Ti copper alloy plates that possess all the properties of strength, electrical conductivity, bendability, and stress relaxation characteristics (stress mitigation characteristics) in a high-level and balanced manner, while having a reduced density (specific gravity).

[0012] Methods for solving problems

[0013] The inventors conducted detailed research and found that in Cu-Ti copper alloys containing a specified amount of Al, which reduces density (specific gravity), by employing a manufacturing process of performing two "solution treatment + intermediate cold rolling" steps followed by aging treatment, it is possible to obtain a sheet material with a microstructure characterized by less formation of coarse grain boundary reaction precipitates and moderate lattice strain. Thus, despite containing Al, it can impart excellent strength, electrical conductivity, bending workability, and stress relaxation properties.

[0014] To achieve the above objectives, the following invention is disclosed in this specification.

[0015] [1] Copper alloy sheet, having the following composition (by mass%): Ti: 1.0–5.0%, Al: 0.5–3.0%, Ag: 0–0.3%, B: 0–0.3%, Be: 0–0.15%, Co: 0–1.0%, Cr: 0–1.0%, Fe: 0–1.0%, Mg: 0–0.5%, Mn: 0–1.5%, Nb: 0.0–0.5%, Ni: 0–1.0%, P: 0–0.2%, Si: 0–0.5%, Sn: 0–1.5%, V: 0–1.0%, Zn: 0–2.0%, Zr: 0–1.0%, S: 0–0.2%. The total content of Ag, B, Be, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, Si, Sn, V, Zn, Zr and S in the stated elements is less than 3.0%, with the balance consisting of Cu and unavoidable impurities. In the observation plane parallel to the plate surface, the maximum width of the region where grain boundary reaction precipitates exist is less than 1000 nm. In the measurement based on EBSD (electron beam backscatter diffraction) with a step size of 0.1 μm in the observation plane parallel to the plate surface, the KAM value when the boundary with a crystal orientation difference of more than 15° is considered as a grain boundary is less than 3.0°, and the tensile strength in the rolling direction is more than 850 MPa.

[0016] [2] The copper alloy plate according to [1] above also has the following composition: containing rare earth elements in a total of less than 3.0% by mass.

[0017] [3] According to the copper alloy plate described in [1] or [2] above, the number density of fine precipitate particles with a major diameter of 5 to 100 nm in the observation plane parallel to the plate surface is 1.0 × 10⁻⁶. 8 pcs / mm 2 Above and 1.0×10 12 pcs / mm 2 the following.

[0018] [4] The copper alloy plate according to any one of [1] to [3] above, wherein the average grain diameter in the observation plane parallel to the plate surface is 2 to 20 μm using the cutting method according to JIS H0501-1986.

[0019] [5] The copper alloy sheet according to any one of [1] to [4] above, wherein the ratio of the minimum bending radius MBR that does not produce cracks to the sheet thickness t, as determined by the W bending test under BW according to the Japanese Copper Association Technical Standard JCBA T307:2007, is 2.0 or less.

[0020] [6] The copper alloy sheet according to any one of [1] to [5] above, wherein the conductivity is 10.0% IACS or higher.

[0021] [7] The copper alloy sheet according to any one of [1] to [6] above, wherein the density is 8.53 g / cm³. 3 the following.

[0022] [8] The copper alloy plate according to any one of [1] to [7] above, wherein the plate thickness is 0.02 to 0.50 mm.

[0023] [9] The method for manufacturing copper alloy sheet according to any one of [1] to [8] above, wherein, in the process of manufacturing copper alloy sheet by sequentially performing a first solution treatment, a first intermediate cold rolling, a second solution treatment, a second intermediate cold rolling, and an aging treatment on an intermediate product sheet having the composition specified in [1] above,

[0024] The first solution treatment was performed at a temperature range of 750–950°C for 10–600 seconds.

[0025] The first intermediate cold rolling is carried out with a rolling ratio of over 70%.

[0026] The second solution treatment was performed at a temperature range of 750–900°C for 10–600 seconds.

[0027] A second intermediate cold rolling process is performed with a rolling rate of 15-50%.

[0028] Aging treatment is carried out at an aging temperature of 300–470℃.

[0029]

[10] According to the method for manufacturing copper alloy sheet described above [9], the intermediate product sheet further comprises the following composition: containing rare earth elements in a total of less than 3.0% by mass.

[0030]

[11] In the method for manufacturing copper alloy sheet according to [9] or

[10] above, in the process of manufacturing copper alloy sheet by further performing fine cold rolling and low temperature annealing after the aging treatment, fine cold rolling is performed with a rolling rate of less than 50%, and low temperature annealing is performed under the condition of holding at a temperature range of 350 to 550°C for less than 60 seconds.

[0031]

[12] The power-conducting component uses copper alloy sheet material as described in any one of [1] to [8] above.

[0032]

[13] The heat dissipation component uses copper alloy plate as material as described in any one of [1] to [8].

[0033] In this specification, "sheet metal" refers to a sheet of metal material formed using the ductility of metal. Thin sheet metal materials are sometimes also called "foil," and such "foil" is also included in the term "sheet metal" as used herein. Sheet metal materials wound into long strips in the shape of coils are also included in "sheet metal." In this specification, the thickness of sheet metal materials is referred to as "sheet thickness." Additionally, "sheet surface" is the surface perpendicular to the thickness direction of the sheet metal. "Sheet surface" is sometimes also referred to as "rolled surface."

[0034] In this specification, the expression "n1~n2" indicating a numerical range means "n1 or higher and n2 or lower". Here, n1 and n2 are numerical values ​​that satisfy n1 < n2.

[0035] Cu-Ti copper alloys typically exhibit a metallic microstructure with precipitates within the matrix (metal substrate). These precipitates include "grain boundary reaction precipitates" that occur at grain boundaries and "granular precipitates" that occur elsewhere. These precipitates are primarily Cu-Ti intermetallic compounds, but depending on the type and amount of alloying elements added, Ni-Ti, Co-Ti, Fe-Ti, and Cu-Ti-Al intermetallic compounds may also be present. Among the granular precipitates, very fine precipitates can also contribute to increased strength. Here, particles with a major diameter of 5–100 nm are referred to as "fine precipitate particles." Grain boundary reaction precipitates exist at grain boundaries as an aggregate of layered particles. The appearance of the layered particles on the observation surface varies depending on the angle at which the aggregate of layered particles is cut.

[0036] [Method for determining the maximum width of the region where grain boundary reaction precipitates exist]

[0037] In a SEM (scanning electron microscope) image taken on an observation plane parallel to the plate surface, the longest distance from any point on the contour line of a region containing a cluster of adjacent layered particles, sandwiching a layered particle, to the contour line on the opposite side of the grain is defined as the width of that region. Then, the maximum width of the grain boundary reaction precipitate region observed in an observation area (one randomly selected or multiple non-repeating fields of view) containing a total of 10 or more grain boundary reaction precipitate regions is defined as the maximum width of the grain boundary reaction precipitate region of that plate.

[0038] Figures 1-3 The image shows an SEM image of a Cu-Ti copper alloy plate (Comparative Example No. 45 described below) with an observation plane parallel to the plate surface, in which excessive grain boundary reaction precipitates are formed. Figure 3 This is a magnified image of a region containing grain boundary reactive precipitates. Figure 3The outline of the region containing grain boundary reactive precipitates is represented by a dashed line. The distance from point P1 on this outline, sandwiching layered particles, to the outline on the opposite grain side is represented by the length of line segment P1Q1. Point Q1 is the point on the grain side of the outline closest to point P1. Similarly, the distance from point P2 on the outline, sandwiching layered particles, to the outline on the opposite grain side is represented by the length of line segment P2Q2. Point Q2 is the point on the grain side of the outline closest to point P2. The maximum value of this distance, calculated for all points on the outlines sandwiching layered particles, to the outline on the opposite grain side, is the width of the region containing grain boundary reactive precipitates. It should be noted that for the end and near the grain boundary reaction precipitate region where the grains on both sides of the layered particles are directly connected by the grain boundary, the "outline of the opposite grain side" of the outline portion cannot be clearly determined, the "distance from the point on the outline of the opposite grain side" to the outline of the opposite grain side can be regarded as 0 (zero).

[0039] [How to calculate KAM value]

[0040] The surface (rolled surface) of the plate sample to be measured is polished and ground to obtain a smooth observation surface through ion polishing. Within this observation surface, an observation area (e.g., a rectangular area of ​​240 × 180 μm) with a field of view equivalent to 500x magnification is randomly set. Crystal orientation data is acquired by irradiating this observation area with an electron beam at 0.1 μm steps using EBSD (electron beam backscattering diffraction). Based on this data, EBSD data analysis software is used to calculate the KAM (Kernel Average Misorientation) value when the boundary between adjacent measurement points with a crystal orientation difference of 15° or more is considered a grain boundary. Regarding the KAM value, for electron beam irradiation points arranged at 0.1 μm intervals, the crystal orientation difference between all adjacent points is measured (hereinafter referred to as "adjacent point orientation difference"). Only the measured values ​​of adjacent point orientation differences less than 15° are extracted, and their average value is calculated, which is equivalent to the KAM value. In the calculation of the KAM value, bicrystalline boundaries are also considered grain boundaries.

[0041] [Method for determining the number density of fine precipitate particles]

[0042] For the observation surface obtained by electropolishing the plate surface under the following electropolishing conditions followed by ultrasonic cleaning in ethanol for 20 minutes, observation was performed using FE-SEM (field emission scanning electron microscope) at a magnification of 100,000x. Randomly selected observation fields were used where some or all of the particles with a major diameter greater than 1.0 μm were not included in the field of view. For this observation field, the number of precipitate particles with a major diameter of 5–100 nm among the particles whose entire outline was visible was counted. This operation was performed on 10 or more observation fields with non-overlapping regions, and the total count N for all observed fields was recorded. 合计 The value obtained by dividing by the total area of ​​the observed field of view is converted to per 1mm 2 The number of particles is used as the number density of fine precipitate particles (particles / mm²). 2 Here, the "major axis" of a particle is represented by the diameter of the smallest circumcircle enclosing the particle in the image.

[0043] (Electrolytic grinding conditions)

[0044] Electrolyte: Distilled water, phosphoric acid, ethanol, and 2-propanol are mixed in a volume ratio of 10:5:5:1.

[0045] ·Liquid temperature: 20℃

[0046] Voltage: 15V

[0047] Electrolysis time: 20 seconds

[0048] Invention Effects

[0049] According to the present invention, in Cu-Ti copper alloy sheets that possess all the properties of strength, conductivity, bending workability and stress relaxation characteristics in a high-level and balanced manner, it is possible to achieve copper alloy sheets with reduced alloy density (specific gravity). Attached Figure Description

[0050] Figure 1 This is a SEM image of the observation surface of the Cu-Ti alloy plate obtained in Comparative Example No. 45 after electrolytic polishing.

[0051] Figure 2 It is Figure 1 A magnified SEM image of a portion of the area.

[0052] Figure 3 It is Figure 2 A magnified SEM image of a portion of the area.

[0053] Figure 4 This is a SEM image of the observation surface of the Cu-Ti alloy plate obtained in Example No. 1 of this invention after electrolytic grinding.

[0054] Figure 5 It is Figure 4 A magnified SEM image of a portion of the area.

[0055] Figure 6 It's enlarged. Figure 5 SEM images of a portion of the area. Detailed Implementation

[0056] [Chemical Composition]

[0057] Unless otherwise specified, the "%" in relation to alloy composition refers to "mass %".

[0058] Titanium (Ti) is an element that contributes to the formation of modulated structures based on the decomposition of spindle lines, the formation of fine second-phase particles due to precipitation, and increases the strength of Cu-Ti copper alloys. It also contributes to improved stress relaxation resistance and reduced density (specific gravity). Here, alloys with a Ti content of 1.0% or more are considered. From the viewpoint of precipitation strengthening, a Ti content of 2.5% or more is more preferable. Excessive Ti content not only becomes a major cause of reduced hot and cold workability but also a major cause of reduced bending workability; therefore, the Ti content is set to 5.0% or less. It can also be managed to be 4.5% or less, or 4.0% or less.

[0059] Al (aluminum) is an effective element for reducing the density (specific gravity) of Cu-Ti copper alloys. To fully realize its effect, an Al content of 0.5% or more is required. 0.7% or more is even more effective, and 1.0% or more is even more effective. When adding more than 0.5% Al to Cu-Ti copper alloys, it is generally difficult to balance strength and bending workability. However, this problem can be eliminated using the manufacturing method described later. However, if the Al content is too high, the electrical conductivity decreases; therefore, the Al content is limited to 3.0% or less. The preferred Al content is 2.75% or less.

[0060] Ag (silver), B (boron), Be (beryllium), Co (cobalt), Cr (chromium), Fe (iron), Mg (magnesium), Mn (manganese), Nb (niobium), Ni (nickel), P (phosphorus), Si (silicon), Sn (tin), V (vanadium), Zn (zinc), Zr (zirconium), and S (sulfur) are optional elements. More than one of these elements may be included as needed. For example, Ni, Co, Fe, and Nb form intermetallic compounds with Ti, contributing to increased strength. Furthermore, these intermetallic compounds suppress grain coarsening, thus allowing for solution treatment at higher temperatures in the manufacture of copper alloy sheets, which is advantageous in terms of ensuring sufficient Ti dissolution. Sufficient Ti dissolution can be expected to suppress the formation of grain boundary reactive precipitates and increase the number of second-phase particles that contribute to higher strength. Sn has a solid solution strengthening effect and improves stress relaxation resistance. Zn, in addition to improving weldability and strength, is also effective in improving castability. Mg has an effect on improving stress relaxation resistance and desulfurization. Si can form compounds with Ti, which helps with pinning during recrystallization in the manufacture of copper alloy sheets, thus reducing grain size. Cr and Zr are effective in dispersion strengthening and suppressing grain coarsening. Mn and V readily form high-melting-point compounds with S, etc., while B and P have a finer-refining effect on the casting structure, thus contributing to improved hot workability.

[0061] The content of the aforementioned optional elements can be set within the range of Ag: 0-0.3%, B: 0-0.3%, Be: 0-0.15%, Co: 0-1.0%, Cr: 0-1.0%, Fe: 0-1.0%, Mg: 0-0.5%, Mn: 0-1.5%, Nb: 0-0.5%, Ni: 0-1.0%, P: 0-0.2%, Si: 0-0.5%, Sn: 0-1.5%, V: 0-1.0%, Zn: 0-2.0%, Zr: 0-1.0%, and S: 0-0.2%. Furthermore, the total content of these Ag, B, Be, Co, Cr, Fe, Mg, Mn, Ni, P, S, Si, Sn, V, Zn, and Zr is preferably set to 3.0% or less, more preferably 1.0% or less, and can also be controlled to 0.8% or less.

[0062] Furthermore, the contents of the aforementioned optional elements are more preferably set in the range of Ag: 0-0.1%, B: 0-0.03%, Be: 0-0.05%, Co: 0-0.1%, Cr: 0-0.1%, Fe: 0-0.2%, Mg: 0-0.25%, Mn: 0-0.2%, Nb: 0-0.04%, Ni: 0-0.2%, P: 0-0.03%, S: 0-0.03%, Si: 0-0.15%, Sn: 0-0.8%, V: 0-0.03%, Zn: 0-0.2%, and Zr: 0-0.5%.

[0063] In addition, the contents of the above-mentioned optional elements can be managed within the range of Ag: 0-0.08%, B: 0-0.02%, Be: 0-0.03%, Co: 0-0.08%, Cr: 0-0.08%, Fe: 0-0.18%, Mg: 0-0.2%, Mn: 0-0.18%, Nb: 0-0.03%, Ni: 0-0.18%, P: 0-0.02%, S: 0-0.02%, Si: 0-0.12%, Sn: 0-0.6%, V: 0-0.02%, Zn: 0-0.18%, and Zr: 0-0.4%.

[0064] In addition to the elements mentioned above, rare earth elements (REM) may be included. Rare earth elements are Sc (scandium), Y (yttrium), and lanthanides, all belonging to Group 3 of the periodic table. The inclusion of rare earth elements is effective for grain refinement and precipitate dispersion. To achieve a good balance between surface properties, strength, and conductivity of the sheet material, the total content of rare earth elements, in mass percent, is preferably 3.0% or less, more preferably 1.5% or less, and can also be controlled to 0.8% or less or 0.5% or less.

[0065] As a specific range of rare earth element content, for example, it can be listed as a range containing one or more rare earth elements selected from La (lanthanum): less than 2.0%, Ce (cerium): less than 1.8%, Pr (praseodymium): less than 0.3%, Nd (neodymium): less than 0.8%, Sm (samarium): less than 2.5%, and Y (yttrium): less than 2.5%, with a total rare earth element content of less than 3.0%.

[0066] As a range of rare earth element content considering economic efficiency and manufacturability, examples include: containing one or more rare earth elements selected from La: 0.8% or less, Ce: 0.7% or less, Pr: 0.1% or less, Nd: 0.2% or less, Sm: 1.0% or less, and Y: 1.0% or less by mass, with a total rare earth element content of 1.5% or less. As a more preferred range of rare earth element content considering economic efficiency and manufacturability, examples include: containing one or more rare earth elements selected from La: 0.35% or less, Ce: 0.32% or less, Pr: 0.04% or less, Nd: 0.1% or less, Sm: 0.5% or less, and Y: 0.5% or less by mass, with a total rare earth element content of 0.8% or less.

[0067] [Maximum width of the region where grain boundary reactive precipitates exist]

[0068] In Cu-Ti copper alloys, grain boundary reaction precipitates are easily formed. These precipitates are a major cause of reduced bending workability. If a soft microstructure is achieved, bending workability can be maintained to some extent even with the formation of a large number of grain boundary reaction precipitates. However, it is understood that controlling the microstructure to minimize the maximum width of the grain boundary reaction precipitate region is important in order to achieve a high balance between strength and bending workability in Cu-Ti copper alloy sheets. Specifically, in the copper alloy sheet of this invention, a microstructure is adopted in which the maximum width of the grain boundary reaction precipitate region in the observation plane parallel to the sheet surface is less than 1000 nm, as determined by the method described above for "determining the maximum width of the grain boundary reaction precipitate region". The manufacturing process described later, which enables finer grain diameter, is extremely effective in reducing the maximum width of the grain boundary reaction precipitate region. It should be noted that in the SEM image described above in the "Method for Determining the Maximum Width of the Region Where Grain Boundary Reactive Precipitates Exist", if the region where grain boundary reactive precipitates exist is not observed, it is considered equivalent to "the maximum width of the region where grain boundary reactive precipitates exist is less than 1000 nm".

[0069] [KAM value]

[0070] To achieve a good balance between strength and bendability, it is also important that the KAM value is not excessively high. The KAM value is one of the indicators that can evaluate the lattice strain within the grains. Based on research, the copper alloy sheet of this invention is designed to have a microstructure with a KAM value of 3.0° or lower according to the "method for calculating the KAM value" described above. As long as sufficient strength can be obtained, there is no particular limitation on the lower limit of the KAM value; it can generally be adjusted within a range of 0.5° or higher. From the viewpoint of balancing strength, bendability, and manufacturability, a KAM value in the range of 0.6 to 2.0 is more preferable.

[0071] Tensile strength

[0072] The tensile strength in the rolling direction of the copper alloy sheet of the present invention is preferably 850 MPa or more, more preferably 880 MPa or more. It can also be adjusted to a tensile strength in the rolling direction of 1000 MPa or more. There is no particular limitation on the upper limit of the tensile strength; for example, it can be adjusted within a range of 1400 MPa or less, or within a range of 1200 MPa or less.

[0073] [Number density of fine precipitate particles]

[0074] Fine precipitate particles with an aspect ratio of 5–100 nm, dispersed within the matrix (metal substrate), contribute to increased strength. The preferred number density of these fine precipitate particles with an aspect ratio of 5–100 nm is 1.0 × 10⁻⁶.8 pcs / mm 2 That's all. On the other hand, if there are too many fine precipitate particles, it can sometimes have an adverse effect on bending processability. Therefore, the number density of fine precipitate particles with a major diameter of 5–100 nm is preferably 1.0 × 10⁻⁶. 12 pcs / mm 2 The following range. Furthermore, there is a tendency that the higher the Ti content, the greater the amount of fine precipitate particles generated.

[0075] Average grain diameter

[0076] A smaller average grain diameter allows for the dispersion of sites for the formation of grain boundary reactive precipitates during the aging treatment in the manufacture of copper alloy sheets, which is advantageous in reducing the maximum width of the region where these precipitates are present. Furthermore, it also contributes to increased strength. In the copper alloy sheet of the present invention, the average grain diameter, measured using the cutting method according to JIS H0501-1986, is preferably 20 μm or less, more preferably 16 μm or less, and even more preferably 5 μm or less, in an observation plane parallel to the sheet surface. Excessively refining the average grain diameter would lead to an increase in process load; therefore, from this perspective, excessive refining of the average grain diameter is not preferable. Generally, an average grain diameter of 2 μm or more is sufficient. The subsequent manufacturing process, which involves two solution treatments, is effective in refining the grain size. It should be noted that in the cutting method specified in JIS H0501-1986, "the average value of the cutting length (mm) is used to express the value". However, since the grain diameter that is the target in this invention is very small relative to this established unit of expression, the average grain diameter in μm is determined by the method according to this standard in a higher magnification field of view.

[0077] [Bending processability]

[0078] Bending is often involved in the processing of electrically conductive components. In Cu-Ti alloys, as long as the bending workability is such that the ratio of the minimum bending radius (MBR) to the plate thickness (MBR / t) without cracking is 2.5 or less, as measured by the BW bending test under the BW (Bad Way) according to the Japanese Copper Industry Association technical standard JCBA T307:2007, it is suitable for most applications of electrically conductive components. In this invention, as a more stringent standard, a bending workability of 2.0 or less of the aforementioned MBR / t is targeted. BW (Bad Way) refers to the bending axis being parallel to the rolling direction. The MBR / t of the copper alloy sheet of this invention is preferably 1.0 or less, more preferably 0.7 or less, and even more preferably 0.0.

[0079] Furthermore, JCBA T307:2007 states that "this standard applies to the evaluation of the bending workability of thin copper and copper alloy sheets with a thickness of 0.1 mm or more and 0.8 mm or less." Based on the inventors' research, it has been confirmed that even in Cu-Ti copper alloy sheets with a thickness less than 0.1 mm, the bending workability can be evaluated using the W bending test method described in this standard. Therefore, in this invention, the W bending test method under BW shown in JCBA T307:2007 is extended to cases with a sheet thickness less than 0.1 mm (e.g., 0.02 mm or more and less than 0.1 mm), and is directly applied.

[0080] [Conductivity]

[0081] Considering the applications of Cu-Ti based copper alloy plates, a conductivity of 10.0% IACS or higher is desired. There is no specific upper limit on the conductivity; it can usually be adjusted within a range below 20.0% IACS.

[0082] [Stress relaxation characteristics]

[0083] Considering the applications of Cu-Ti copper alloy sheets, it is preferable that the stress relaxation rate (stress relief rate) after holding at 250°C for 100 hours is below 15%. There is no particular limitation on the lower limit of the stress relaxation rate, and the aforementioned stress relaxation rate is typically above 3%.

[0084] [density]

[0085] Since the atomic weight sequence of Cu, Ti, and Al is Cu > Ti > Al, increasing the Al content is most effective in reducing the density (specific gravity) of Cu-Ti copper alloys, while the effect of the Ti content cannot be ignored. The Al and Ti contents are limited in maintaining all properties—strength, workability, electrical conductivity, and stress relaxation characteristics—within the aforementioned favorable range. According to the present invention, the density at 20°C can be reduced to 8.53 g / cm³. 3 The following describes how, in Cu-Ti copper alloys, the density was reduced to 8.53 g / cm³ while maintaining all desirable properties such as strength, workability, electrical conductivity, and stress relaxation characteristics within the aforementioned range. 3 The following is something that was difficult with previous techniques. It should be noted that there is no particular limitation on the lower limit of density; for example, as long as it is within 7.8 g / cm³. 3 The above ranges can be adjusted accordingly.

[0086] [Manufacturing Method]

[0087] The copper alloy sheet described above can be manufactured, for example, through the following manufacturing process.

[0088] Melting and casting → Casting sheet heating → Hot working → Rough cold rolling → First solution treatment → First intermediate cold rolling → Second solution treatment → Second intermediate cold rolling → Aging treatment → (Fine cold rolling) → (Low-temperature annealing)

[0089] In the above, the steps marked in parentheses can be omitted. It should be noted that although not described in the above steps, surface cutting may be performed as needed after heat treatment, and pickling, grinding, or further degreasing may be performed as needed after each heat treatment. The following is a description of each of the above steps.

[0090] [Melting & Casting]

[0091] The castings with the chemical composition specified in this invention can be manufactured using a crucible furnace or similar apparatus. To prevent oxidation of Ti and Al, it is preferable to proceed in an inert gas atmosphere or a vacuum melting furnace.

[0092] [Slab heating]

[0093] Heating of the cast sheet before hot working can be carried out, for example, by holding it at 900–960°C for 0.5–5 hours.

[0094] [Hot working, rough and cold rolling]

[0095] There are no particular limitations on the hot working method. Hot forging and hot rolling are commonly used. In the case of hot rolling, the total hot rolling ratio can be, for example, 60-99%. After hot working, rapid cooling (quenching) by water cooling or the like is preferred. Then, cold rolling is performed. In this specification, the cold rolling in this stage is referred to as "rough cold rolling". The rolling ratio of rough cold rolling can be, for example, 50-99%. In this way, intermediate product sheet can be obtained for use in the first solution treatment.

[0096] Here, the rolling ratio is expressed by the following equation (1).

[0097] Rolling rate (%) = 100 × (t0 - t1) / t0…(1)

[0098] t0: Plate thickness before rolling (mm)

[0099] t1: Thickness of the rolled plate (mm)

[0100] [First solution treatment]

[0101] The aforementioned intermediate product sheet undergoes a first solution treatment. In this solution treatment, the strain introduced during hot working and rough cold rolling causes recrystallization, ensuring sufficient dissolution of coarse grain boundary reaction precipitates and granular precipitates generated after casting and hot working. If the precipitates are not sufficiently dissolved in this first solution treatment stage, they will remain in the final process, failing to achieve the desired properties. In the first solution treatment, it is advantageous to increase the amount of heat introduced to prioritize solution. While recrystallized grain growth is likely in this case, grain refinement is achieved through a subsequent second solution treatment, thus eliminating the problem. The first solution treatment can be performed at a temperature range of 750–950°C for 10–600 seconds, more preferably at 800–900°C for 20–600 seconds.

[0102] [First Intermediate Cold Rolling Mill]

[0103] The cold rolling performed on the material after the first solution treatment is called the first cold rolling. In the first cold rolling, the purpose is not only to reduce the plate thickness but also to introduce strain. If the strain introduction is insufficient, it is impossible to adequately ensure nucleation sites for recrystallization in the subsequent second solution treatment, making grain refinement difficult. For these reasons, the rolling rate needs to be set to 70% or higher in the first intermediate cold rolling. Setting it to 85% or higher is more effective, and setting it to 90% or higher is even more effective. There is no particular upper limit to the rolling rate; depending on the capacity of the cold rolling mill, it is usually set to a range below 99%.

[0104] [Second solution treatment]

[0105] In the material after the first intermediate cold rolling, the precipitates have been fully dissolved, and strain has been introduced into the crystallization of the matrix (metal substrate). A second solution treatment is then performed on the sheet material with this microstructure. In this solution treatment, new recrystallization is generated from numerous locations using the strain introduced in the first intermediate cold rolling, resulting in grain refinement. The primary objective is not the dissolution of the precipitates, but rather the grain refinement caused by recrystallization; therefore, the upper limit of the allowable heating temperature is lower than that of the first solution treatment. Specifically, this can be carried out at a temperature range of 750–900°C for 10–600 seconds. If the temperature exceeds 900°C, grain growth accompanied by grain boundary movement between recrystallized grains is likely to occur, sometimes resulting in grain coarsening. Furthermore, if the temperature is below 750°C, precipitation rather than recrystallization is more likely to occur, making it difficult to sufficiently generate fine precipitates during the aging treatment described later. The second solution treatment is more preferably performed at a temperature range of 750–880°C for 10–300 seconds, and even more preferably at a temperature range of 750–860°C for 10–150 seconds. Furthermore, from the viewpoint of appropriately achieving grain refinement in the second solution treatment, it is more effective for the heating temperature 2 in the second solution treatment to be lower than the heating temperature 1 in the first solution treatment. Additionally, when the heating temperature 2 is higher than the heating temperature 1, it is more effective if the difference is 50°C or less, and the holding time 2 at the heating temperature 2 of the second solution treatment is less than one-third of the holding time 1 at the heating temperature 1 of the first solution treatment.

[0106] [Second intermediate cold rolling]

[0107] The cold rolling performed on the material after the second solution treatment is called the second intermediate cold rolling. In the second intermediate cold rolling, a suitable strain is introduced in a way that promotes the formation of fine precipitates within the grains during the subsequent aging treatment. In addition, this strain also contributes to the improvement of strength. If too much strain is introduced, the microstructure will eventually become too high in KAM value, which may lead to a decrease in bending workability. Therefore, the rolling rate of the second intermediate cold rolling cannot be set as high as that of the first intermediate cold rolling. Specifically, the rolling rate of the second intermediate cold rolling needs to be set in the range of 15% to 50%. More preferably, it is set in the range of 15% to 40%, and can be managed in the range of 15% to 35%.

[0108] [Time-sensitive processing]

[0109] For materials that have undergone a second intermediate cold rolling process, an aging treatment is performed at 300–470°C, preferably 320–450°C, to generate fine precipitates that contribute to strength. Grain boundary reaction precipitates are also generated during aging, but because the grains are already finer, the formation sites of these precipitates are dispersed throughout the material, resulting in a metallic microstructure with a small maximum width of the region where the grain boundary reaction precipitates are present, as described above. Regarding the aging treatment time (holding time at 300–470°C), a sufficient aging treatment time can typically be set within the range of 1–24 hours to achieve the desired effect. For example, an aging treatment time preferably set within the range of 8–20 hours is preferred.

[0110] [Cold rolling, low-temperature annealing]

[0111] After aging treatment, cold rolling and low-temperature annealing can be performed as needed for purposes such as thickness adjustment and strength improvement. This stage of cold rolling is called "finish cold rolling." If the rolling ratio in finish cold rolling is too high, it results in a microstructure with an excessively high KAM value, leading to reduced bending workability. In finish cold rolling, the rolling ratio should be set to 50% or less, more preferably 30% or less, and can also be managed within the range of 25% or less. To improve strength, a rolling ratio of 5% or more is effective, and 10% or more is even more effective. Low-temperature annealing can be performed at a temperature range of 350–550°C, preferably 400–500°C, for a holding time of 60 seconds or less. A holding time of 15 seconds or more within the above temperature range is effective.

[0112] The final plate thickness can be, for example, in the range of 0.02 to 0.50 mm.

[0113] [Electrified components]

[0114] The copper alloy sheet of the present invention described above possesses all the characteristics of strength, conductivity, bending workability, and stress relaxation properties in a high-level and balanced manner, and its density (specific gravity) is reduced. Therefore, using this sheet for electrical components meets the high-functionality requirements of portable terminals and automotive electronic devices in recent years.

[0115] [Heat dissipation components]

[0116] The copper alloy sheet of the present invention described above possesses all the characteristics of strength, conductivity, bending workability, and stress relaxation properties in a high-level and balanced manner (materials with excellent conductivity generally have excellent heat dissipation), and the density (specific gravity) is reduced. Therefore, using this sheet as a heat dissipation component of a material meets the high-functionality requirements of portable terminals and automotive electronic devices in recent years.

[0117] Example

[0118] The copper alloy with the chemical composition shown in Table 1 was smelted and then cast. In Example No. 14 of this invention, a cerium-lanthanum alloy (a mixture of rare earth elements) was added to the total amount of copper alloy raw materials at a ratio of 0.32% by mass as a source of rare earth elements. The mass ratio of the main rare earth elements contained in this cerium-lanthanum alloy (misch metal) was La:Ce:Pr:Nd = 28:50:5:17.

[0119] The resulting castings were heated at the temperatures and times shown in Tables 2 and 3. Except for a few examples (Comparative Examples No. 40 and 41), the castings were removed from the furnace, hot-rolled to the thicknesses recorded in Tables 2 and 3, and then water-cooled. The total hot rolling rate was 87.5%–95%. After hot rolling, the oxide layer on the surface was removed by mechanical grinding (surface cutting), and each hot-rolled material was cold-rolled to the thicknesses recorded in the "Rough Cold Rolling" column of Tables 2 and 3.

[0120] Subsequently, except for a few examples (Comparative Examples No. 31, 38, 39, 40, 41, 45), the first solution treatment, first intermediate cold rolling, second solution treatment, second intermediate cold rolling, and aging treatment were performed sequentially under the conditions shown in Tables 2 and 3. The aging treatment was carried out in a batch heat treatment furnace under a nitrogen atmosphere. For Invention Examples No. 4, 5, 11, and Comparative Example 37, fine cold rolling and low-temperature annealing were performed after the aging treatment under the conditions described in Tables 2 and 3. The "-" (hyphen) in Tables 2 and 3 indicates that a process was omitted. No. 31, 39, and 45 omitted the first intermediate cold rolling and the second solution treatment. No. 38 is a process in which a pre-aging treatment (pre-treatment) is performed after solution treatment, followed by aging treatment after cold rolling with a light rolling ratio. No. 40 is a process in which the aging treatment is performed directly on the cast sheet that has undergone homogenization heat treatment, without hot rolling or cold rolling. Example No. 41 describes a process where a heat-treated, homogenized casting is cold-rolled at a rate of 85% to produce a sheet with a thickness of 0.10 mm, followed by solution treatment and aging treatment, without hot rolling. The thickness of the final sheet is shown in Tables 2 and 3. This sheet was used as the test material for the following investigation. In example No. 40, since no rolling process was performed, a sample cut from the material after aging treatment was etched to a thickness of 0.08 mm as the test material. It should be noted that density (specific gravity) was measured using a block sample cut from the material after the heating stage of the casting.

[0121] (Average grain diameter)

[0122] The surface of the test material was ground using the electrolytic grinding conditions described in the "Method for Determining the Number Density of Fine Precipitate Particles" section above. The surface, refined by electrolytic grinding, was etched to create an observation surface. The observation surface was observed using an optical microscope at 1000x magnification to obtain an image. Three straight lines parallel to the rolled surface were drawn, and the number of grain boundaries cut by each line was counted using the cutting method according to JIS H0501-1986. The average grain diameter in the observation field was then calculated. This operation was performed on five randomly selected fields of view, and the arithmetic mean of the average grain diameters obtained in each field was taken as the average grain diameter of the material. It should be noted that an OLYMPUS LEXT OLS4000 optical microscope was used.

[0123] (Maximum width of the region where grain boundary reactive precipitates exist)

[0124] The surface of the test material was ground using the electrolytic grinding conditions described in the "Method for Determining the Number Density of Fine Precipitate Particles" above. The observation surface refined by electrolytic grinding was observed using SEM (scanning electron microscope). The maximum width of the grain boundary reaction type precipitate area was determined according to the "Method for Determining the Maximum Width of the Grain Boundary Reaction Type Precipitate Area" above.

[0125] (Number density of fine precipitate particles)

[0126] The number density of fine precipitate particles is calculated according to the above-mentioned method for "determining the number density of fine precipitate particles".

[0127] (KAM value)

[0128] After polishing and grinding the sample surface cut from the test material, ion milling was performed to prepare the sample surface for EBSD (electron beam backscatter diffraction) measurement. The sample surface was observed using a FE-SEM (JSM-7200F, NEC Corporation) at an accelerating voltage of 15 kV and a magnification of 500x. For a rectangular measurement area of ​​240 μm × 180 μm in the thickness direction, EBSD data was acquired using an EBSD device (Symmetry, Oxford Instruments) installed on the FE-SEM, with a step size of 0.1 μm. Based on the crystalline orientation data measured in the measurement area of ​​five fields of view, the KAM value was calculated according to the "KAM value calculation method" described above. OIM-Analysis 7.3.1, manufactured by TSL Solutions Co., Ltd., was used as the software for EBSD data analysis.

[0129] (Tensile strength)

[0130] Tensile test specimens (JIS No. 5) were collected from each test material along the rolling direction (arbitrary direction in example No. 40). Tensile tests were conducted according to JIS Z2241 with a test number n=3, and the tensile strength was determined. The average value of n=3 was taken as the score for the test material. Furthermore, the 0.2% yield strength obtained from this tensile test was used for the determination of the stress relaxation rate, which will be discussed later.

[0131] (Conductivity)

[0132] According to JIS H0505, the conductivity of each test material was determined using the double-bridge, average cross-sectional area method.

[0133] (MBR / t with 90° W bending)

[0134] The ratio of the minimum bending radius (MBR) without cracking to the plate thickness (t) was determined using the BW bending test according to the Japanese Copper Industry Association technical standard JCBA T307:2007, based on the BW standard. The test piece dimensions were 30 mm in the right-angle direction of rolling and 10 mm in the rolling direction. However, in Example No. 40, the arbitrary direction was defined as the longitudinal direction. Bending tests with progressively varying bending radii were conducted for one bending radius with a test number n=3. The minimum bending radius among all three test pieces from which no cracks were observed on the bending surface was taken as the MBR of the test material. The determination of whether cracks were present on the bending surface was performed according to JCBA T307:2007. For samples judged as "wrinkles: large" based on visual observation of the bending surface, a specimen was prepared by cutting the deepest wrinkle in a direction perpendicular to the bending axis. The ground cross-section was observed using an optical microscope to confirm whether cracks propagating inwards towards the plate thickness were present. If no such cracks were observed, it was determined as "no cracks observed".

[0135] (Stress relaxation rate)

[0136] A 10mm wide test piece was cut from the test material, rolled at a right angle (any direction in example No. 40). The stress relaxation rate was determined using a cantilever beam method according to the Japanese Copper Industry Association technical standard JCBA T309:2004. The test piece was placed with the deflection along the thickness direction, under a load stress equivalent to 80% of the yield strength (0.2%), and the stress relaxation rate was measured after holding at 250°C for 100 hours. If the stress relaxation rate is less than 15% under these conditions, it can be determined that the Cu-Ti copper alloy sheet has good stress relaxation resistance.

[0137] (density)

[0138] Density at room temperature (20°C) was determined using the Archimedes method (gravimetric method in water) on 10g block samples cut from material after the casting heating stage.

[0139] The results are shown in Tables 4 and 5.

[0140] [Table 1]

[0141] Table 1

[0142]

[0143] Underlined: Outside the scope defined in this invention [Table 2]

[0144]

[0145] [Table 3]

[0146]

[0147] [Table 4]

[0148]

[0149] [Table 5]

[0150]

[0151] The sheet material of this invention, whose chemical composition and manufacturing conditions were strictly controlled in accordance with the above provisions, exhibits good strength, electrical conductivity, bending workability, and stress relaxation characteristics, and also shows excellent density (specific gravity) reduction effect.

[0152] In contrast, in Comparative Example No. 31, only one solution treatment was performed, resulting in a larger maximum width of the region containing grain boundary reaction precipitates and poor bending workability.

[0153] No. 32 has reduced conductivity due to excessive Al content.

[0154] No. 33 Due to the low temperature of the first solution treatment, the solidification of the precipitated phase is insufficient, resulting in a large maximum width of the region containing grain boundary reaction precipitates and poor bending workability. In addition, the amount of fine precipitates is insufficient, and their strength is also low.

[0155] No. 34: Due to the excessively high temperature of the first solution treatment, the grains became coarse and the strength was low.

[0156] No. 35 has low strength because the rolling rate in the first intermediate cold rolling is low, so it is impossible to achieve grain refinement in the second solution treatment.

[0157] No. 36 has poor bending workability because the rolling rate in the second intermediate cold rolling is too high.

[0158] No. 37 Because the rolling rate in the cold rolling process is too high, the KAM value becomes too large, resulting in poor bending workability.

[0159] Since No. 38 does not contain Al, it does not achieve a reduction in density (specific gravity).

[0160] Since No. 39 does not contain Al, it does not achieve a reduction in density (specific gravity). Furthermore, due to the use of a single solution treatment process at high temperature, the maximum width of the region containing grain boundary reaction precipitates increases, resulting in poor bending workability.

[0161] Example No. 40 is an example where no rolling process was performed. In this case, due to its soft nature, although the maximum width of the region where grain boundary reaction precipitates are present is large, the bending workability is good. However, the amount of fine precipitates formed is small, resulting in low electrical conductivity. In addition, due to the small amount of fine precipitates and the large average grain diameter, the strength is also low.

[0162] No. 41 contains no Al but contains Mg, thus achieving a reduction in density (specific gravity). However, it does not achieve high strength.

[0163] No. 42 has insufficient Ti content, resulting in inadequate formation of fine precipitates and low strength. Furthermore, it does not achieve a reduction in density (specific gravity).

[0164] No. 43 has excessive Ti content, resulting in excessive formation of fine precipitates and poor bending processability.

[0165] No. 44 did not achieve a reduction in density (specific gravity) because of its low Al content.

[0166] Since No. 45 does not contain Al, it does not achieve a reduction in density (specific gravity). Furthermore, because only one solution treatment was performed, the maximum width of the region containing grain boundary reactive precipitates is increased, resulting in poor bending workability.

[0167] No. 46 has low strength because the temperature of the second solution treatment is low, resulting in insufficient grain refinement.

[0168] For reference only. Figures 1-3 The image shows a SEM photograph of the observation surface of the Cu-Ti alloy sheet obtained in Comparative Example No. 45, after electrolytic polishing. Additionally, Figures 4-6 The image shows SEM photographs of the observation surface of the Cu-Ti alloy sheet obtained in Example No. 1 of this invention, after electrolytic polishing. Regarding the length of the white scale bar at the bottom of each photograph, [the text is incomplete]. Figure 1 , Figure 4 The equivalent of 10μm is in Figure 2 , Figure 3 , Figure 5 , Figure 6 The middle part is equivalent to 1μm.

Claims

1. Copper alloy sheet, having the following composition (by mass%): Ti: 1.0–5.0%, Al: 0.5–3.0%, Ag: 0–0.3%, B: 0–0.3%, Be: 0–0.15%, Co: 0–1.0%, Cr: 0–1.0%, Fe: 0–1.0%, Mg: 0–0.5%, Mn: 0–1.5%, Nb: 0.0–0.5%, Ni: 0–1.0%. The composition is as follows: P: 0-0.2%, Si: 0-0.5%, Sn: 0-1.5%, V: 0-1.0%, Zn: 0-2.0%, Zr: 0-1.0%, S: 0-0.2%. The total content of Ag, B, Be, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, Si, Sn, V, Zn, Zr, and S is less than 3.0%, with the balance consisting of Cu and unavoidable impurities. In the observation plane parallel to the plate surface, the maximum width of the region where grain boundary reaction precipitates exist is less than 1000 nm. In the measurement based on EBSD (electron beam backscatter diffraction) with a step size of 0.1 μm in the observation plane parallel to the plate surface, the KAM value when the boundary with a crystal orientation difference of more than 15° is regarded as a grain boundary is less than 3.0°, and the tensile strength in the rolling direction is more than 850 MPa.

2. The copper alloy plate according to claim 1 further comprises the following composition: containing rare earth elements in a total of less than 3.0% by mass.

3. The copper alloy sheet according to claim 1 or 2, wherein, In the observation plane parallel to the plate surface, the number density of fine precipitate particles with a major diameter of 5–100 nm is 1.0 × 10⁻⁶. 8 pcs / mm 2 Above and 1.0×10 12 pcs / mm 2 the following.

4. The copper alloy sheet according to claim 1 or 2, wherein, In the observation plane parallel to the plate surface, the average grain diameter using the cutting method according to JIS H0501-1986 is 2–20 μm.

5. The copper alloy sheet according to claim 1 or 2, wherein, The minimum bending radius (MBR) without cracking, as determined by the W-bending test under BW according to the Japanese Copper Industry Association technical standard JCBAT307:2007, has a ratio of MBR / t of 2.0 or less to the plate thickness (t).

6. The copper alloy sheet according to claim 1 or 2, wherein, The conductivity is above 10.0% IACS.

7. The copper alloy sheet according to claim 1 or 2, wherein, The density is 8.53 g / cm³. 3 the following.

8. The copper alloy sheet according to claim 1 or 2, wherein, The plate thickness is 0.02 to 0.50 mm.

9. The method for manufacturing the copper alloy plate according to claim 1, wherein, In the process of manufacturing copper alloy sheets by sequentially performing a first solution treatment, a first intermediate cold rolling, a second solution treatment, a second intermediate cold rolling, and an aging treatment on intermediate product sheets, The first solution treatment was performed at a temperature range of 750–950°C for 10–600 seconds. The first intermediate cold rolling is carried out with a rolling ratio of over 70%. The second solution treatment was carried out at a temperature range of 750–900°C for 10–600 seconds. A second intermediate cold rolling process is performed with a rolling rate of 15-50%. Aging treatment is carried out at an aging temperature of 300–470℃. The intermediate product sheet has the following composition (by mass%): Ti: 1.0–5.0%, Al: 0.5–3.0%, Ag: 0–0.3%, B: 0–0.3%, Be: 0–0.15%, Co: 0–1.0%, Cr: 0–1.0%, Fe: 0–1.0%, Mg: 0–0.5%, Mn: 0–1.5%, Nb: 0.0–0.5%, Ni: 0–1.0%. The total content of Ag, B, Be, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, Si, Sn, V, Zn, Zr and S is less than 3.0%, with the balance consisting of Cu and unavoidable impurities.

10. The method for manufacturing copper alloy sheet according to claim 9, wherein, The intermediate product board also has the following composition: containing rare earth elements in a total range of less than 3.0% by mass.

11. The method for manufacturing copper alloy sheet according to claim 9 or 10, wherein, In the process of manufacturing copper alloy plates by further performing precision cold rolling and low-temperature annealing after the aging treatment, precision cold rolling is performed with a rolling rate of less than 50%, and low-temperature annealing is performed under the condition of holding at a temperature range of 350 to 550°C for less than 60 seconds.

12. An electrically conductive component, which uses the copper alloy sheet as described in claim 1 or 2 as a material.

13. A heat dissipation component, which uses the copper alloy plate as described in claim 1 or 2 as the material.

Citation Information

Patent Citations

  • Copper alloy sheet, and method for producing the same

    JP2010126777A

  • Cu-Ti-BASED COPPER ALLOY PLATE, MANUFACTURING METHOD THEREFOR AND ELECTRIC CONDUCTION PARTS

    JP2014185370A

  • Cu-Ti based copper alloy sheet material and method for producing the same, and electric current carrying component

    CN104073678A