By designing gradient multilayer metal layers on flexible current collectors, the problems of poor bonding and insufficient conductivity were solved, resulting in composite current collector materials with high bonding strength, good conductivity and long life, thus improving production efficiency and yield.
Patent Information
- Application Number
- CN202310753904.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-21
AI Technical Summary
Traditional flexible current collectors are easily damaged during the coating process, resulting in poor adhesion, insufficient conductivity and strength, and short service life.
The design employs a gradient multilayer metal layer structure. By depositing multiple metal layers of different thicknesses and grain sizes on the surface of the flexible insulating film material, thickness gradients and grain gradients are formed, thereby optimizing the bonding force and conductivity between the metal layers and the insulating film.
This improved the bonding strength between the metal layer and the insulating film, enhanced the conductivity and mechanical properties of the composite current collector, extended its service life, and reduced production costs.
Smart Images

Figure CN116895761B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery current collector technology, and particularly relates to a flexible composite positive electrode current collector with a gradient multilayer metal layer structure and its preparation method. Background Technology
[0002] Current collectors are crucial components in lithium-ion battery electrodes, primarily functioning to collect and output the current generated by the active material or to input the electrode current to the active material. Traditional lithium-ion battery positive electrode current collectors are made of aluminum foil. Composite current collectors, which use a flexible insulating thin film material as a support layer and further fabricate a conductive metal layer on its surface using vacuum deposition technology, effectively reduce battery weight and improve specific power and safety compared to traditional current collectors.
[0003] The commonly used vacuum deposition technology for preparing flexible current collector metal layers refers to physical vapor deposition (PVD), mainly including vacuum evaporation deposition and magnetron sputtering deposition. However, from the perspective of substrate materials, flexible insulating thin film materials have significant differences in mechanical properties, thermal properties, and surface activity compared to traditional metal materials. They are easily damaged during the deposition process, including mechanical and thermal damage, making it difficult to obtain composite current collector materials with good adhesion and high strength. Furthermore, from the perspective of the coating, the electrical properties of the metal layer are closely related to its macroscopic and microscopic structure, and the interface matching degree between the metal layer and the flexible substrate must be considered during the deposition of the metal layer. Therefore, it is necessary to rationally control the deposition parameters and design and optimize the macroscopic and microscopic structure of the metal layer to obtain flexible composite current collector materials with high adhesion, good conductivity, high strength, and long service life. Summary of the Invention
[0004] In view of the problems described above, this invention proposes a flexible composite positive electrode current collector with gradient multilayer metal layers and its preparation method. This composite positive electrode current collector uses a flexible insulating thin film material as a support layer, on which gradient multilayer metal layers are prepared. Through optimized design of the macroscopic and microscopic structures of the metal layers, the bonding force between the metal layers and the insulating thin film is improved, resulting in a composite current collector with good conductivity, high strength, and long service life. This invention mainly solves the problems of poor bonding force between the metal layers and the flexible thin film material, as well as poor strength and conductivity of the composite current collector after metal layer deposition.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] The first objective of this invention is a flexible composite positive current collector with a gradient multilayer metal layer structure, comprising a flexible insulating film layer, an adhesive layer deposited on both sides of the flexible insulating film layer, and a metal composite layer deposited on the surface of the adhesive layer; the metal composite layer comprises multiple metal layers of different thicknesses, the thickness of the multiple metal layers increasing with the increase of the distance between them and the flexible insulating film layer, and the grain size in the multiple metal layers decreasing with the increase of the distance between them and the flexible insulating film layer.
[0007] Furthermore, the flexible insulating film layer is made of PET, PP, PI, PC, PMMA, PVC or TAC, and its thickness is 2-12μm.
[0008] Furthermore, the adhesive layer and the metal composite layer are made of the same material, namely aluminum or aluminum alloy. The thickness of the adhesive layer is 5-20 nm.
[0009] Furthermore, the total number of metal layers in the metal composite layer does not exceed six; the total thickness of the metal composite layer is 0.6-1.2 μm, wherein the thinnest metal layer has a thickness of 20-100 nm and the thickest metal layer has a thickness of 200-700 nm; the grain size in the thinnest metal layer is 1000-2000 nm and the grain size in the thickest metal layer is 50-250 nm.
[0010] Another object of the present invention is to provide a method for preparing a flexible composite positive current collector having a gradient multilayer metal layer structure as described in the first object, comprising the following steps:
[0011] (1) The flexible insulating film is placed in the vacuum chamber of the vacuum evaporation and winding coating machine and subjected to plasma surface pretreatment; preferably, the vacuum degree in the vacuum chamber of the vacuum evaporation and winding coating machine is 8.0 × 10⁻⁶. -3 Pa ~ 1.0 × 10 -3 Pa; the current for plasma surface pretreatment is 0.5 to 5 A, and the Ar gas flow rate is 10 to 300 sccm.
[0012] (2) An adhesive layer is deposited on the surface of the insulating film material by vacuum evaporation deposition; preferably, the process parameters of vacuum evaporation deposition are: the wire feeding speed of the evaporation boat is 100 to 150 mm / min, the winding speed is 120 to 180 m / min, and the cooling temperature is not lower than 10℃.
[0013] (3) A first metal layer is deposited on the surface of the insulating film with the already deposited adhesive layer by vacuum evaporation deposition;
[0014] (4) By adjusting the deposition parameters of vacuum evaporation deposition, repeat step (3) to sequentially deposit multiple metal layers of different thicknesses and different grain sizes to form a metal composite layer and obtain the final product.
[0015] Furthermore, in step (3), the process parameters for vacuum evaporation deposition are: the evaporation boat wire feeding speed is 50 to 150 mm / min, the winding speed is 150 to 250 m / min, and the cooling temperature is 40 to 60 °C; in step (4), the method for adjusting the deposition parameters of vacuum evaporation deposition is: the evaporation boat wire feeding speed is gradually increased, but not higher than 700 mm / min; the winding speed is gradually decreased, but not lower than 30 m / min; and the cooling temperature is gradually decreased, but not lower than 0 °C.
[0016] Compared with existing technologies, the present invention has the following advantages:
[0017] The flexible composite positive current collector provided by this invention includes a metal composite layer. This layer comprises multiple metal layers of varying thicknesses, with the thickness of each layer increasing with the distance between it and the flexible insulating film layer, thus creating a thickness gradient. This thickness gradient provides favorable conditions for the release of thermal stress in the insulating film during the initial stage of metal layer deposition, enabling rapid heat dissipation, reducing or avoiding thermal damage, and improving the bonding strength between the metal layers and the insulating film, as well as the mechanical properties of the composite current collector. Furthermore, the grain size of each metal layer decreases with increasing distance from the flexible insulating film layer, creating a grain gradient. The interfacial resistance between the insulating film and the metal layers has a significant impact on the conductivity of the current collector. Therefore, using a metal layer with a large grain size (few grain boundaries) near the film can reduce the interfacial resistance by decreasing the scattering of free electrons by the grain boundaries. This approach can be applied to the entire metal layer, thereby reducing the interfacial resistance between metal layers, improving the overall conductivity of the metal layer, and ultimately enhancing the electrical performance of the composite current collector. The outermost metal layer has the smallest grain size (with a high number of grain boundaries), ensuring the density of the metal layer surface. This is beneficial for improving the oxidation resistance and corrosion resistance of the metal composite layer, and increasing the service life of the current collector. Therefore, the grain gradient design can reduce the influence of grain boundary scattering and interface resistance on the resistance of the composite current collector, improve conductivity, and extend service life. This invention, through a multi-layer gradient metal layer design, can improve the bonding force between the metal layer and the insulating film, obtaining a composite current collector material with good conductivity, high strength, and long service life. The preparation method provided by this invention can be achieved using a single vacuum evaporation and winding plating equipment, which can improve yield and production efficiency, and reduce costs. Attached Figure Description
[0018] Figure 1 A cross-sectional view of the flexible composite positive electrode current collector provided by the present invention;
[0019] Figure 2for Figure 1 Enlarged view of the metal composite layer;
[0020] Figure 3 The statistical results of the grain size of each metal layer in the product prepared in Example 1;
[0021] Reference numerals: 10-flexible insulating film layer; 20-adhesive layer; 30-metal composite layer; 31-first metal layer; 32-second metal layer; 33-third metal layer; 34-fourth metal layer; 35-fifth metal layer. Detailed Implementation
[0022] The present invention will be further described below with reference to embodiments, so that those skilled in the art can better understand and implement the present invention, but the embodiments are not intended to limit the present invention.
[0023] In addition, unless otherwise specified, the preparation processes in the following embodiments are all conventional methods in the prior art, and therefore will not be described in detail.
[0024] Example 1
[0025] refer to Figure 1 A flexible composite positive current collector with a gradient multilayer metal structure includes a flexible insulating film layer 10, an adhesive layer 20 deposited on both sides of the flexible insulating film layer, and a metal composite layer 30 deposited on the surface of the adhesive layer. The metal composite layer 30 includes multiple metal layers of different thicknesses. The thickness of the multiple metal layers increases with the increase of the distance between them and the flexible insulating film layer, and the grain size in the multiple metal layers decreases with the increase of the distance between them and the flexible insulating film layer. Specifically, there are five metal layers in total, from the inside out: a first metal layer 31, a second metal layer 32, a third metal layer 33, a fourth metal layer 34, and a fifth metal layer 35. It should be noted that the number of metal layers can be adjusted according to actual needs, as long as the number of layers does not exceed six, the purpose of this invention can be achieved.
[0026] The preparation method of this flexible composite positive electrode current collector includes the following steps:
[0027] (1) A flexible insulating film layer 10 of PET material with a thickness of 6 μm was selected and placed in the vacuum chamber of a vacuum evaporation roll coating machine for plasma surface pretreatment; the vacuum degree in the vacuum chamber of the vacuum evaporation roll coating machine was 5 × 10⁻⁶. -3 Pa, the current for plasma surface pretreatment is 1A, and the Ar gas flow rate is 100sccm.
[0028] (2) An adhesive layer 20 was deposited on the surface of the insulating film material by vacuum evaporation deposition. The adhesive layer material was Al. The process parameters for vacuum evaporation deposition were: evaporation boat wire feeding speed of 125 mm / min, winding speed of 150 m / min, and cooling temperature of 45 °C. After the adhesive layer was deposited, the average sheet resistance of the PET material was approximately 9.5 Ω / □.
[0029] (3) A first metal layer is deposited on the surface of the insulating film with the already deposited adhesive layer by vacuum evaporation deposition;
[0030] (4) By adjusting the deposition parameters of the vacuum evaporation deposition, step (3) is repeated to sequentially deposit multiple metal layers of different thicknesses, forming a metal composite layer and obtaining the final product. The material of the obtained metal composite layer is Al, and the total thickness is approximately 800 nm. The first metal layer 31 has a thickness of approximately 50 nm, and its evaporation parameters are as follows: evaporation boat wire feeding speed of 80 mm / min, winding speed of 200 m / min, and main drum temperature of 50 °C. The second metal layer 32 has a thickness of approximately 100 nm, and its evaporation parameters are as follows: evaporation boat wire feeding speed of 100 mm / min, winding speed of 120 m / min, and main drum temperature of 40 °C. The third metal layer 33 has a thickness of approximately 150 nm, and its evaporation parameters are as follows: evaporation boat wire feeding speed of 160 mm / min, winding speed of 110 m / min, and main drum temperature of 30 °C. The fourth metal layer 34 has a thickness of approximately 200 nm, and its evaporation parameters are as follows: evaporation boat wire feeding speed of 200 mm / min, winding speed of 75 m / min, and main drum temperature of 20 °C. The fifth metal layer 35 has a thickness of approximately 300 nm, and its evaporation parameters are as follows: evaporation boat wire feeding speed of 360 mm / min, winding speed of 45 m / min, and main drum temperature of 0 °C.
[0031] The average grain size after deposition of each metal layer was statistically analyzed using scanning electron microscope (SEM) surface morphology images at the same magnification. The results are as follows: Figure 3 As shown. Subsequent embodiments use the same method to calculate grain size. From Figure 3 As can be seen, with the increase of deposition cycles, the grain size of each layer gradually decreases, inversely proportional to the change in the thickness of each layer of the metal composite layer. This is due to the synergistic effect of wire feed speed, winding speed, and main drum temperature. Decreasing wire feed speed and increasing winding speed both reduce the deposition efficiency of the metal layer, i.e., the metal layer thickness decreases. In this case, the grains do not have enough time to grow, thus easily resulting in small grain size and poor electrical conductivity. This embodiment uses a high main drum temperature under evaporation parameters with low deposition efficiency to promote nucleation, increase grain size, and reduce resistivity; conversely, under evaporation parameters with high deposition efficiency, a low main drum temperature is used to inhibit nucleation and limit grain growth, thereby forming a small-grain-size metal layer, increasing the density of the metal layer, and improving its service life.
[0032] Example 2
[0033] The preparation method of the flexible composite positive current collector in this embodiment is the same as that in Example 1, steps (1) to (3) are the same, and the specific parameters of step (4) are as follows:
[0034] By adjusting the deposition parameters of vacuum evaporation deposition, step (3) is repeated to sequentially deposit multiple metal layers of different thicknesses, forming a metal composite layer and obtaining the final product. The material of the obtained metal composite layer is Al, and the total thickness is approximately 800 nm. Among them, the thickness of the first metal layer 31 is approximately 130 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 150 mm / min, winding speed of 150 m / min, and main drum temperature of 60 °C; the thickness of the second metal layer 32 is approximately 670 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 650 mm / min, winding speed of 35 m / min, and main drum temperature of 25 °C.
[0035] Example 3
[0036] The preparation method of the flexible composite positive current collector in this embodiment is the same as that in Example 1, steps (1) to (3) are the same, and the specific parameters of step (4) are as follows:
[0037] By adjusting the deposition parameters of vacuum evaporation deposition, step (3) is repeated to sequentially deposit multiple metal layers of different thicknesses, forming a metal composite layer and obtaining the final product. The material of the obtained metal composite layer is Al, and the total thickness is approximately 800 nm. Among them, the thickness of the first metal layer 31 is approximately 20 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 50 mm / min, winding speed of 250 m / min, and main drum temperature of 60 °C; the thickness of the second metal layer 32 is approximately 60 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 90 mm / min, winding speed of 200 m / min, and main drum temperature of 55 °C; the thickness of the third metal layer 33 is approximately 120 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 140 mm / min, winding speed of 140 m / min, and main drum temperature of 40 °C. The fourth metal layer 34 has a thickness of approximately 150 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 160 mm / min, winding speed of 110 m / min, and main drum temperature of 30 °C; the fifth metal layer 35 has a thickness of approximately 200 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 200 mm / min, winding speed of 75 m / min, and main drum temperature of 15 °C; the sixth metal layer 36 has a thickness of approximately 250 nm, and the specific evaporation parameters are: evaporation boat wire feeding speed of 300 mm / min, winding speed of 45 m / min, and main drum temperature of 0 °C.
[0038] Comparative Example 1
[0039] The composite current collector described in Comparative Example 1 mainly comprises: 10-a flexible insulating film; 20-an adhesive layer and 30-a metal layer. Among them, the 30-metal layer is a single-layer structure.
[0040] The evaporation parameters of the 10-flexible insulating film and the 20-adhesive layer used in this comparative example are the same as those in Example 1.
[0041] In this comparative example, the 30-metal layer is Al prepared by vacuum evaporation deposition, with a total thickness of approximately 800 nm. The specific evaporation parameters are: evaporation boat wire feeding speed of 900 mm / min, winding speed of 40 m / min, and main drum temperature of 0 °C.
[0042] Comparative Example 2
[0043] The composite current collector described in Comparative Example 2 mainly comprises: 10-a flexible insulating film; 20-an adhesive layer and 30-a metal composite layer. The 30-metal layer has a multilayer structure with each layer having equal thickness and a total of 10 layers.
[0044] The evaporation parameters of the 10-flexible insulating film and the 20-adhesive layer used in this comparative example are the same as those in Example 1.
[0045] In this comparative example, the 30-metal layer is Al prepared by vacuum evaporation deposition, with a total thickness of approximately 800 nm. In the multilayer structure of equal thickness, each layer has a thickness of approximately 80 nm. The specific evaporation parameters for each layer are: evaporation boat wire feed speed of 100 mm / min, winding speed of 180 m / min, and main drum temperature of 0 °C. To meet the thickness requirements, this process was repeated 10 times to obtain the target product.
[0046] Comparative Example 3
[0047] The composite current collector described in Comparative Example 3 mainly comprises: 10-a flexible insulating film; 20-an adhesive layer and 30-a metal composite layer. The 30-metal layer has a multi-layer structure with each layer having equal thickness and a total of 5 layers.
[0048] The evaporation parameters of the 10-flexible insulating film and the 20-adhesive layer used in this comparative example are the same as those in Example 1.
[0049] In this comparative example, the 30-metal layer is Al prepared by vacuum evaporation deposition, with a total thickness of approximately 800 nm. In the multilayer structure of equal thickness, each layer has a thickness of approximately 160 nm. The specific evaporation parameters for each layer are: evaporation boat wire feed speed of 180 mm / min, winding speed of 120 m / min, and main drum temperature of 30 °C. To meet the thickness requirements, this process was repeated 5 times, resulting in Comparative Example 3.
[0050] The composite current collectors obtained in each embodiment and comparative example were subjected to statistical analysis of grain size and tests of coating adhesion and conductivity. Coating adhesion was tested using the EAA thin film peel test method, with five different locations randomly selected in the composite current collector for testing; the final adhesion value was the average of the five tests. Resistivity was tested using a four-probe resistance meter, with five different locations randomly selected in the composite current collector for testing; the final resistivity value was the average of the five tests. The results are shown in Table 1.
[0051] Table 1. Performance test results of the products prepared in each embodiment and comparative example.
[0052]
[0053]
[0054] As can be seen from Table 1, Example 1 has the smallest surface grain size, followed by Example 3, then Example 2. The surface grain size of the comparative examples is larger than that of the examples, with Comparative Example 1 having the smallest, followed by Comparative Example 2, and then Comparative Example 3. Example 3 has the best bonding strength, similar to Example 1 and Comparative Example 2, followed by Example 2, then Comparative Example 3, and Comparative Example 1 has the worst. Example 2 has the lowest resistivity, followed by Example 1. The resistivity of Example 3 and Comparative Example 1 is similar but higher than that of Example 1, with Example 2 having the highest resistivity.
[0055] Comparing Examples 1, 2, and 3, it can be seen that the more layers of the metal composite layer there are, the better its bonding force with the polymer insulating film, but the worse its conductivity; this rule can also be seen in the comparison of each comparative example.
[0056] Comparing Example 1 and Comparative Example 1, it can be seen that the single-layer metal layer has good conductivity but poor adhesion. Therefore, in order to obtain a composite current collector with adhesion that meets the application requirements, it is necessary to adopt a multi-layer structure.
[0057] Comparing Example 1 and Comparative Example 2, it can be seen that when the coating adhesion is similar, the higher the number of layers, the higher the resistivity of the composite current collector. Therefore, in order to obtain a composite current collector with electrical performance that meets the application requirements, it is necessary to control the number of coating layers.
[0058] Comparing Example 1 and Comparative Example 3, it can be seen that with the same number of metal composite layers, the use of a gradient structure can achieve better bonding and conductivity. Comparing Example 3 and Comparative Example 3, it can be seen that even with a greater number of metal composite layers, Example 3 still exhibits better bonding and conductivity. This indicates that a gradient design in terms of thickness and grain size is beneficial for improving the overall performance of the composite current collector.
[0059] Comparing Example 2 and Comparative Example 1, it can be seen that when the metal composite layer has two layers, the bonding force can be improved to a certain extent and better conductivity can be obtained. Comparing Example 3 and Comparative Example 1, it can be seen that when the resistivity is not much different, the use of a gradient multilayer structure can significantly improve the bonding force.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A flexible composite positive current collector with a gradient multilayer metal layer structure, characterized in that: The invention includes a flexible insulating film layer, an adhesive layer deposited on both sides of the flexible insulating film layer, and a metal composite layer deposited on the surface of the adhesive layer; the metal composite layer includes multiple metal layers of different thicknesses, the thickness of the multiple metal layers increases with the increase of the distance between them and the flexible insulating film layer, and the grain size in the multiple metal layers decreases with the increase of the distance between them and the flexible insulating film layer. The total number of metal layers in the metal composite layer does not exceed six; the total thickness of the metal composite layer is 0.6-1.2 μm, wherein the thinnest metal layer has a thickness of 20-100 nm and the thickest metal layer has a thickness of 200-700 nm; the grain size in the thinnest metal layer is 1000-2000 nm and the grain size in the thickest metal layer is 50-250 nm.
2. The flexible composite positive current collector with a gradient multilayer metal layer structure according to claim 1, characterized in that: The flexible insulating film layer is made of PET, PP, PI, PC, PMMA, PVC or TAC.
3. The flexible composite positive current collector with a gradient multilayer metal layer structure according to claim 1, characterized in that: The adhesive layer and the metal composite layer are made of the same material, namely aluminum or aluminum alloy.
4. The method for preparing a flexible composite positive current collector with a gradient multilayer metal layer as described in any one of claims 1 to 3, characterized in that: Includes the following steps: (1) The flexible insulating film is placed in the vacuum chamber of the vacuum evaporation and winding coating machine and subjected to plasma surface pretreatment; (2) An adhesive layer is deposited on the surface of the insulating film material by vacuum evaporation deposition; (3) A first metal layer is deposited on the surface of the insulating film with the already deposited adhesive layer by vacuum evaporation deposition; (4) By adjusting the wire feeding speed, winding speed and cooling temperature of the vacuum evaporation coating boat, step (3) is repeated to sequentially deposit multiple metal layers of different thicknesses and grain sizes to form a metal composite layer and obtain the final product. In step (2), the process parameters for vacuum evaporation plating are: the wire feeding speed of the evaporation boat is 100 to 150 mm / min, the winding speed is 120 to 180 m / min, and the cooling temperature is not lower than 10°C. In step (3), the process parameters for vacuum evaporation deposition are: the wire feeding speed of the evaporation boat is 50 to 150 mm / min, the winding speed is 150 to 250 m / min, and the cooling temperature is 40 to 60 °C. In step (4), the method for adjusting the wire feeding speed, winding speed and cooling temperature of the evaporation boat for vacuum evaporation coating is as follows: the wire feeding speed of the evaporation boat is gradually increased, but not higher than 700 mm / min; the winding speed is gradually decreased, but not lower than 30 m / min; the cooling temperature is gradually decreased, but not lower than 0°C.
Citation Information
Patent Citations
Negative current collector, negative pole piece, electrochemical device, and electric vehicle and electronic product comprising electrochemical device
CN113363499A
Preparation method of negative electrode composite current collector and product prepared by preparation method
CN114678534A