Composite carbon material, and preparation method and application thereof

By using a composite material of activated carbon and soft carbon coating, the specific capacity and cycle stability problems of sodium-ion battery anode materials have been solved, realizing the preparation of high-capacity, high-rate, and low-cost sodium-ion battery anode materials suitable for sodium-ion batteries.

CN116936765BActive Publication Date: 2026-11-24SHENZHEN INST OF ADVANCED TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310958180.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-31
Publication Date
2026-11-24
Estimated Expiration
2043-07-31

AI Technical Summary

Technical Problem

Existing carbon-based anode materials for sodium-ion batteries suffer from low specific capacity, low initial coulombic efficiency, poor cycle stability and rate performance, and are also costly and complex to manufacture, making it difficult to achieve both high capacity and high rate performance.

Method used

A composite material of activated carbon and soft carbon coating is used. By coating the surface of activated carbon with a soft carbon layer, abundant active pores for sodium storage are formed. By utilizing the advantages of both activated carbon and soft carbon, structural stability and efficient sodium storage are achieved.

Benefits of technology

It improves the specific capacity, initial coulombic efficiency, and cycle stability of sodium-ion batteries, reduces the manufacturing cost, is suitable for large-scale production, and has high energy density and good electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116936765B_ABST
    Figure CN116936765B_ABST
Patent Text Reader

Abstract

This invention discloses a composite carbon material, its preparation method, and its application. The composite carbon material comprises activated carbon and a soft carbon layer coating the surface of the activated carbon. The activated carbon is selected from at least one of coal-based activated carbon, coconut shell activated carbon, and bamboo charcoal activated carbon. The soft carbon layer includes sodium storage active pores, and is prepared by melting a soft carbon precursor, coating it onto the surface of the activated carbon, and then calcining it once. This material is not only simple and environmentally friendly to prepare, with low raw material costs, but also has a small specific surface area, abundant sodium storage active pores, and a stable structure. Furthermore, it can fully utilize the matrix and mass transfer functions of activated carbon, the fluidity of the soft carbon precursor, and the activity of the soft carbon, effectively converting the surface of the activated carbon into sodium storage active pores. Sodium-ion batteries made using this material as a negative electrode active material exhibit advantages such as high specific capacity, high initial coulombic efficiency, good cycle reversibility, good long-term cycle stability, and excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrode materials and battery technology, specifically relating to a composite carbon material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries are widely used in electric vehicles, computers, mobile phones, and other electronic products, and the demand for lithium is increasing year by year. However, global lithium reserves are extremely limited, and the high price, high cost, and difficulty in recycling limit the development of low-cost, large-scale energy storage devices. Sodium's outermost electron structure is similar to that of lithium, thus possessing similar electrochemical performance. Furthermore, it is abundant and inexpensive, making it the next generation of commercially viable rechargeable batteries after lithium-ion batteries. Currently, sodium-ion batteries can achieve energy densities close to those of lithium-ion batteries, but at a significantly lower cost.

[0003] Currently, common anode materials for sodium-ion batteries fall into four main categories: carbon-based, titanium-based, organic, and alloy-based. Among them, titanium-based oxides, metal oxides, sulfides, and phosphides exhibit good cycle performance but have very low specific capacity. Organic composites can achieve the reversible capacity required for applications, but they suffer from low conductivity and low initial coulombic efficiency. Relatively speaking, carbon-based anode materials are the most commercially viable.

[0004] Among carbon-based anode materials, hard carbon is considered a widely studied type of anode material for sodium-ion batteries due to its specific capacity, which can generally reach 300 mAh / g. CN 108682815 A typically describes the preparation of hard carbon through the carbonization of biomass such as dandelion, London plane tree, foxtail grass, rabbit's tail grass, and Penicillium. CN 109742383 A describes the preparation of hard carbon using polymers of chemical products such as phenol-phenolic resin, m-diphenol-formaldehyde resin, p-diphenol-formaldehyde resin, and phenol-furfural resin as raw materials. CN 115566145 A proposes a method for preparing anode materials for sodium-ion batteries and a sodium-ion battery. This method utilizes a composite of cobalt tetroxide and carbon nanotubes. The cobalt tetroxide-filled carbon nanotube composite material exhibits significant structural advantages. The tubular structure not only provides active sites for sodium ion storage and ensures the uniform distribution of cobalt tetroxide, but also provides a large buffer space for the volume expansion of cobalt tetroxide, dispersing the stress caused by volume changes and improving the battery cycle performance, etc. However, existing carbon-based anode materials for sodium-ion batteries include hard carbon, soft carbon, graphene, carbon nanotubes, and their composites. However, due to the high cost and low sodium storage capacity of carbon materials such as carbon nanotubes and graphene, large-scale and practical applications are difficult to achieve. Furthermore, although hard carbon utilizes its disordered carbon layer structure and defective active sites to store sodium, it suffers from low initial efficiency and cannot simultaneously achieve high rate capability and high capacity.

[0005] Therefore, existing carbon-based anodes still have defects and problems such as the need for hetero-elements and transition metal elements, high preparation cost, complex process, low initial coulombic efficiency, poor structural stability and electrochemical long-cycle stability, and the inability to simultaneously achieve high capacity and high rate capability.

[0006] Therefore, there is an urgent need to develop a composite carbon material that is simple to prepare, low in cost, environmentally friendly, simple in composition, structurally stable, and has stable electrochemical performance. Summary of the Invention

[0007] In order to overcome the problems of low specific capacity of carbon-based anodes and low initial coulombic efficiency of sodium-ion batteries, poor cycle stability and rate performance of sodium-ion batteries, and high cost in existing technologies, one of the objectives of this invention is to provide a composite carbon material.

[0008] In order to solve the problems of complex preparation process, expensive raw materials, multiple components, pollution and high toxicity in the existing technology, the second objective of the present invention is to provide a method for preparing composite carbon materials.

[0009] The third objective of this invention is to provide applications of the aforementioned composite carbon materials.

[0010] The inventive concept of this invention: This invention provides a composite carbon material comprising activated carbon with a rich pore structure on its surface and a soft carbon coating layer supported on the surface of the activated carbon, thereby utilizing the respective advantages of activated carbon and soft carbon to work together to obtain a structurally stable negative electrode active material with a rich sodium storage active pore structure on its surface.

[0011] Meanwhile, activated carbon is a typical amorphous carbon, with long-range disorder in its carbon layers and a rich porous structure on its surface. Soft carbon can transform into a graphite structure at high temperatures. This invention provides a method for preparing a composite carbon material using soft carbon coated with activated carbon, which can be used as a negative electrode for sodium-ion batteries. At the calcination temperature in the embodiments of this invention, the carbon layers of soft carbon are short-range ordered, and after covering the surface of activated carbon, ineffective pores can be transformed into sodium storage active pores. After solvated sodium ions migrate to the sodium storage active pore interface of the composite carbon material, a desolvation reaction occurs. Solvent molecules in the electrolyte are blocked outside the pores, continuing to transport the next batch of sodium ions. The sodium ions that enter the pores gain electrons during the electrochemical reaction and are stored in the pores in the form of sodium clusters. Therefore, the assembled sodium-ion battery also has high initial coulombic efficiency and cycle stability.

[0012] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0013] In a first aspect, the present invention provides a composite carbon material comprising activated carbon and a soft carbon layer coated on the surface of the activated carbon;

[0014] The activated carbon is selected from at least one of coal-based activated carbon, coconut shell activated carbon, and bamboo-based activated carbon (bamboo charcoal activated carbon).

[0015] The soft carbon layer includes sodium storage active pores, and the soft carbon layer is prepared by melting a soft carbon precursor, coating it onto the surface of activated carbon, and then calcining it once.

[0016] In some embodiments, the composite carbon material consists of activated carbon and a soft carbon layer coating the surface of the activated carbon.

[0017] In some embodiments, the activated carbon is selected from at least one of coal-based activated carbon and coconut shell activated carbon.

[0018] In some embodiments, the soft carbon precursor is selected from at least one of mesophase pitch, medium-temperature pitch, low-temperature pitch, high-temperature pitch, coal tar pitch, aromatic coal pitch, ethylene tar pitch, coal pitch, petroleum coke, needle coke, coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

[0019] In some preferred embodiments, the soft carbon precursor is selected from at least one of mesophase pitch, medium-temperature pitch, aromatic coal pitch, ethylene tar pitch, petroleum coke, needle coke, coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

[0020] In some embodiments, the sodium storage active pore is a semi-closed pore, and the pore size of the sodium storage active pore is 0.1 to 30 nm.

[0021] Specifically, sodium storage active pores with a pore size of 0.1–30 nm are beneficial for sodium transport and storage.

[0022] In some preferred embodiments, the pore size of the sodium storage active pore is approximately 1 nm.

[0023] Specifically, the composite carbon material prepared by this invention has abundant sodium storage active pores (reflected in the long plateau capacity in BET tests and charge-discharge curves), which can store sodium ions with high capacity and high rate, and greatly improves the problem of electrolyte decomposition.

[0024] In some embodiments, the mass ratio of the soft carbon precursor to activated carbon is 1:3 to 3:1.

[0025] In some preferred embodiments, the mass ratio of the soft carbon precursor to activated carbon is 1:1 to 2:1.

[0026] In some embodiments, the specific surface area of ​​the composite carbon material is ≤20m². 2 / g.

[0027] In some preferred embodiments, the specific surface area of ​​the composite carbon material is 1 to 10 m². 2 / g.

[0028] In some preferred embodiments, the specific surface area of ​​the composite carbon material is 2–6 m². 2 / g.

[0029] In some embodiments, the specific surface area of ​​the activated carbon is 500 m². 2 / g~3200m 2 / g.

[0030] In some preferred embodiments, the specific surface area of ​​the activated carbon is 800 m². 2 / g~2500m 2 / g.

[0031] In some preferred embodiments, the specific surface area of ​​the activated carbon is 1200 m². 2 / g~1800m 2 / g.

[0032] In some embodiments, the activated carbon has a porous structure with a pore size of 0.1 nm to 5 μm.

[0033] In a second aspect, the present invention provides a method for preparing the composite carbon material described in the first aspect, comprising the following steps:

[0034] S1: After mixing the activated carbon and dispersant, add the soft carbon precursor and mix, then heat until the soft carbon precursor melts to obtain an intermediate.

[0035] S2: The intermediate is calcined in an inert atmosphere to obtain a composite carbon material.

[0036] In some embodiments, in step S1, the activated carbon is selected from at least one of coal-based activated carbon, coconut shell activated carbon, and activated carbon with bamboo as the carbon source.

[0037] In some embodiments, in step S1, the dispersant is selected from at least one of ethanol, deionized water, methanol, ethylene glycol, glycerol, acetone, benzene, toluene, diethyl ether, and tetrahydrofuran.

[0038] In some preferred embodiments, in step S1, the dispersant is selected from at least one of ethanol, deionized water, methanol, ethylene glycol, and glycerol.

[0039] In some embodiments, in step S1, the soft carbon precursor is selected from at least one of mesophase pitch, medium-temperature pitch, low-temperature pitch, high-temperature pitch, coal tar pitch, aromatic coal pitch, ethylene tar pitch, coal pitch, petroleum coke, needle coke, coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

[0040] In some preferred embodiments, in step S1, the soft carbon precursor is selected from at least one of mesophase pitch, medium-temperature pitch, aromatic coal pitch, ethylene tar pitch, petroleum coke, needle coke, coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

[0041] In some embodiments, in step S1, the mass ratio of the soft carbon precursor to activated carbon is 1:3 to 3:1.

[0042] In some preferred embodiments, in step S1, the mass ratio of the soft carbon precursor to activated carbon is 1:1 to 2:1.

[0043] In some embodiments, in step S1, the mass ratio of the activated carbon to the volume ratio of the dispersant is 0.01 to 0.5 g / mL.

[0044] In some embodiments, the heating process in step S1 further includes a stirring step.

[0045] In some embodiments, the heating temperature in step S1 is 30–80°C.

[0046] In some embodiments, the heating time in step S1 is 1 to 20 hours. Preferably, the heating time is 5 to 15 hours.

[0047] In some embodiments, a drying step is also included in step S2 before calcination.

[0048] In some embodiments, in step S2, the inert atmosphere is selected from at least one of nitrogen, argon, and neon.

[0049] In some embodiments, in step S2, the heating rate of the calcination is 2°C / min to 10°C / min.

[0050] In some preferred embodiments, the calcination heating rate is 5°C / min.

[0051] In some embodiments, the calcination temperature in step S2 is 500°C to 1900°C.

[0052] In some preferred embodiments, the calcination temperature in step S2 is 700℃ to 1600℃. Specifically, the calcination temperature can be 700℃ to 1000℃ or 1300℃ to 1500℃.

[0053] In some more preferred embodiments, in step S2, the calcination temperature is 1000°C to 1400°C.

[0054] In some embodiments, the calcination time in step S2 is 0.5h to 10h.

[0055] In some preferred embodiments, the calcination time in step S2 is 1 to 10 hours; specifically 1 hour, 3 hours, 5 hours, 7 hours, and 10 hours.

[0056] Specifically, this invention selects activated carbon with suitable specific surface area and pore size distribution, a soft carbon precursor with high flowability and coating effect, controls the mass ratio of soft carbon precursor to activated carbon, and achieves composite and uniform mixing of activated carbon and soft carbon precursor through a simple process. Medium-high temperature calcination (one-time calcination) achieves a composite structure of soft carbon coating activated carbon, thereby transforming exposed ineffective pores into high-capacity, highly reversible sodium storage active pores. Furthermore, the preparation process of this invention is not only simple, pollution-free, and low-cost, suitable for large-scale production, but also produces sodium-ion batteries with advantages such as high energy density, high initial coulombic efficiency, and good cycle stability.

[0057] Thirdly, the present invention provides a negative electrode slurry comprising the composite carbon material described in the first aspect.

[0058] In some embodiments, the negative electrode slurry further includes a binder and carbon black, and the mass ratio of the composite carbon material, binder and carbon black is (5-10):1:1.

[0059] In some embodiments, the adhesive is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polymethyl methacrylate, polyacrylonitrile, polyimide, polyvinylpyrrolidone, polyethylene oxide, polyvinyl alcohol, sodium carboxymethyl cellulose, styrene-butadiene rubber, and gelatin.

[0060] In some embodiments, the negative electrode slurry further includes a solvent for the binder.

[0061] In some embodiments, the solvent of the adhesive is selected from at least one of methanol, ethanol, propanol, glycerol, N-methylpyrrolidone, dimethyl sulfoxide, tetrahydrofuran, and N,N-dimethylformamide.

[0062] Fourthly, the present invention provides a composite carbon material for the negative electrode as described in the first aspect.

[0063] In some embodiments, the negative electrode further includes a current collector. Preferably, the current collector is one or more of aluminum and copper.

[0064] In some embodiments, the effective loading of the negative electrode is 1–5 mg / cm³. 2 .

[0065] In some preferred embodiments, the effective loading of the negative electrode is approximately 2 mg / cm³. 2 .

[0066] Specifically, the above-mentioned effective loading amount refers to the effective loading amount of the negative electrode active material.

[0067] Fifthly, the present invention provides a sodium-ion battery comprising the negative electrode described in the fourth aspect.

[0068] In some embodiments, the sodium-ion battery further includes: using metallic sodium as the negative electrode and using carbonate-sodium salt or ether-sodium salt as the electrolyte.

[0069] In some preferred embodiments, the electrolyte in the electrolyte is at least one of NaPF6 and NaClO4.

[0070] In some preferred embodiments, the solvent in the electrolyte is at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethylene glycol dimethyl ether (DEGDME), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC).

[0071] In some preferred embodiments, the electrolyte comprises: a carbonate-sodium salt or ether-sodium salt electrolyte of 0.5 to 4 mol / L.

[0072] The beneficial effects of this invention are as follows: The composite carbon material of this invention not only has a simple composition and low raw material cost, but also possesses abundant sodium storage active pores, a small specific surface area, and a stable structure. Furthermore, it can fully utilize the matrix and mass transfer functions of activated carbon, the fluidity of the soft carbon precursor, and the inherent advantages of soft carbon itself, making it particularly suitable for use as a negative electrode active material. Due to the large specific surface area of ​​activated carbon and the enhanced fluidity of the soft carbon precursor during heating, conditions are created for effectively coating the surface of activated carbon and obtaining abundant sodium storage active pores.

[0073] The method for preparing composite carbon materials of the present invention relies solely on heating, melting, mixing, and a single medium-high temperature calcination to uniformly cover the porous surface of activated carbon with soft carbon, thereby achieving the coating of activated carbon and converting the ineffective pores on the surface of activated carbon into sodium storage active pores, resulting in a composite carbon material with abundant sodium storage active pores. Therefore, this method is characterized by its simple process, environmental friendliness, and low cost, making it suitable for large-scale production and practical applications.

[0074] Because the composite carbon material has a good coating effect, abundant sodium storage active pores, small specific surface area, and stable structure, the sodium-ion battery made by using the composite carbon material of the present invention as the negative electrode active material has advantages such as large specific capacity, high initial coulombic efficiency, good cycle reversibility, good long cycle stability, and excellent rate performance.

[0075] Specifically:

[0076] (1) This invention can solve the problems of low anode capacity of existing sodium-ion batteries (the specific capacity of most commercial hard carbon batteries is below 350mAh / g), low initial coulombic efficiency (hard carbon itself has a rich pore structure, and the electrolyte is prone to decomposition on the surface during the first charge and discharge process, resulting in side reactions, and some intercalation and pore filling capacity cannot be reversibly released, resulting in low initial coulombic efficiency), poor rate performance (the kinetic performance of the capacity of the plateau region of conventional hard carbon anode is poor, and the degree of irreversibility is large under high current, so the capacity decay is serious at high rate), and poor cycle stability (the intercalation, pore filling and adsorption capacity of hard carbon has a certain degree of irreversibility, especially the capacity decay is fast under high current, and the cycle stability needs to be improved).

[0077] (2) The innovation of this invention lies in using inexpensive activated carbon as a raw material to soft-coat the porous surface of the activated carbon. Based on the derived sodium storage active pores, the plateau capacity of the carbon anode of sodium-ion batteries is significantly improved. Due to the large and dense pore size range on the surface of activated carbon, high-speed sodium exchange can be achieved between the derived sodium storage active pores, improving sodium ion transport kinetics and thus enhancing the rate performance of sodium-ion batteries. After soft carbon coating, solvated ion clusters desolvate on the surface of the active pores (i.e., sodium storage active pores), greatly reducing the decomposition of electrolyte solvent molecules and the occurrence of side reactions, thereby improving the initial coulombic efficiency and cycle stability of sodium-ion batteries.

[0078] The sodium-ion half-cell assembled by this invention achieves an initial coulombic efficiency of 90.5%, and the composite carbon prepared by the preferred scheme achieves a specific capacity of 419 mAh / g. After increasing the charge / discharge rate from 0.1C to 5C, the capacity retention reaches 75%, and after decreasing it back to 0.1C, the capacity recovers to 400 mAh / g, demonstrating good rate performance.

[0079] (3) The composite carbon material of the present invention has a simple preparation process, abundant and inexpensive raw materials, no environmental pollution, is suitable for large-scale production, conforms to the sustainable development strategy and green economy principle, and can be widely used in the field of energy storage. Attached Figure Description

[0080] Figure 1 This is a schematic diagram of the structure of the composite carbon material in this invention;

[0081] Figure 2 SEM images of the coal-based activated carbon and composite carbon materials in Example 1;

[0082] Figure 3 The nitrogen adsorption / desorption curves and pore size distribution of the coal-based activated carbon in Comparative Example 1 are shown.

[0083] Figure 4 The diagram shows the nitrogen adsorption / desorption curves and pore size distribution of the composite carbon material in Example 1.

[0084] Figure 5 The following are small-angle X-ray diffraction patterns of the composite carbon materials in Examples 1, 108, and 127;

[0085] Figure 6 The XRD patterns of the composite carbon material, activated carbon, and soft carbon in Example 1 are shown.

[0086] Figure 7 The constant current charge-discharge curve of the sodium-ion battery made from the composite carbon material in Example 1 under 0.1C conditions.

[0087] Figure 8 The image shows the long-cycle curve of a sodium-ion battery made with the composite carbon material as the negative electrode material in Example 1 at 0.1C.

[0088] Figure 9 The graph shows the rate performance test curve of a sodium-ion battery made using the composite carbon material as the negative electrode material in Example 1. Detailed Implementation

[0089] The present invention will be further described in detail below through specific embodiments.

[0090] The composite carbon material prepared by this invention utilizes coal-based activated carbon and biomass-based activated carbon with different specific surface areas as the matrix; and uses petrochemical and coal chemical byproducts such as asphalt and anthracite as soft carbon precursors. The composite structure of soft carbon-coated activated carbon is achieved through a one-step calcination at medium and high temperatures. The raw material cost is low and there is no pollution. The specific capacity, cycle performance and first coulombic efficiency of the prepared composite carbon anode material are all improved, making it particularly suitable for use as a high-performance sodium-ion battery anode.

[0091] Furthermore, the preparation process of this invention is simple and the equipment cost is low, making it suitable for large-scale production. The emergence of sodium-ion batteries not only alleviates the problems of limited and high-cost lithium-ion resources, but also provides simple, inexpensive, readily available, environmentally friendly, and safe positive and negative electrode materials. The production process is simple and low-cost, making it a sodium-ion battery that combines high specific capacity, high cycle performance, and high safety.

[0092] A schematic diagram of the structure of the composite carbon material in this invention is shown below. Figure 1 As shown.

[0093] Depend on Figure 1 It is understood that the composite carbon material provided by this invention consists of activated carbon particles and a soft carbon layer uniformly coated on the surface of the activated carbon particles. This effectively modifies the exposed ineffective pores on the activated carbon surface, transforming them into high-capacity, highly reversible sodium storage active pores (semi-closed pores with a pore size of approximately 0.1–30 nm). This synergistically leverages the pore structure of the activated carbon particles as the matrix and the inherent advantages of soft carbon. Furthermore, this invention enables the preparation of low-cost, simple-composition, structurally stable, and electrochemically excellent composite carbon materials without the need for additional metal or heteroatom doping, making it particularly suitable for use as a negative electrode active material in sodium-ion batteries.

[0094] Example 1

[0095] This embodiment provides a method for preparing a composite carbon material, including the following steps:

[0096] S1: Disperse 1g of activated carbon particles in a dispersant, gradually add 1g of soft carbon precursor, continue heating to 70℃ and stirring for 10 hours to obtain an intermediate;

[0097] S2: After drying the intermediate at 65℃ to constant weight, it was placed in a tube furnace and calcined at 1300℃ for 5 hours under an argon atmosphere (heating rate: 5℃ / min) to obtain the composite carbon material.

[0098] In step S1, the activated carbon particles are coal-based activated carbon, specifically coal-based-1600, with a Langmuir specific surface area of ​​1600±50 m². 2 / g; the dispersant is ethanol, and the amount of dispersant used is 20mL; the soft carbon precursor is mesophase pitch.

[0099] This embodiment provides a method for preparing a negative electrode slurry and a sodium-ion battery half-cell, including the following steps:

[0100] 1) The composite carbon material of this embodiment is mixed with polyvinylidene fluoride (PVDF binder, solid) and conductive carbon black (SP conductive agent) in a mass ratio of 8:1:1. After grinding for 30 minutes, N-methylpyrrolidone (NMP) is added and stirred until it becomes a paste to obtain the negative electrode slurry.

[0101] 2) The negative electrode slurry was coated onto a carbon-coated aluminum foil measuring 15cm × 25cm to prepare the electrode, with an effective loading of approximately 2mg / cm². 2 A sodium-ion battery half-cell was assembled using a sodium sheet as the counter electrode and NaPF4 carbonate electrolyte.

[0102] The NaPF4 carbonate electrolyte is composed of an electrolyte and a solvent; the concentration of the electrolyte NaPF4 is 1 mol / L; the solvent is a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1.

[0103] In the negative electrode slurry, the amount of N-methylpyrrolidone (NMP) added is 3 mL (N-methylpyrrolidone) / g.

[0104] Characterization and performance testing:

[0105] 1. A scanning electron microscope (SEM) image of the coal-based activated carbon in Example 1 at a magnification of 3700, as shown below. Figure 2 As shown in (a); SEM images of the composite carbon material of Example 1 measured at different magnifications are shown in Figure 1. Figure 2 As shown in (b) and (c) in the figure.

[0106] Depend on Figure 2 It can be seen that: in Figure 2 (a) shows that coal-based activated carbon has a very obvious macroporous structure (pore size > 50 nm, mainly micron-sized macropores, especially micron-sized macropores with pore sizes of 1–5 μm). Although these macropores can improve kinetics and facilitate mass transport, these pores are ineffective sodium storage pores and are also prone to electrolyte decomposition.

[0107] It should be noted that the sodium storage active pores are pores with a diameter of approximately 0.1–30 nm (preferably 1 nm). Due to the small pore size, the active pores cannot be well characterized by the precision of SEM and BET tests. However, the electrochemical performance demonstrates that the composite carbon material of Example 1 possesses abundant sodium storage active pores. The mesophase pitch, as a soft carbon precursor, can deposit and coat the surface of the activated carbon pores (0.1 nm–5 μm in diameter) after carbonization, transforming the micropores in the activated carbon into sodium storage pores and inhibiting the decomposition of the electrolyte on the surface of the mesopores and macropores of the activated carbon.

[0108] Figure 2 (b) and (c) show that the number of macropores on the surface of the composite carbon material provided in Example 1 is significantly reduced, and a layer of soft carbon material covers the surface of the macropores, thereby effectively modifying the surface structure of activated carbon, transforming ineffective pores into pores that can store sodium, and reducing the decomposition of electrolyte.

[0109] 2. The nitrogen adsorption / desorption curves and pore size distribution diagrams of the coal-based activated carbon in Comparative Example 1 are shown below. Figure 3As shown in (a) and (b) in Example 1, the nitrogen adsorption / desorption curves and pore size distribution diagrams of the composite carbon material are respectively shown in (a) and (b). Figure 4 As shown in (a) and (b) in the figure.

[0110] Depend on Figure 3 and Figure 4 It can be known that: Figure 3 (a) shows that coal-based activated carbon (coal-based-1600 activated carbon) was analyzed using different analytical methods. The specific surface area of ​​the coal-based activated carbon (coal-based-1600 activated carbon) was determined to be 1402.55 m² using single-point BET surface area analysis. 2 / g; the specific surface area measured by the multi-point BET surface area method was 1435.21m². 2 / g; Langmuir specific surface area (i.e., Langmuir surface area) is 1671.32m². 2 / g; t-plot microporous specific surface area is 1198.65m² 2 / g. Based on the nitrogen desorption curve, the pore size distribution was obtained using the Harkins & Jura method. Figure 3 (b) Figure 3 (b) shows that the pore size of coal-based-1600 activated carbon is mainly distributed in the range of 1 to 50 nm, that is, its pores are mainly micropores and mesopores.

[0111] Figure 4 (a) shows that the composite carbon material of Example 1 was analyzed using different analytical methods. The specific surface area of ​​the composite carbon material of Example 1 was determined to be 3.76 m² using single-point BET surface area analysis. 2 / g; the specific surface area measured by the multi-point BET surface area method is 3.80m². 2 / g; Langmuir specific surface area (i.e., Langmuir surface area) is 2.78m². 2 / g; t-plot microporous specific surface area is 5.78m². 2 / g. Based on the nitrogen desorption curve, the pore size distribution was obtained using the Harkins & Jura method. Figure 4 (b) Figure 4 (b) shows that after high-temperature coating with soft carbon, the original micropores of the activated carbon become sodium storage pores. Because the soft carbon covers the pore surface, these pores cannot be identified in the BET test, and the electrolyte will not decompose on the surface of these sodium storage pores to form an SEI film. However, due to the inherent porous structure of carbon materials, ... Figure 4 (b) always exhibits a certain pore structure distribution.

[0112] Figure 5The results show that the small-angle X-ray diffraction curves of the composite carbon materials prepared in Examples 1, 108, and 127 all have obvious peaks, corresponding to scattering intensities Q in the range of 0.5–2 nm. -1 The range indicates that all three composite carbons have nanoscale pore size distributions, and these pores were not detected by BET. Examples 1, 127, and 108 are all preferred embodiments, all possessing nanoscale active storage pores (pore size: 0.1–30 nm). Moreover, it is evident that the small-angle X-ray diffraction peaks of the composite carbons prepared in Examples 1, 127, and 108 gradually increase, indicating that their nanoscale active storage pores gradually decrease, and therefore their sodium storage capacity also decreases sequentially.

[0113] 3. The X-ray diffraction (XRD) spectra of the soft carbon, the composite carbon material in Example 1, and the coal-based activated carbon obtained by calcining the soft carbon precursor mesophase pitch raw material in Example 1 at 1300℃ for 5 hours under an argon atmosphere are shown below. Figure 6 As shown.

[0114] Depend on Figure 6 It can be seen that, compared with composite carbon and soft carbon, activated carbon has a flatter (002) peak near 24°, indicating that its carbon layer has a high degree of disorder in the c-axis direction. After soft carbon coating and high-temperature calcination, the (002) peak becomes sharper, indicating that the carbon layer structure of composite carbon has increased in order. It should be noted that both soft carbon and activated carbon are amorphous carbon, but their carbon layer order and surface morphology differ, and their effects on sodium ion storage and transport are also different.

[0115] 4. Electrochemical performance testing:

[0116] The sodium half-cell provided in Example 1 was subjected to charge-discharge tests at different rates and long-cycle tests at 0.1C. The number of cycles in which the capacity decreased to 80% during the long-cycle tests was recorded. Simultaneously, the remaining Examples 2-141, Comparative Examples 1, and Comparative Examples 3-9 were subjected to charge-discharge tests at different rates using the same test methods and conditions, and long-cycle tests were conducted at 0.1C. The number of cycles in which the capacity decreased to 80% during the long-cycle tests was recorded.

[0117] Unless otherwise specified, the examples and comparative examples in this invention all measured their initial coulombic efficiency at a rate of 0.1C and a charge-discharge condition of 0.001-2V. The specific electrochemical performance measured is shown in Tables 1-9. Figures 7-9 As shown.

[0118] The rate performance test curve of the sodium-ion battery made with the composite carbon material as the negative electrode material in Example 1 is shown in the figure. Figure 9 As shown; the constant current charge-discharge curve of the sodium-ion battery made from the composite carbon material in Example 1 under 0.1C conditions is shown in the figure. Figure 7 As shown; the long-cycle curve of the sodium-ion battery made with the composite carbon material as the negative electrode material in Example 1 at 0.1C is as follows. Figure 8 As shown.

[0119] Depend on Figure 7 , Figure 8 , Figure 9 As shown in Table 9, the sodium-ion battery of Example 1 had a specific capacity of 419 mAh / g measured under constant current charge-discharge at 0.1C and a specific capacity of 388 mAh / g measured under constant current charge-discharge at 0.5C. The initial coulombic efficiency was 90.5% measured at 0.1C.

[0120] Meanwhile, during long-cycle testing at 0.1C, the number of cycles required for the capacity to decay to 80% was measured to be 2109.

[0121] Further analysis, Figure 7 The sodium-ion half-cell prepared by the composite carbon material in Example 1 has a plateau capacity of sodium storage in the pores below 0.1V. Sodium is stored in the form of sodium clusters in the nanopores, and the capacity is provided by the sodium storage active pores of the composite carbon. Therefore, the plateau capacity in the constant current charge-discharge curve of Example 1 of the present invention reaches more than 300mAh / g.

[0122] BET test and long platform capacity test results in charge-discharge curve ( Figure 4 and Figure 7 This demonstrates that the composite carbon material prepared by this invention has abundant sodium storage active pores.

[0123] also, Figure 9 This indicates that the composite carbon material of Example 1 has excellent rate performance and good electrochemical stability.

[0124] Examples 2 to 21

[0125] The preparation methods of the composite carbon materials, negative electrode slurry and sodium-ion battery half-cells in Examples 2 to 21 differ from those in Example 1 only in the type of activated carbon used; all other contents can be found in Example 1.

[0126] Test conditions and methods for the electrochemical performance of the negative electrode:

[0127] The composite carbon materials were assembled into sodium-ion battery half-cells according to the method in Example 1. Specifically:

[0128] (1) Test conditions for rate performance: The current was charged and discharged for 10 cycles at current densities of 0.1C, 0.5C, 1C, 2C and 5C respectively, and then returned to 0.1C for long cycle. The specific capacity under 0.1C and 0.5C conditions was recorded at the same time.

[0129] (2) Test conditions for the first coulomb efficiency: The coulomb efficiency was measured during the first charge-discharge cycle at 0.1C.

[0130] (3) Long cycle test conditions: The number of cycles at which the capacity decays to 80% is measured under constant current of 0.1C.

[0131] The types of activated carbon used in Examples 1 to 21 and the electrochemical performance of the negative electrode after assembly into a sodium-ion battery are shown in Table 1.

[0132] Table 1. Parameters of activated carbon and performance of sodium-ion batteries in Examples 1-21

[0133]

[0134]

[0135] Note: The composite carbon materials of the negative electrode in Table 1 all use mesophase pitch as soft carbon precursor, and the mass ratio of activated carbon to soft carbon precursor is 1:1 during the preparation process.

[0136] The specific surface area in Table 1 is the reference value given by the purchased activated carbon. Due to differences in the accuracy of specific surface area testing instruments, differences in testing environments, and theoretical differences in obtaining specific surface area based on nitrogen adsorption-desorption, the specific surface area measured in this invention may differ to some extent from the given reference value of the product. However, the values ​​are at the same level and are within the normal range of difference.

[0137] As shown in Table 1, different types of activated carbon have a significant impact on the performance of composite carbon anodes, mainly due to differences in their specific surface area and microstructure. Activated carbon prepared from different activated carbon precursors exhibits considerable differences in microstructure. While the specific surface area and pore size distribution of activated carbon can be controlled through different pore-forming processes and parameters, as an anode material, a higher specific surface area is not always better; the stability of the material must also be considered.

[0138] In contrast, the specific surface area prepared using coconut shells in Example 5 was 1500 ± 50 m². 2 / activated carbon (coconut shell-1500), and the specific surface area of ​​coal prepared in Example 1 with a specific surface area of ​​1600±50m². 2 Composite carbon materials prepared from activated carbon (coal-based-1600) at a concentration of / g are preferred embodiments for use as anode materials. They not only exhibit good electrochemical performance in sodium-ion batteries, but also demonstrate excellent electrochemical stability.

[0139] In summary, one of the key aspects of this invention lies in the type of activated carbon. Examples 1-21 demonstrate that the specific surface area of ​​the activated carbon is 1200-1800 m². 2Coal-based activated carbon with a yield of / g has good electrochemical performance and stability (including structural stability and electrochemical stability), and coconut shell-1500 and coal-based-1600 activated carbon are preferred activated carbon raw materials.

[0140] The purpose of this invention is to utilize soft carbon to coat activated carbon, transforming the exposed ineffective pores on the surface into high-capacity, highly reversible sodium storage active pores. Therefore, another key aspect of this invention is the use of soft carbon to coat activated carbon. The key to this step lies in the joint control of process parameters such as the type of soft carbon precursor, the ratio of activated carbon to soft carbon precursor, and temperature, in order to achieve the goal of transforming the exposed ineffective pores on the surface of activated carbon into high-capacity, highly reversible sodium storage active pores.

[0141] Examples 22 to 27

[0142] The preparation methods of composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 22, 24 and 26 differ from those in Example 1 only in the mass ratio of soft carbon precursor and activated carbon used. All other contents can be found in Example 1.

[0143] The preparation methods of composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 23, 25 and 27 differ from those in Example 5 only in the mass ratio of soft carbon precursor and activated carbon used. All other contents can be found in Example 5.

[0144] The electrochemical performance testing conditions for Examples 22–27 were the same as those for Example 1;

[0145] The mass ratio of soft carbon precursor to activated carbon used in Examples 22 to 27, and the electrochemical performance of the sodium-ion battery half-cell or negative electrode are shown in Table 2.

[0146] Table 2 shows the performance of sodium-ion batteries in Examples 1, 5, and 22-27.

[0147]

[0148] Note: The examples in Table 2 all use mesophase pitch as a soft carbon precursor.

[0149] As can be seen from Table 2, the composite carbon materials prepared by using different mass ratios of mesophase pitch and activated carbon affect the effect of soft carbon coating of activated carbon and the transformation of the activated carbon surface structure into sodium storage pores, which in turn affects the specific capacity, initial coulombic efficiency, rate performance and long-cycle stability of the composite carbon material as a negative electrode in sodium-ion batteries.

[0150] When the mass ratio of soft carbon precursor to activated carbon is 1:2 to 1:3, the initial coulombic efficiency and capacity in Examples 22 to 25 are all low. This is mainly because the content of soft carbon is too low and is not enough to completely cover the pores on the surface of activated carbon. It is necessary to further increase the mass ratio of soft carbon precursor.

[0151] As the proportion of soft carbon precursor increases, the specific capacity, initial coulombic efficiency, and number of cycles before capacity decays to 80% at different current densities show a trend of first increasing and then rapidly decreasing. This indicates that within a certain ratio range (soft carbon precursor to activated carbon mass ratio of 1:3 to 1:1), increasing the mass ratio of soft carbon precursor can improve the coating effect on activated carbon. Furthermore, considering comprehensive electrochemical performance, the preferred mass ratio of mesophase pitch to activated carbon is 2:1 to 1:1.

[0152] However, when the mass ratio of soft carbon precursor to activated carbon was 2:1, the electrochemical performance of Examples 26-27 decreased. This is because excessive soft carbon coating of the precursor reduces the active mass ratio of the composite carbon material, leading to a decrease in sodium storage capacity. Therefore, the optimal mass ratio of soft carbon precursor to activated carbon is 1:1.

[0153] Examples 28 to 54

[0154] The preparation methods of composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 28 to 54 differ from those in Example 1 or Example 5 only in the type of soft carbon precursor used; all other contents can be found in Example 1 or Example 5.

[0155] The electrochemical performance testing conditions for Examples 28 to 54 were the same as those for Example 1;

[0156] The types of soft carbon precursors used in Examples 28 to 54, and the electrochemical performance of the assembled sodium-ion batteries, are shown in Table 3.

[0157] Table 3 Performance of sodium-ion batteries in Examples 1, 5, and 28–54

[0158]

[0159]

[0160] Note: The mass ratio of soft carbon precursor to activated carbon in the examples in Table 3 is 1:1.

[0161] Examples 55 to 79

[0162] The preparation methods of composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 55 to 79 differ from those in Example 1 or Example 5 only in the type of soft carbon precursor used and the mass ratio of soft carbon precursor to activated carbon. All other contents can be found in Example 1 or Example 5.

[0163] The electrochemical performance testing conditions for Examples 55 to 79 were the same as those for Example 1;

[0164] The types of soft carbon precursors used in Examples 55 to 79, the mass ratio of soft carbon precursors to activated carbon, and the electrochemical performance of the assembled sodium-ion batteries are shown in Table 4.

[0165] Table 4. Performance of sodium-ion batteries in Examples 26, 27, and 55–79

[0166]

[0167]

[0168] Note: The mass ratio of soft carbon precursor to activated carbon in the examples in Table 4 is 2:1.

[0169] Examples 80 to 105

[0170] The preparation methods of composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 80 to 105 differ from those in Example 1 or Example 5 only in the type of soft carbon precursor used and the mass ratio of soft carbon precursor to activated carbon. All other contents can be found in Example 1 or Example 5.

[0171] The electrochemical performance testing conditions for Examples 80 to 105 were the same as those for Example 1;

[0172] The types of soft carbon precursors used in Examples 80 to 105, the mass ratio of soft carbon precursors to activated carbon, and the electrochemical performance of the assembled sodium-ion batteries are shown in Table 5.

[0173] Table 5 Performance of sodium-ion batteries in Examples 24, 25, and 80–105

[0174]

[0175] Note: The mass ratio of soft carbon precursor to activated carbon in the examples in Table 5 is 1:2.

[0176] As shown in Tables 3, 4, and 5, when coconut shell-1500 or coal-based-1600 activated carbon is selected, the composite carbon materials of Examples 1, 5, and 22-105 of this invention have a specific capacity of 324-419 mAh / g at 0.1C; a specific capacity of 301-388 mAh / g at 0.5C; an initial coulombic efficiency of 80.6%-90.5%; and 953-2109 cycles before the capacity decays to 80%.

[0177] In contrast, when the mass ratio of soft carbon precursor to activated carbon is 1:1, 2:1, and 1:2, the composite carbon materials prepared using mesophase pitch, aromatic coal pitch, and needle coke as soft carbon precursors exhibit superior electrochemical performance when used as anodes in sodium-ion batteries. Furthermore, considering different types of soft carbon precursors, a 1:1 mass ratio of soft carbon precursor to activated carbon is generally considered the preferred ratio, resulting in composite carbon materials with excellent electrochemical performance and structural stability.

[0178] Based on this, the examples in Table 3 use preferred coconut shell-1500 and coal-1600 as activated carbon, and control the ratio of soft carbon precursor to activated carbon to be 1:1, so that the resulting composite carbon material can have a good coating effect, more effective sodium storage pores and good electrochemical performance.

[0179] Examples 106 to 134

[0180] The preparation methods of the composite carbon materials, negative electrode slurry and sodium-ion battery half cells in Examples 106 to 134 differ from those in Example 1 only in the calcination process parameters, specifically the calcination temperature and calcination time. All other details can be found in Example 1.

[0181] The electrochemical performance testing conditions for Examples 106 to 134 were the same as those for Example 1;

[0182] The calcination process parameters used in Examples 106 to 134, the mass ratio of soft carbon precursor to activated carbon, and the electrochemical performance of the assembled sodium-ion batteries are shown in Table 6.

[0183] Table 6 Performance of sodium-ion batteries in Examples 1, 106-134

[0184]

[0185]

[0186] Note: The soft carbon precursors in the examples in Table 6 are all mesophase pitch, and the activated carbon is all coal-based-1600 activated carbon. The mass ratio of soft carbon precursor to activated carbon is 1:1.

[0187] As shown in Table 6, the calcination temperature and time parameters have a significant impact on the performance of the prepared composite carbon anode. The main reason is that under suitable calcination processes, the soft carbon coating layer structure, defects, and some pore structures are continuously optimized, resulting in a better coating effect. This leads to the formation of high-capacity, highly reversible sodium storage active pores on the activated carbon surface, resulting in a low-cost, structurally stable, and electrochemically excellent composite carbon material suitable for use as a sodium-ion battery anode. In comparison, the preferred calcination process parameters of this invention are: a calcination temperature of 700–1900℃ and a calcination time of 1–10 hours under an argon atmosphere; the optimal calcination process parameters of this invention are: a calcination temperature of approximately 1300℃ and a calcination time of 3–7 hours under an argon atmosphere.

[0188] Examples 135 to 141

[0189] The preparation methods of the composite carbon materials, negative electrode slurry and sodium-ion battery half-cells in Examples 135 to 141 differ from those in Example 1 only in the dispersant; all other contents can be found in Example 1.

[0190] The electrochemical performance testing conditions for Examples 135 to 141 were the same as those for Example 1;

[0191] The types of dispersants used in Examples 135 to 141, and the electrochemical performance of the sodium-ion batteries assembled from them, are shown in Table 7.

[0192] Table 7 Performance of sodium-ion batteries in Examples 1, 135-141

[0193]

[0194] Note: The soft carbon precursors in the examples in Table 7 are all mesophase pitch, the activated carbons are all coal-based-1600 activated carbons, the mass ratio of soft carbon precursors to activated carbons is 1:1, and the calcination process parameters are: argon atmosphere, calcination temperature of 1300℃, and calcination time of 5 hours.

[0195] The soft carbon precursor and activated carbon need to be uniformly dispersed in a system to achieve uniform coating of activated carbon by the soft carbon. It is necessary to select water-soluble or fat-soluble soft carbon precursors, or to mix the two by stirring and evaporating. Therefore, a suitable dispersant is needed to ensure uniform dispersion of activated carbon and soft carbon precursor.

[0196] As can be seen from Table 7, the performance of composite carbon anodes prepared with ethanol, acetone, diethyl ether and tetrahydrofuran as active solvents is not significantly different. However, benzene, toluene, diethyl ether and tetrahydrofuran are highly toxic and expensive. In order to achieve a green, environmentally friendly and low-cost preparation process, ethanol can be selected as the preferred dispersant.

[0197] Comparative Example 1

[0198] This comparative example provides an activated carbon, which is the coal-based activated carbon (coal-based-1600) of Example 1.

[0199] This comparative example provides a method for preparing a negative electrode slurry and a sodium-ion battery half-cell. The only difference between this example and Example 1 is that the composite carbon material is replaced with coal-based activated carbon (coal-based-1600). The performance testing methods are the same as those in Example 1, and the measured performance is shown in Table 8.

[0200] Comparative Example 2

[0201] This comparative example provides a method for preparing a hard carbon anode material, specifically referring to Example 2 of application number 201811631507.1, publication number CN109742383A, entitled "Hard Carbon Anode Material for Sodium-ion Batteries Based on Phenolic Resin and Its Preparation Method and Application"; the method includes the following steps:

[0202] Liquid phenolic resin and ethanol were mixed at a volume ratio of 2:1 and stirred until homogeneous. The mixture of phenolic resin and ethanol was transferred to a reaction vessel and hydrothermally treated at 180°C for 4 hours to cure the phenolic resin. The cured phenolic resin was removed and mechanically ground into granules. The granules were then placed in a tube furnace and heated to 1550°C at a heating rate of 3°C / min. The raw material was subjected to high-temperature treatment for 2 hours under argon protection to cause it to decompose and carbonize. Finally, the material was cooled to room temperature and removed to obtain a hard carbon anode material. The performance of the sodium-ion battery in Example 2 is shown in Table 8.

[0203] Comparative Example 3

[0204] This comparative example provides a method for preparing a composite carbon material, which differs from Example 1 of the present invention only in that: the coal-based activated carbon is replaced with chitosan from Example 4 of CN115911320A. The rest of the preparation process and parameters, the preparation of sodium-ion half-cells and the electrochemical performance testing methods are consistent with Example 1 of the present invention. The measured performance is shown in Table 9.

[0205] Comparative Example 4

[0206] This comparative example provides a method for preparing a composite hard carbon material. The only difference between this method and Example 4 of CN115911320A is that chitosan is replaced with coal-based activated carbon (coal-based-1600). The rest of the preparation process and process parameters are the same as those in Example 4 of CN115911320A.

[0207] Using the composite hard carbon material prepared in this comparative example as the negative electrode active material, the performance was measured by the sodium-ion battery preparation method, electrochemical performance testing method and conditions of Example 1 of this invention, and the results are shown in Table 9.

[0208] Comparative Example 5

[0209] This comparative example provides a method for preparing a composite carbon material, which differs from Example 1 of the present invention only in that: coal-based activated carbon is replaced with wood-based activated carbon (i.e., wood-based activated carbon with a specific surface area of ​​1100±100 m²). 2 The remaining preparation process and parameters, as well as the preparation and electrochemical performance testing methods of the sodium-ion half-cell, are consistent with those in Example 1 of this invention. The measured performance is shown in Table 9.

[0210] Comparative Example 6

[0211] This comparative example provides a method for preparing a composite carbon material. The only difference between this method and Example 3 of CN109148838A is that iron charcoal is replaced with coal-based activated carbon (coal-based-1600) in Example 1 of this invention. The rest of the preparation process and process parameters are the same as those in Example 3 of CN109148838A.

[0212] Using the composite carbon material prepared in this comparative example as the negative electrode active material, the performance was measured by the sodium-ion battery preparation method, electrochemical performance testing method and conditions of Example 1 of this invention, and the results are shown in Table 9.

[0213] Comparative Example 7

[0214] This comparative example provides a method for preparing a composite carbon material. The only difference between this method and Example 4 of CN115911320A is that chitosan is replaced with activated carbon charcoal. All other preparation processes and parameters are the same as in Example 4 of CN115911320A.

[0215] Using the composite hard carbon material prepared in this comparative example as the negative electrode active material, the performance was measured by the sodium-ion battery preparation method, electrochemical performance testing method and conditions of Example 1 of this invention, and the results are shown in Table 9.

[0216] Comparative Example 8

[0217] This comparative example provides a method for preparing a composite carbon material. The only difference between this method and Example 3 of CN109148838A is that iron charcoal is replaced with chitosan. The rest of the preparation process and process parameters are the same as those in Example 3 of CN109148838A.

[0218] Using the composite carbon material prepared in this comparative example as the negative electrode active material, the performance was measured by the sodium-ion battery preparation method, electrochemical performance testing method and conditions of Example 1 of this invention, and the results are shown in Table 9.

[0219] Table 8. Comparison of electrochemical performance of sodium-ion batteries in Example 1, Comparative Example 1, and Comparative Example 2

[0220]

[0221] Note: For the test conditions of the sodium-ion battery and negative electrode electrochemical performance of Comparative Example 2, please refer to Example 2 of Publication No. CN109742383A.

[0222] As can be seen from Table 8, compared with the anode material prepared directly from activated carbon and the hard carbon anode material prepared in Example 2 of CN109742383A, the composite carbon anode material of the present invention has better specific capacity, first coulombic efficiency and cycle performance when used as anode active material for sodium-ion batteries.

[0223] Table 9 Comparison of electrochemical performance of sodium-ion batteries in Example 1 and Comparative Examples 3-9

[0224]

[0225]

[0226] Note: The sodium-ion batteries or negative electrodes in Table 9 were all tested for electrochemical performance using the same electrochemical testing methods and conditions.

[0227] As shown in Table 9, compared with Example 1, Comparative Example 3, using chitosan as the main material, yielded a composite material with poor performance in sodium-ion batteries based on the preparation parameters of Example 1 of this invention. Unlike CN115911320A, the innovation of this invention lies in using activated carbon with abundant pore structure and large specific surface area as the matrix material. Through appropriate soft carbon precursors, raw material amounts, and a single calcination process, the ineffective pores on its surface are transformed into highly efficient sodium storage active pores. Furthermore, the preparation process of this invention does not require cumbersome steps such as doping; good rate performance can be obtained simply by utilizing the electrochemical coupling between active pores.

[0228] Compared to Example 1, Comparative Example 4, using the preferred coal-based activated carbon (i.e., coal-based-1600 activated carbon) from Example 1 as the main material, showed poor performance in sodium-ion batteries based on the preparation parameters of CN115911320A. This is because the hard carbon obtained after chitosan carbonization differs significantly from activated carbon in terms of surface structure, carbon layer order, and internal pores; the two experimental schemes employed two different types of materials.

[0229] It is evident that this invention differs from CN115911320A in its inventive concept, raw materials used, performance improvement mechanism, and process steps.

[0230] Compared to Example 1, Comparative Example 5, which uses charcoal activated carbon as the main material and is prepared based on the parameters of Example 1, shows poor performance in sodium-ion batteries. This is because charcoal activated carbon and coal-based activated carbon belong to different categories of carbon materials. The pore structure on the surface of charcoal activated carbon is uncontrollable and cannot be effectively converted into active pores for sodium storage.

[0231] Compared to Example 1, Comparative Example 6, using coal-based activated carbon (coal-1600) as the main material in Example 1 of this invention, showed poor performance in sodium-ion batteries when prepared according to the preparation parameters of CN109148838A. This is because the preparation method of CN109148838A cannot transform the ineffective pores on the surface of the coal-based activated carbon into sodium storage active pores.

[0232] Compared to Example 1, Comparative Example 7, using charcoal activated carbon as the main material in CN109148838A and prepared according to the parameters of CN115911320A, showed poor performance in sodium-ion batteries; similarly, the composite material using chitosan as the main material in CN115911320A and prepared according to the parameters of CN109148838A also showed poor performance in sodium-ion batteries. This is because the charcoal activated carbon in CN109148838A cannot be transformed into a high-efficiency sodium storage carbon material using the preparation method of CN115911320A. Likewise, chitosan in CN115911320A cannot be transformed into a high-efficiency sodium storage carbon material using the preparation method of CN109148838A.

[0233] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A composite carbon material, characterized in that, Includes activated carbon and a soft carbon layer coating the surface of the activated carbon; The activated carbon is selected from at least one of coal-based activated carbon, coconut shell activated carbon, and bamboo charcoal activated carbon; The soft carbon layer includes sodium storage active pores, and the soft carbon layer is prepared by melting a soft carbon precursor, coating it onto the surface of activated carbon, and then calcining it once. The soft carbon precursor is melted and coated on the surface of activated carbon by mixing the activated carbon and dispersant, then adding the soft carbon precursor and mixing, and heating until the soft carbon precursor melts. The heating temperature is 30–80°C; The mass ratio of the soft carbon precursor to activated carbon is (1~2):1; The calcination temperature is 500℃~1900℃, and the calcination time is 0.5h~10h.

2. The composite carbon material according to claim 1, characterized in that, The composite carbon material consists of activated carbon and a soft carbon layer coating the surface of the activated carbon.

3. The composite carbon material according to claim 1 or 2, characterized in that: The sodium storage active pore is a semi-closed pore, and the pore size of the sodium storage active pore is 0.1~30nm.

4. The composite carbon material according to claim 3, characterized in that: The specific surface area of ​​the composite carbon material is ≤20 m². 2 / g.

5. The composite carbon material according to claim 3, characterized in that: The activated carbon is selected from at least one of coal-based activated carbon and coconut shell activated carbon; And / or, The specific surface area of ​​the activated carbon is 500 m². 2 / g ~3200m 2 / g.

6. The composite carbon material according to claim 5, characterized in that: The activated carbon has a porous structure with a pore size of 0.1 nm to 5 μm.

7. The composite carbon material according to claim 4, characterized in that: The soft carbon precursor is selected from at least one of mesophase pitch, coal tar pitch, aromatic coal pitch, ethylene tar pitch, coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

8. The composite carbon material according to claim 4, characterized in that: The soft carbon precursor is selected from at least one of the following: mesophase pitch, medium-temperature pitch, low-temperature pitch, high-temperature pitch, aromatic coal pitch, ethylene tar pitch, petroleum coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

9. The composite carbon material according to claim 4, characterized in that: The soft carbon precursor is selected from at least one of the following: mesophase pitch, coal tar pitch, aromatic coal pitch, ethylene tar pitch, needle coke, anthracite, mesophase carbon microspheres, and medium-temperature coal tar.

10. A method for preparing the composite carbon material according to any one of claims 1 to 9, characterized in that, Includes the following steps: S1: After mixing the activated carbon and dispersant, add the soft carbon precursor and mix, and heat until the soft carbon precursor melts to obtain an intermediate. The heating temperature is 30-80°C, and the mass ratio of the soft carbon precursor to the activated carbon is (1-2):

1. S2: The intermediate is placed in an inert atmosphere and calcined at a temperature of 500℃~1900℃ for a time of 0.5h~10h to obtain the composite carbon material.

11. The method for preparing the composite carbon material according to claim 10, characterized in that: In step S1, the heating process further includes a stirring step; and / or, the heating time is 1 to 20 hours.

12. The method for preparing the composite carbon material according to claim 10, characterized in that: In step S1, the dispersant is selected from at least one of ethanol, deionized water, methanol, ethylene glycol, and glycerol.

13. A negative electrode slurry, characterized in that, Includes the composite carbon material as described in any one of claims 1 to 9; The negative electrode slurry also includes a binder and carbon black.

14. The negative electrode slurry according to claim 13, characterized in that, The mass ratio of the composite carbon material, binder and carbon black is (5~10):1:

1.

15. A negative electrode, characterized in that, Includes the composite carbon material as described in any one of claims 1 to 9.

16. A sodium-ion battery, characterized in that, Includes the negative electrode as described in claim 15.

Citation Information

Patent Citations

  • Efficient hard carbon material and preparation method and application of efficient hard carbon material

    CN108682815A

  • Sodium ion battery hard carbon anode material based on phenolic resin and preparation method and application thereof

    CN109742383A

  • Phenolic Resin-Based Hard Carbon Anode Material for Sodium-Ion Batteries, Its Preparation Method and Application

    CN109742383B

  • Preparation method of sodium ion battery negative electrode material and sodium ion battery

    CN115566145A

  • Composite hard carbon material and preparation method and application thereof

    CN115911320A