Light emitting diode epitaxial wafer and preparation method thereof, LED
By setting a stress-relieving layer structure of Si-doped AlN layer, binary co-doped GaN layer and alternating Si-doped GaN layer and Mg-doped InN layer between N-type GaN layer and multiple quantum well layer, the problem of reduced luminous efficiency caused by lattice mismatch in the prior art is solved, and high-efficiency light emission of light-emitting diode is realized.
Patent Information
- Application Number
- CN202311008965.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-11
AI Technical Summary
In the prior art, the high In content in the InGaN quantum well leads to lattice mismatch and generates large compressive stress, which causes the polarization electric field to reduce the spatial overlap of the electron-hole wave function and the luminous efficiency. Furthermore, the existing stress relief layer cannot effectively release the thermal expansion stress of the high-temperature deposited undoped GaN/n-type GaN layer and the tensile stress between the substrate and the GaN epitaxial layer, resulting in a decrease in the luminous efficiency of the light-emitting diode.
A stress relief layer is set between the N-type GaN layer and the multiple quantum well layer, including a Si-doped AlN layer, a binary co-doped GaN layer, and alternating stacked Si-doped GaN layers and Mg-doped InN layers. The stress is relieved through the combination structure of these layers, the crystal quality is improved, and the incorporation of In atoms in the InGaN quantum well layer is promoted, the electron expansion channels are increased, and the luminescence efficiency is improved.
It effectively releases stress in the multi-quantum-well layer, improves crystal quality, enhances the luminous efficiency of the light-emitting diode, and reduces the operating voltage.
Smart Images

Figure CN116960246B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and an LED. Background Technology
[0002] LEDs (Light Emitting Diodes) are a type of diode. When a forward voltage is applied across their terminals and exceeds a certain value, LEDs emit light with a specific wavelength. The specific wavelength of the light depends on the materials used to manufacture the LED. Currently, the main materials used in LED manufacturing are group III phosphide and group III nitride semiconductor material systems.
[0003] In multi-quantum-well layers, the InGaN quantum wells have a high In content. Due to the large lattice mismatch (approximately 11%) between InN and GaN, there is significant compressive stress in the InGaN quantum wells, inducing a polarization electric field. The generation of the polarization electric field reduces the spatial overlap of the electron-hole wavefunction and the luminous efficiency. Therefore, to alleviate the stress in the multi-quantum-well layers, an InGaN / GaN superlattice layer stress relief layer is usually inserted in front of the multi-quantum-well layers. However, this stress relief layer has the following drawbacks: First, it cannot release the thermal expansion stress of the high-temperature deposited undoped GaN / n-type GaN layer; second, the InGaN / GaN superlattice layer cannot release the large tensile stress between the substrate and the GaN epitaxial layer, leading to accumulated stress in the multi-quantum-well layer and the resulting polarization effect, which reduces the luminous efficiency of the light-emitting diode. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode.
[0005] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.
[0006] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; the stress relief layer comprises a first sublayer, a second sublayer, and a third sublayer sequentially stacked on the N-type GaN layer.
[0007] The first sublayer is a Si-doped AlN layer;
[0008] The second sublayer is a binary co-doped GaN layer, with Cr and Si as the doping elements;
[0009] The third sublayer is a periodic structure formed by alternating layers of Si-doped GaN and Mg-doped InN.
[0010] As an improvement to the above technical solution, the Si doping concentration in the Si-doped AlN layer is 5 × 10⁻⁶. 17 cm -3 ~5×10 18 cm -3 Its thickness is 40nm to 100nm.
[0011] As an improvement to the above technical solution, the Si doping concentration in the binary co-doped GaN layer is 1×10⁻⁶. 17 cm -3 ~1×10 18 cm -3 The Cr doping concentration is 5×10 16 cm -3 ~1×10 18 cm -3 The thickness is 50nm to 100nm.
[0012] As an improvement to the above technical solution, the number of periods of the third sub-layer is 2 to 12, the thickness of the Si-doped GaN layer is 10 nm to 50 nm, and the thickness of the Mg-doped InN layer is 1 nm to 10 nm.
[0013] The Si doping concentration in the Si-doped GaN layer is 5 × 10⁻⁶. 16 cm -3 ~7×10 17 cm -3 The Mg doping concentration in the Mg-doped InN layer is 1×10⁻⁶. 16 cm -3 ~1×10 18 cm -3 .
[0014] As an improvement to the above technical solution, the Si doping concentration in the Si-doped AlN layer is greater than the Si doping concentration in the binary co-doped GaN layer, and the Si doping concentration in the binary co-doped GaN layer is greater than the Si doping concentration in the Si-doped GaN layer.
[0015] As an improvement to the above technical solution, the multi-quantum well layer is a periodic structure, and each period includes an InGaN quantum well layer and an AlGaN quantum barrier layer stacked sequentially.
[0016] The InGaN quantum well layer has an In content of 0.15–0.25 and a thickness of 2 nm–5 nm.
[0017] The Al component in the AlGaN quantum barrier is 0.01 to 0.1%, and its thickness is 5 nm to 15 nm.
[0018] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:
[0019] A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown; the stress relief layer includes a first sublayer, a second sublayer, and a third sublayer sequentially stacked on the N-type GaN layer.
[0020] The first sublayer is a Si-doped AlN layer;
[0021] The second sublayer is a binary co-doped GaN layer, with Cr and Si as the doping elements;
[0022] The third sublayer is a periodic structure formed by alternating layers of Si-doped GaN and Mg-doped InN.
[0023] As an improvement to the above technical solution, the growth temperature of the Si-doped AlN layer is 900℃~1100℃, and the growth pressure is 50 torr~500 torr;
[0024] The growth temperature of the binary co-doped GaN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr.
[0025] The growth temperature of the Si-doped GaN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr.
[0026] The growth temperature of the Mg-doped InN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr.
[0027] As an improvement to the above technical solution, the growth atmosphere of the stress relief layer is a mixture of N2 and NH3, with a volume ratio of N2 to NH3 of 1:1 to 1:10.
[0028] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.
[0029] Implementing this invention has the following beneficial effects:
[0030] In the epitaxial wafer of the light-emitting diode of the present invention, a stress relief layer is provided between the N-type GaN layer and the multi-quantum-well layer, which includes a first sublayer, a second sublayer, and a third sublayer. The first sublayer is a Si-doped AlN layer. Since the lattice constant of AlN is smaller than that of GaN, the coherent growth of the Si-doped AlN layer on the N-type GaN layer can generate compressive stress on the N-type GaN layer, which is beneficial for releasing the tensile stress in the N-type GaN layer. The second sublayer is a binary co-doped GaN layer, with Cr and Si as doping elements. Firstly, it can release the thermal stress accumulated during the growth of the high-temperature undoped GaN layer and the N-type GaN layer; secondly, Cr doping also introduces compressive stress, releasing residual tensile stress. The third sublayer is a superlattice structure formed by alternating layers of Si-doped GaN layers and Mg-doped InN layers. Due to the smaller lattice constant of GaN... Lattice constant of InN The differences exist; during alternating growth, the compressive and tensile stresses fluctuate repeatedly. This effectively releases residual stress before depositing the multi-quantum-well layer, which in turn promotes the incorporation of In atoms into the InGaN quantum well layer, improving crystal quality and enhancing the device's luminous efficiency. Furthermore, Si doping is introduced into the Si-doped AlN layer, the binary co-doped GaN layer, and the Si-doped GaN layer of this invention. This increases the electron expansion channels, promotes the uniform distribution of electrons in the multi-quantum-well layer, improves luminous efficiency, and reduces the operating voltage. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;
[0032] Figure 2 This is a schematic diagram of the structure of the third sublayer in one embodiment of the present invention;
[0033] Figure 3 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation
[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0035] refer to Figure 1 and Figure 2This invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1 and a buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a stress-relieving layer 5, a multiple quantum well layer 6, an electron blocking layer 7, and a P-type GaN layer 8 sequentially disposed on the substrate 1. The stress-relieving layer 5 comprises a first sublayer 51, a second sublayer 52, and a third sublayer 53 sequentially stacked on the N-type GaN layer 4. The first sublayer 51 is a Si-doped AlN layer, the second sublayer 52 is a binary co-doped GaN layer, and the third sublayer 53 is a periodic structure formed by alternating layers of Si-doped GaN layer 531 and Mg-doped InN layer 532. Based on this structure, the polarization effect caused by stress accumulation in the multiple quantum well layer can be effectively weakened, thereby improving the luminous efficiency of the light-emitting diode epitaxial wafer.
[0036] The thickness of the Si-doped AlN layer is 30 nm to 120 nm, with exemplary thicknesses of 35 nm, 50 nm, 65 nm, 80 nm, 105 nm, or 110 nm, but not limited thereto. Preferably, it is 40 nm to 100 nm.
[0037] The Si doping concentration in the Si-doped AlN layer is 5 × 10⁻⁶. 17 cm -3 ~5×10 18 cm -3 An example is 7×10 17 cm -3 9×10 17 cm -3 1×10 18 cm -3 Or 3×10 18 cm -3 However, it is not limited to this.
[0038] The thickness of the binary co-doped GaN layer is 40 nm to 150 nm. When the thickness is greater than 150 nm, the crystal quality is too poor. When the thickness is less than 40 nm, it is difficult to effectively compensate for thermal stress. For example, the thickness of the binary co-doped GaN layer is 50 nm, 70 nm, 90 nm, 110 nm, or 130 nm, but is not limited to these. Preferably, the thickness of the binary co-doped GaN layer is 50 nm to 100 nm.
[0039] The binary co-doped GaN layer consists of Si and Cr as doping elements. The Si doping concentration is 1 × 10⁻⁶. 17 cm -3 ~1×10 18 cm -3 An example is 3×10 17 cm -3 5×10 17 cm -3 7×10 17 cm-3 Or 9×10 17 cm -3 However, this is not the only one. Specifically, the Cr doping concentration in the binary co-doped GaN layer is 5 × 10⁻⁶. 16 cm -3 ~1×10 18 cm -3 An example is 6×10 16 cm -3 9×10 16 cm -3 3×10 17 cm -3 7×10 17 cm -3 Or 9×10 17 cm -3 However, it is not limited to this.
[0040] The number of cycles in the third sublayer 53 is 2 to 20, with 3, 5, 7, 12, 16 or 18 being exemplary, but not limited to these. Preferably, it is 2 to 18.
[0041] The thickness of the Si-doped GaN layer 531 is 5nm to 60nm, with exemplary thicknesses of 7nm, 13nm, 20nm, 32nm, 41nm, 50nm, or 58nm, but not limited thereto. Preferably, it is 10nm to 50nm.
[0042] The Si doping concentration in the Si-doped GaN layer 531 is 5 × 10⁻⁶. 16 cm -3 ~7×10 17 cm -3 An example is 6×10 16 cm -3 9×10 16 cm -3 1×10 17 cm -3 3×10 17 cm -3 Or 5×10 17 cm -3 However, it is not limited to this.
[0043] Preferably, in one embodiment of the present invention, the Si doping concentration in the Si-doped AlN layer is controlled to be greater than the Si doping concentration in the binary co-doped GaN layer, which is greater than the Si doping concentration in the Si-doped GaN layer 531. Based on this scheme, electron expansion can be further improved, luminous efficiency can be increased, and operating voltage can be reduced.
[0044] In the Mg-doped InN layer 532, Mg is incorporated. Firstly, this creates a small number of holes, replenishing the hole concentration in the previous quantum well layers. Secondly, the Mg doping promotes more three-dimensional growth of the Mg-doped InN layer, facilitating stress release from multiple dimensions and promoting a uniform distribution of In in the multi-quantum well layer 6. Specifically, the Mg doping concentration in the Mg-doped InN layer 532 is 1 × 10⁻⁶. 16 cm -3 ~1×10 18 cm -3 When its doping concentration is >1×10 18 cm -3 Holes can recombine with electrons nonradiatively, reducing luminescence efficiency; when the doping concentration is <1×10⁻⁶, the luminescence efficiency is reduced. 16 cm -3 At this time, the stress release effect is poor. For example, the Mg doping concentration in the Mg-doped InN layer 532 is 1×10⁻⁶. 16 cm -3 ~1×10 18 cm -3 An example is 3×10 16 cm -3 7×10 16 cm -3 1×10 17 cm -3 5×10 17 cm -3 Or 9×10 17 cm -3 However, it is not limited to this.
[0045] The thickness of the Mg-doped InN layer 532 is 0.5 nm to 12 nm, with exemplary thicknesses of 0.7 nm, 1.5 nm, 3 nm, 5 nm, 7 nm, 9 nm, or 11 nm, but not limited thereto. Preferably, it is 1 nm to 10 nm.
[0046] Substrate 1 can be a sapphire substrate, a silicon substrate, a zinc oxide substrate, a gallium oxide substrate, or a silicon carbide substrate, but is not limited to these.
[0047] The buffer layer 2 is an AlN layer or an AlGaN layer, but is not limited to these. The thickness of the buffer layer 2 is 20nm to 80nm, with 25nm, 40nm, 55nm, 70nm or 78nm being exemplary, but not limited to these.
[0048] The thickness of the undoped GaN layer 3 is 1 μm to 3 μm, with exemplary thicknesses of 1.2 μm, 1.5 μm, 1.8 μm, 2.1 μm, 2.5 μm or 2.8 μm, but not limited thereto.
[0049] The doping element of the N-type GaN layer 4 is Si or Ge, but is not limited to these, with Si being preferred. The doping concentration of the N-type GaN layer 4 is 1×10⁻⁶. 19 cm -3 ~5×10 19 cm -3 An example is 1.5 × 10 19 cm -3 2×10 19 cm -3 2.5×10 19 cm -3 3×10 19 cm -3 Or 4×10 19 cm -3 However, it is not limited to this. The thickness of the N-type GaN layer 4 is 2μm to 3μm, with exemplary thicknesses of 2.2μm, 2.4μm, 2.6μm, 2.8μm or 2.9μm, but it is not limited to this.
[0050] The multiple quantum well layer 6 consists of alternating stacked InGaN quantum well layers 61 and AlGaN quantum barrier layers 62, with a stacking period of 3 to 15. The In content of the InGaN quantum well layer 61 is 0.1% to 0.25%, exemplarily 0.12%, 0.15%, 0.18%, 0.21%, or 0.23%, but not limited thereto. Preferably, it is 0.15% to 0.25%, and the stress relief layer 5 of this invention can effectively increase the In content of the InGaN quantum well layer 61. The thickness of a single InGaN quantum well layer 61 is 2nm to 5nm, exemplarily 2.5nm, 3.3nm, 3.7nm, 4.1nm, 4.5nm, or 4.9nm, but not limited thereto. The Al content of the AlGaN quantum barrier layer 62 is 0.01% to 0.1%, exemplarily 0.02%, 0.04%, 0.06%, or 0.08%, but not limited thereto. The thickness of a single AlGaN quantum barrier layer 62 is 5nm to 15nm, with exemplary thicknesses of 6.4nm, 8nm, 10nm, 12nm or 14nm, but not limited thereto.
[0051] The electron blocking layer 7 is an AlInGaN layer, but is not limited thereto. The thickness of the electron blocking layer 7 is 10nm to 50nm, and exemplary examples are 12nm, 18nm, 25nm, 30nm, 42nm or 45nm, but is not limited thereto.
[0052] The P-type dopant element in the P-type GaN layer 8 is Mg, Be, or Zn, but is not limited to these. Mg is preferred. The P-type doping concentration in the P-type GaN layer 8 is 1 × 10⁸. 19 cm -3 ~1×10 21 cm -3An example is 3×10 19 cm -3 7×10 19 cm -3 1×10 20 cm -3 4×10 20 cm -3 Or 8×10 20 cm -3 However, it is not limited to this. The thickness of the p-type GaN layer 8 is 10nm to 50nm, with examples being 12nm, 18nm, 25nm, 30nm, 42nm or 45nm, but not limited to this.
[0053] Accordingly, refer to Figure 3 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes the following steps:
[0054] S1: Provides a substrate;
[0055] S2: A buffer layer, an undoped GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate.
[0056] Specifically, step S2 includes:
[0057] S21: Grow a buffer layer on the substrate;
[0058] Specifically, the buffer layer can be grown using PVD, MOCVD, MBE, or VPE, but is not limited to these methods.
[0059] Preferably, in one embodiment of the present invention, an AlN layer is grown by PVD as a buffer layer.
[0060] S22: Growing an undoped GaN layer on the buffer layer;
[0061] In one embodiment of the present invention, an undoped GaN layer is grown in MOCVD at a growth temperature of 1050°C to 1200°C and a growth pressure of 100 torr to 500 torr.
[0062] S23: Growing an N-type GaN layer on an undoped GaN layer;
[0063] In one embodiment of the present invention, an N-type GaN layer is grown in MOCVD at a growth temperature of 1050°C to 1200°C and a growth pressure of 100 torr to 500 torr.
[0064] S24: Growing a stress-relieving layer on an N-type GaN layer;
[0065] Specifically, step S24 includes:
[0066] S241: Growing the first sublayer on an N-type GaN layer;
[0067] Among them, Si-doped AlN layers can be grown by MOCVD, MBE or VPE as the first sublayer, but are not limited to these methods.
[0068] Preferably, in one embodiment of the present invention, a Si-doped AlN layer is grown by MOCVD at a growth temperature of 900°C to 1100°C, a growth pressure of 50 torr to 500 torr, and a growth atmosphere of a mixture of N2 and NH3 with a volume ratio of N2 to NH3 of 1:1 to 1:10. Based on these growth conditions, the crystal quality of the layer can be improved.
[0069] S242: Growing a second sublayer on the first sublayer;
[0070] Binary co-doped GaN layers can be grown via MOCVD, MBE, or VPE as a second sublayer, but are not limited to these methods.
[0071] Preferably, in one embodiment of the present invention, a binary co-doped GaN layer is grown by MOCVD at a growth temperature of 750°C to 950°C, a growth pressure of 50 torr to 500 torr, and a growth atmosphere of a mixture of N2 and NH3 with a volume ratio of N2 to NH3 of 1:1 to 1:10. Based on these growth conditions, the crystal quality of the layer can be improved.
[0072] S243: A third sublayer is grown on the second sublayer to obtain a stress-relieving layer;
[0073] Among these methods, Si-doped GaN layers and Mg-doped InN layers can be periodically grown using MOCVD, MBE, or VPE until a third sublayer is obtained, but this method is not the only one that can be used.
[0074] Preferably, in one embodiment of the present invention, Si-doped GaN layers and Mg-doped InN layers are periodically grown by MOCVD. The growth temperature of the Si-doped GaN layer is 750℃~950℃, the growth pressure is 50 torr~500 torr, and the growth atmosphere is a mixture of N2 and NH3, with a volume ratio of N2 to NH3 of 1:1~1:10. The growth temperature of the Mg-doped InN layer is 750℃~950℃, the growth pressure is 50 torr~500 torr, and the growth atmosphere is a mixture of N2 and NH3, with a volume ratio of N2 to NH3 of 1:1~1:10.
[0075] S25: Growth of a multi-quantum well layer on the stress-relief layer;
[0076] In one embodiment of the present invention, InGaN quantum well layers and AlGaN quantum barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the InGaN quantum well layer is 750°C to 850°C, and the growth pressure is 50 torr to 300 torr. The growth temperature of the AlGaN quantum barrier layer is 800°C to 900°C, and the growth pressure is 50 torr to 300 torr.
[0077] S26: Growth of an electron blocking layer on a multi-quantum-well layer;
[0078] In one embodiment of the present invention, an AlInGaN layer is grown by MOCVD as an electron blocking layer. The growth temperature is 800℃~900℃, and the growth pressure is 50 torr~300 torr.
[0079] S27: Grow a P-type GaN layer on an electron blocking layer;
[0080] In one embodiment of the present invention, a P-type GaN layer is grown by MOCVD at a growth temperature of 900°C to 1050°C and a growth pressure of 100 torr to 500 torr.
[0081] The present invention will be further described below with reference to specific embodiments:
[0082] Example 1
[0083] refer to Figure 1 This embodiment provides a light-emitting diode epitaxial wafer, which includes a substrate 1 and a buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a stress relief layer 5, a multiple quantum well layer 6, an electron blocking layer 7, and a P-type GaN layer 8 sequentially disposed on the substrate 1.
[0084] In this design, substrate 1 is a sapphire substrate, buffer layer 2 is an AlN layer with a thickness of 35 nm, undoped GaN layer 3 has a thickness of 1.8 μm, and N-type GaN layer 4 has a thickness of 2.2 μm, with Si as the dopant element and a Si doping concentration of 3 × 10⁻⁶. 19 cm -3 .
[0085] The stress relief layer 5 comprises a first sublayer 51, a second sublayer 52, and a third sublayer 53 sequentially stacked on an N-type GaN layer 4. The first sublayer 51 is a Si-doped AlN layer with a thickness of 110 nm and a Si doping concentration of 6 × 10⁻⁶. 17 cm -3 The second sublayer 52 is a binary co-doped GaN layer with a thickness of 45 nm. Its doping elements are Cr and Si, with a Si doping concentration of 6 × 10⁻⁶. 17 cm -3The Cr doping concentration is 7×10 17 cm -3 The third sublayer 53 is a periodic structure formed by alternating layers of Si-doped GaN layer 531 and Mg-doped InN layer 532, with a period number of 6. The thickness of the Si-doped GaN layer 531 is 55 nm, and the Si doping concentration is 6 × 10⁻⁶. 17 cm -3 The thickness of the Mg-doped InN layer 532 is 11 nm, and the Mg doping concentration is 5 × 10⁻⁶. 16 cm -3 .
[0086] The multi-quantum-well layer 6 has a periodic structure with 10 periods. Each period includes an InGaN quantum well layer 61 and an AlGaN quantum barrier layer 62 stacked sequentially. The InGaN quantum well layer 61 has an In content of 0.2% and a thickness of 3 nm, while the AlGaN quantum barrier layer 62 has an Al content of 0.06% and a thickness of 10 nm.
[0087] Among them, electron blocking layer 7 is an AlInGaN layer with a thickness of 40 nm. P-type GaN layer 8 has a thickness of 20 nm, and the doping element is Mg with a doping concentration of 5 × 10⁻⁶. 20 cm -3 .
[0088] The method for fabricating an epitaxial wafer for a light-emitting diode in this embodiment includes the following steps:
[0089] (1) Provide a substrate.
[0090] (2) Grow a buffer layer on the substrate;
[0091] Among them, an AlN layer is grown by PVD as a buffer layer.
[0092] (3) Grow an undoped GaN layer on the buffer layer;
[0093] Undoped GaN layers were grown in MOCVD at a temperature of 1080℃ and a pressure of 300 torr.
[0094] (4) An N-type GaN layer is grown on an undoped GaN layer;
[0095] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr.
[0096] (5) Grow the first sublayer on the N-type GaN layer;
[0097] In this process, a Si-doped AlN layer was grown by MOCVD as the first sublayer. The growth temperature was 980℃, the growth pressure was 200 torr, and the growth atmosphere was a mixture of N2 and NH3 with a volume ratio of 1:1.5.
[0098] (6) Grow the second sublayer on the first sublayer;
[0099] In this process, a binary co-doped GaN layer is grown by MOCVD as the second sublayer. The growth temperature is 820℃, the growth pressure is 200 torr, and the growth atmosphere is a mixture of N2 and NH3 with a volume ratio of 1:3.
[0100] (7) A third sublayer is grown on the second sublayer to obtain a stress-relieving layer;
[0101] The process involves periodically growing Si-doped GaN and Mg-doped InN layers using MOCVD until a third sublayer is obtained. The Si-doped GaN layer is grown at 800℃ and 200 torr under a mixed N2 and NH3 atmosphere with a volume ratio of 1:1.5. The Mg-doped InN layer is grown at 760℃ and 200 torr under a mixed N2 and NH3 atmosphere with a volume ratio of 1:8.
[0102] (8) Grow a multi-quantum well layer on the stress relief layer;
[0103] In this process, InGaN quantum well layers and AlGaN quantum barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the InGaN quantum well layer is 790℃, and the growth pressure is 200 torr. The growth temperature of the AlGaN quantum barrier layer is 880℃, and the growth pressure is 200 torr.
[0104] (9) Grow an electron blocking layer on a multi-quantum-well layer;
[0105] In this method, an AlInGaN layer was grown using MOCVD as an electron blocking layer. The growth temperature was 880℃ and the growth pressure was 200 torr.
[0106] (10) Grow a P-type GaN layer on an electron blocking layer;
[0107] P-type GaN layers were grown using MOCVD at a temperature of 1000℃ and a pressure of 200 torr.
[0108] Example 2
[0109] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that:
[0110] The thickness of the Si-doped AlN layer is 45 nm, and the thickness of the binary co-doped GaN layer is 65 nm.
[0111] Everything else is the same as in Example 1.
[0112] Example 3
[0113] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that:
[0114] The thickness of the Si-doped GaN layer 531 is 30 nm, and the thickness of the Mg-doped InN layer 532 is 3.5 nm.
[0115] Everything else is the same as in Example 2.
[0116] Example 4
[0117] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that:
[0118] The Si doping concentration in the Si-doped AlN layer is 3 × 10⁻⁶. 18 cm -3 The Si doping concentration in the binary co-doped GaN layer is 6 × 10⁻⁶. 17 cm -3 The Si doping concentration in the Si-doped GaN layer 531 is 8 × 10⁻⁶. 16 cm -3 .
[0119] Everything else is the same as in Example 3.
[0120] Comparative Example 1
[0121] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that:
[0122] The stress relief layer is not provided, and correspondingly, the preparation method does not include the step of preparing this layer.
[0123] Everything else is the same as in Example 1.
[0124] Comparative Example 2
[0125] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that:
[0126] The stress relief layer has a periodic structure with 8 periods, each period consisting of sequentially stacked In layers. a Ga 1-a N-layer (a = 0.11) and GaN layer. Among them, a single In... a Ga 1-aThe thickness of the N layer is 2.5 nm, and the thickness of a single GaN layer is 9 nm.
[0127] The stress relief layer is prepared by periodically growing In in MOCVD. a Ga 1-a N-layers and GaN layers are added until a stress-relieving layer is obtained. In... a Ga 1-a The N-layer was grown at a temperature of 800℃ and a growth pressure of 150 torr. The GaN-layer was grown at a temperature of 860℃ and a growth pressure of 150 torr.
[0128] The LED epitaxial wafers obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were fabricated into 10×24mil LED chips with a vertical structure. Their brightness at a current of 120mA was tested. Ten chips were tested for each example and comparative example, and the average value was taken. The brightness improvement rate was calculated using Comparative Example 1 as a benchmark.
[0129] The specific results are as follows:
[0130] Brightness improvement rate / % Example 1 2.8 Example 2 3.2 Example 3 4.1 Example 4 5.3 Comparative Example 1 - Comparative Example 2 0.9
[0131] As can be seen from the table, when the stress relief layer of the present invention (Examples 1-4) is added to the conventional light-emitting diode structure (Comparative Example 1), or when the conventional stress relief layer (Comparative Example 2) is replaced with the stress relief layer of the present invention (Examples 1-4), the luminous efficiency of the light-emitting diode epitaxial wafer is effectively improved.
[0132] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light-emitting diode epitaxial wafer, characterized in that, It includes a substrate and a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; the stress relief layer includes a first sublayer, a second sublayer, and a third sublayer sequentially stacked on the N-type GaN layer. The first sublayer is a Si-doped AlN layer; The second sub-layer is a binary co-doped GaN layer, the doping elements of which are Cr and Si, the Si doping concentration is 1×10 17 cm -3 ~1×10 18 cm -3 , the Cr doping concentration is 5×10 16 cm -3 ~1×10 18 cm -3 , and the thickness is 50nm~100nm; The third sub-layer is a periodic structure formed by alternately stacking Si-doped GaN layers and Mg-doped InN layers, the number of periods is 2-12, the thickness of the Si-doped GaN layer is 10-50 nm, the Si doping concentration is 5*10 16 cm -3 -7*10 17 cm -3 , and the thickness of the Mg-doped InN layer is 1-10 nm, the Mg doping concentration is 1*10 16 cm -3 -1*10 18 cm -3 .
2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Si doping concentration in the Si-doped AlN layer is 5 × 10⁻⁶. 17 cm -3 ~5×10 18 cm -3 Its thickness is 40nm~100nm.
3. The light-emitting diode epitaxial wafer as described in claim 1 or 2, characterized in that, The Si doping concentration in the Si-doped AlN layer is greater than the Si doping concentration in the binary co-doped GaN layer, and the Si doping concentration in the binary co-doped GaN layer is greater than the Si doping concentration in the Si-doped GaN layer.
4. The light-emitting diode epitaxial wafer as described in claim 1 or 2, characterized in that, The multi-quantum-well layer has a periodic structure, and each period includes an InGaN quantum well layer and an AlGaN quantum barrier layer stacked sequentially. The InGaN quantum well layer has an In content of 0.15~0.25 and a thickness of 2nm~5nm. The Al component in the AlGaN quantum barrier layer is 0.01~0.1%, and its thickness is 5nm~15nm.
5. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, include: A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown; the stress relief layer includes a first sublayer, a second sublayer, and a third sublayer sequentially stacked on the N-type GaN layer. The first sublayer is a Si-doped AlN layer; The second sublayer is a binary co-doped GaN layer, with Cr and Si as the doping elements; The third sublayer is a periodic structure formed by alternating layers of Si-doped GaN and Mg-doped InN.
6. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth temperature of the Si-doped AlN layer is 900℃~1100℃, and the growth pressure is 50 torr~500 torr. The growth temperature of the binary co-doped GaN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr. The growth temperature of the Si-doped GaN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr. The growth temperature of the Mg-doped InN layer is 750℃~950℃, and the growth pressure is 50 torr~500 torr.
7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The growth atmosphere of the stress relief layer is a mixture of N2 and NH3, with a volume ratio of N2 to NH3 of 1:1 to 1:
10.
8. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1 to 4.
Citation Information
Patent Citations
Light-emitting diode
CN103137803A
Display apparatus using semiconductor light-emitting device and manufacturing method therefor
WO2019203404A1