A deep ultraviolet bimetallic mixed halogen nonlinear optical crystal material, a preparation method and application thereof
The KBa₃Zr₂F₁₄Cl crystal material prepared by hydrothermal synthesis solves the problems of insufficient frequency doubling effect and phase matching performance of existing deep ultraviolet nonlinear optical materials, and achieves a strong frequency doubling effect and wide transmission band, which is suitable for phase matching of deep ultraviolet lasers.
Patent Information
- Application Number
- CN202310953502.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-01
AI Technical Summary
Existing deep ultraviolet nonlinear optical materials are insufficient in terms of frequency doubling effect and birefringence, and cannot achieve phase matching, which limits their application in deep ultraviolet lasers.
A novel bimetallic mixed-halogen nonlinear optical crystal material, KBa₃Zr₂F₁₄Cl, was prepared by hydrothermal synthesis. The material has a tetragonal crystal system, space group α=β=γ=90°, Z=1, and a unit cell volume of [missing information]. By controlling the molar ratio of K, Ba, Zr, F, and Cl sources and crystallizing at 190–220 °C for 48–120 h, a ZrF₇ single-cap triangular prism structure was formed, with K, Ba, and Cl atoms filling the interstitial spaces as counterions.
It achieves strong frequency doubling effect, wide transmission band and phase matching performance, ultraviolet absorption cutoff wavelength is less than 200nm, and has stable physicochemical properties, making it suitable for deep ultraviolet laser frequency converters.
Smart Images

Figure CN116971031B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a nonlinear optical crystal material, its preparation method, and its applications. Background Technology
[0002] Laser technology is widely used in laser welding and cutting, medicine, laser communication, and laser guidance. To date, available lasers cover the wavelength range from ultraviolet to infrared, but this still cannot meet the growing demand of modern society for deep ultraviolet and mid / far-infrared light. Nonlinear optical materials, as core components of solid-state lasers, can generate new light wavelengths through frequency conversion methods such as second harmonic generation, sum-frequency generation, difference-frequency generation, and optical parametric oscillation. Therefore, exploring new nonlinear optical materials is necessary and meaningful.
[0003] All-solid-state lasers have become the optimal choice for deep ultraviolet (<200nm) laser applications due to their advantages in size, usage, and beam quality. Therefore, the performance of deep ultraviolet nonlinear optical materials, as the core components of deep ultraviolet all-solid-state lasers, has become crucial to the generation and application of deep ultraviolet lasers. Deep ultraviolet nonlinear optical materials can be broadly classified into two categories: π-conjugated systems and non-π-conjugated systems. To date, researchers have made a series of efforts to design and synthesize deep ultraviolet nonlinear optical materials composed of borates, carbonates, nitrates, sulfates, silicates, and phosphates. However, materials that currently meet the stringent nonlinear optical property standards are still few. Furthermore, the weak frequency doubling effect and extremely low birefringence of the three reported deep ultraviolet halides prevent phase matching, limiting their further application in the deep ultraviolet nonlinear field. Therefore, discovering or designing novel deep ultraviolet nonlinear optical materials with excellent properties (large frequency doubling effect, short ultraviolet cutoff edge, and moderate birefringence for phase matching) remains a long-term goal. Summary of the Invention
[0004] Objective of the invention: To address the aforementioned limitations of existing technologies, this invention proposes a deep-ultraviolet bimetallic mixed-halogen nonlinear optical crystal material, its preparation method, and its applications. The nonlinear optical crystal material is KBa3Zr2F. 14 Cl exhibits excellent performance, including strong frequency doubling effect, wide transmission band, phase matching performance, and stable physicochemical properties.
[0005] Technical solution: A deep ultraviolet bimetallic mixed halide nonlinear optical crystal material, wherein the chemical formula of the crystal material is KBa3Zr2F 14 Cl belongs to the tetragonal crystal system and has space group 1. Cell parameters are α=β=γ=90°, Z=1, cell volume is
[0006] A method for preparing a deep ultraviolet bimetallic mixed halide nonlinear optical crystal material, employing a hydrothermal synthesis method, specifically includes the following steps:
[0007] Step 1: Mix the K source, Ba source, Zr source, F source, Cl source and water to form the initial mixed raw material;
[0008] Step 2: The initial mixed raw materials are placed in a closed reactor and crystallized under hydrothermal conditions of 190-220°C to obtain the crystalline material.
[0009] Furthermore, the molar ratio of K source, Ba source, Zr source, F source and Cl source in the initial mixed raw material is 1~3:1~3:1~2:1~2:6~12.
[0010] Furthermore, the crystallization time is 48–120 h, and after crystallization, the temperature is reduced to room temperature at a rate of 1–5 °C / h.
[0011] Furthermore, the K source is one of potassium fluoride, potassium chloride, and potassium bromide; the Ba source is one of barium fluoride and barium chloride; the Zr source is zirconium fluoride; the F source is zirconium fluoride; and the Cl source is hydrochloric acid.
[0012] Application of the deep ultraviolet nonlinear optical crystal material in the fabrication of laser frequency converters.
[0013] Beneficial effects: 1. This invention provides a novel bimetallic mixed halide crystal KBa3Zr2F 14 Cl, whose each asymmetric unit contains one K, two Ba, one Zr, four F, and one Cl atom. For example... Figure 1 As shown, each Zr atom is bonded to 7 F atoms, forming a ZrF7 single-capped triangular prism. Each ZrF7 single-capped triangular prism is isolated from each other and arranged along the c-axis, forming a zero-dimensional structure. K, Ba, and Cl atoms fill the interstices as counter ions to balance the valence.
[0014] 2. The bimetallic mixed halide crystal KBa3Zr2F of the present invention 14 Cl, under 1064 nm laser irradiation, exhibits a powder frequency doubling effect comparable to KDP, and demonstrates good phase matching performance and stable physicochemical properties. Therefore, KBa3Zr2F 14 Cl crystals have great potential applications as nonlinear optical crystal materials.
[0015] 3. The bimetallic mixed halide crystal KBa3Zr2F provided by this invention 14Cl, with a wide transmission band of 2.5-23.0 μm and an ultraviolet absorption cutoff wavelength of less than 200 nm, is the first deep ultraviolet nonlinear mixed halide that can achieve phase matching.
[0016] 4. This invention provides a bimetallic mixed halide compound crystal KBa3Zr2F 14 The preparation method of Cl involved hydrothermal crystallization, resulting in the growth of KBa3Zr2F. 14 Cl crystals. This method is simple and can yield high-purity, high-cleanliness bimetallic mixed halide compound KBa3Zr2F. 14 Cl crystal materials. Attached Figure Description
[0017] Figure 1 It is KBa3Zr2F 14 Schematic diagram of the crystal structure of Cl;
[0018] Figure 2 The X-ray diffraction pattern of the sample in Example 1, obtained by fitting the crystal structure at the single crystal X-ray diffraction analysis, is compared with the X-ray diffraction pattern obtained after the sample is ground into powder.
[0019] Figure 3 This is the UV-Vis-diffuse reflectance spectrum of the sample from Example 1;
[0020] Figure 4 This is the infrared absorption spectrum of the sample from Example 1;
[0021] Figure 5 This is the thermogravimetric analysis spectrum of the sample from Example 1;
[0022] Figure 6 This is a comparison chart of the frequency doubling effect of the sample and the standard KDP in Example 1 at the maximum particle size (200-250 μm);
[0023] Figure 7 This is the second harmonic phase matching diagram of the sample in Example 1 at the 1064nm band. Detailed Implementation
[0024] The invention will now be further explained with reference to the accompanying drawings.
[0025] Example 1
[0026] KCl, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:1.5:2:12. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210°C under hydrothermal conditions and held at that temperature for 96 hours. Then, the system temperature was slowly lowered to room temperature at a rate of 1°C / h. After separation and drying, colorless lumpy KBa3Zr2F4 was obtained. 14Cl crystals.
[0027] Example 2
[0028] KCl, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:1.5:1:6. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 200°C under hydrothermal conditions and held at that temperature for 72 hours. Then, the system temperature was slowly lowered to room temperature at a rate of 2°C / h. After separation and drying, colorless lumps of KBa3Zr2F4 were obtained. 14 Cl crystals.
[0029] Example 3
[0030] KCl, BaF2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:2:2:8. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 220°C under hydrothermal conditions and held at that temperature for 96 hours. The system temperature was then slowly cooled to room temperature at a rate of 3°C / h. After separation and drying, colorless, blocky KBa3Zr2F4 was obtained. 14 Cl crystals.
[0031] Example 4
[0032] KCl, BaF2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 2:3:1:8. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 190°C under hydrothermal conditions and held at that temperature for 120 hours. The system temperature was then slowly cooled to room temperature at a rate of 5°C / h. After separation and drying, colorless, blocky KBa3Zr2F4 was obtained. 14 Cl crystals.
[0033] Example 5
[0034] KF, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:3:2:12. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 200°C under hydrothermal conditions and held at that temperature for 72 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 2°C / h. After separation and drying, colorless granular KBa3Zr2F4 was obtained. 14 Cl crystals.
[0035] Example 5
[0036] KF, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:1.5:2:6. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210°C under hydrothermal conditions and held at that temperature for 96 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 1°C / h. After separation and drying, colorless lumpy KBa3Zr2F4 was obtained. 14 Cl crystals.
[0037] Example 6
[0038] KF, BaF2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:2:2:8. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210°C under hydrothermal conditions and held at that temperature for 120 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 1°C / h. After separation and drying, colorless granular KBa3Zr2F was obtained. 14 Cl crystals.
[0039] Example 7
[0040] KF, BaF2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:3:2:8. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 220°C under hydrothermal conditions and held at that temperature for 120 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 1°C / h. After separation and drying, colorless granular KBa3Zr2F was obtained. 14 Cl crystals.
[0041] Example 7
[0042] KBr, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 3:1:2:12. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 190°C under hydrothermal conditions and held at that temperature for 48 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 5°C / h. After separation and drying, colorless granular KBa3Zr2F4 was obtained. 14 Cl crystals.
[0043] Example 8
[0044] KBr, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 2:1:2:10. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210℃ under hydrothermal conditions and held at that temperature for 120 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 1℃ / h. After separation and drying, colorless granular KBa3Zr2F4 was obtained. 14 Cl crystals.
[0045] Example 9
[0046] KBr, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:1:2:8. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210℃ under hydrothermal conditions and held at that temperature for 96 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 2℃ / h. After separation and drying, colorless granular KBa3Zr2F4 was obtained. 14 Cl crystals.
[0047] Example 10
[0048] KBr, BaCl2, ZrF4, and HCl were mixed thoroughly in a molar ratio of 1:1.5:2:10. Deionized water was added, and the mixture was placed in a high-pressure reactor with a fine polytetrafluoroethylene liner. After sealing, the mixture was heated to 210℃ under hydrothermal conditions and held at that temperature for 120 hours. Then, the system temperature was slowly cooled to room temperature at a rate of 1℃ / h. After separation and drying, colorless lumps of KBa3Zr2F4 were obtained. 14 Cl crystals.
[0049] Crystal structure analysis of samples 1-10 in Examples:
[0050] The structures of the samples in Examples 1-10 were analyzed using single-crystal X-ray diffraction and powder X-ray diffraction methods.
[0051] The single-crystal X-ray diffraction tests were performed on a Bruker D8 QUEST X-ray single-crystal diffractometer (Germany). The crystal size was 0.08 × 0.07 × 0.06 mm. 2 The data collection temperature was 296 K, and the diffraction source was graphite-monochromatic Mo-Kα rays. Data were processed using the Multi-scan method for absorption correction. Structural analysis was performed using the SHELXTL package; the positions of heavy atoms were determined using a direct method, and the coordinates of the remaining atoms were obtained using difference Fourier synthesis; F-based... 2 The coordinates and anisotropic thermal parameters of all atoms were refined using the full matrix least squares method. The final crystal structure parameters obtained in Example 1 are shown in Table 1.
[0052] Table 1
[0053]
[0054]
[0055] a R1=||F o |–|F c || / |F o ; bwR2=[w(F o 2 –F c 2 ) 2 ] / [w(F o 2 ) 2 ] 1 / 2 .
[0056] Powder X-ray diffraction tests were performed on a Bruker D8 Advance X-ray powder diffractometer (Germany), under the following conditions: fixed target, monochromatic Cu-Kα light source, and wavelength [wavelength missing]. The scanning range was 10–60°, with a scanning step size of 0.02°. Powder X-ray diffraction (PXRD) analysis showed that the peak positions of the samples in Examples 1–10 were basically the same, although the diffraction intensities differed slightly.
[0057] Taking the sample from Example 1 as a typical example, such as Figure 2 As shown, the X-ray diffraction pattern obtained by fitting the crystal structure obtained from single-crystal X-ray diffraction analysis is consistent with the X-ray diffraction pattern obtained after the sample is ground into powder, showing consistent peak positions and intensities. This indicates that the sample has high purity.
[0058] UV-Vis-Diffuse Reflectance Spectroscopy of Sample 1: Taking Sample 1 as a typical representative, the UV-Vis-Diffuse Reflectance spectroscopy of KBa3Zr2F was performed. 14 Cl was subjected to UV-Vis-diffuse reflectance spectroscopy measurements using a Varian Carry 5000 UV-Vis-NIR spectrophotometer. The crystal sample was ground into powder, with BaSO4 used as a reference. The test results are as follows: Figure 3 As shown, this indicates that compound KBa3Zr2F 14 Cl crystals have a wide transmission range, exhibiting high transmittance in the 200–800 nm spectral range, with an ultraviolet absorption cutoff wavelength below 200 nm.
[0059] Infrared spectroscopy test of sample in Example 1: Taking sample in Example 1 as a typical representative, the infrared spectrum of KBa3Zr2F was analyzed. 14 Infrared spectroscopy tests were performed on a Bruker TENSOR27 Fourier transform infrared spectrometer (BIR) from Germany. The test results are as follows: Figure 4 As shown, the positions of the characteristic peaks are consistent with the characteristics of this compound.
[0060] Thermogravimetric analysis of Sample 1 in Example 1: Taking Sample 1 as a typical representative, the thermogravimetric analysis of KBa3Zr2F was conducted. 14 Cl was subjected to infrared spectroscopy testing on a Netzsch STA449F3 thermogravimetric analyzer from Netzsch Equipment Manufacturing Co., Ltd., Germany. The results are as follows: Figure 5As shown, by Figure 5 It can be seen that the compound is stable up to 362℃.
[0061] Frequency doubling test experiment and results of sample 1 in Example 1: Taking sample 1 in Example 1 as a typical representative, the frequency doubling test of KBa3Zr2F was conducted. 14 The frequency doubling test of Cl was performed using the following steps: A Q-switched Nd:YAG solid-state laser with a frequency converter was used to generate a 1064nm wavelength laser as the fundamental frequency light, which was then used to irradiate the crystal powder under test. The generated second harmonic was detected using a photomultiplier tube, and the harmonic intensity was displayed on an oscilloscope. Crystal samples of different particle sizes were sieved using a standard sieve: 25-45μm, 45-75μm, 75-110μm, 110-150μm, 150-200μm, and 200-250μm. The trend of the frequency doubling signal intensity with particle size was observed to determine whether phase matching could be achieved. Under the same test conditions, the second harmonic intensity generated by the sample and the KDP sample was compared to obtain the relative magnitude of the frequency doubling effect of the sample. The test results show that compound KBa3Zr2F... 14 Cl crystals exhibit a significant frequency doubling effect; under 1064nm wavelength laser irradiation, the intensity of the frequency doubling signal is comparable to that of the control sample KDP crystal, and phase matching can be achieved. Figure 6 As shown.
[0062] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A deep ultraviolet bimetallic mixed halide nonlinear optical crystal material, characterized in that, The chemical formula of the crystalline material is KBa3Zr2F. 14 Cl belongs to the tetragonal crystal system and has space group 1. Cell parameters are α=β=γ=90°, Z=1, cell volume is 2. The method for preparing the deep ultraviolet bimetallic mixed halide nonlinear optical crystal material according to claim 1, characterized in that, The hydrothermal synthesis method includes the following steps: Step 1: Mix the K source, Ba source, Zr source, F source, Cl source and water to form the initial mixed raw material; Step 2: The initial mixed raw materials are placed in a closed reactor and crystallized under hydrothermal conditions of 190-220°C to obtain the crystalline material.
3. The preparation method according to claim 2, characterized in that, The molar ratio of K source, Ba source, Zr source, F source and Cl source in the initial mixed raw material is 1~3:1~3:1~2:1~2:6~12.
4. The preparation method according to claim 2, characterized in that, The crystallization time is 48 to 120 hours. After crystallization, the temperature is reduced to room temperature at a rate of 1 to 5 °C / h.
5. The preparation method according to any one of claims 2-4, characterized in that, The K source is one of potassium fluoride, potassium chloride, and potassium bromide; the Ba source is one of barium fluoride and barium chloride; the Zr source is zirconium fluoride; the F source is zirconium fluoride; and the Cl source is hydrochloric acid.
6. The application of the deep ultraviolet nonlinear optical crystal material according to claim 1 in the fabrication of laser frequency converters.