A semiconductor structure and a method of fabricating the same

By controlling the upper surface of the connecting ridge to be higher than the upper surface of the filling layer during the etching process of the semiconductor fins and filling layer, the sidewalls and top are exposed, which solves the problem of insufficient bit line process technology, realizes the formation of high-quality metal silicide, and improves the conductivity and signal transmission rate of the bit line.

CN116981247BActive Publication Date: 2026-11-20CHANGXIN MEMORY TECH INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210398939.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-15
Publication Date
2026-11-20
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

In the manufacturing process of advanced dynamic random access memory (DRAM), there are deficiencies in the bit line manufacturing technology, which affect the conductivity of the bit lines and the electrical properties and reliability of the chip.

Method used

By controlling the upper surface of the connecting ridge to be higher than the upper surface of the first filling layer during the etching process of the semiconductor fin and the first filling layer, the sidewalls and top of the connecting ridge are exposed, increasing the contact area between the metal and the substrate, and forming high-quality metal silicide.

Benefits of technology

It improves the quality of the bit lines, optimizes connectivity, reduces contact resistance, and increases the bit line signal transmission rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116981247B_ABST
    Figure CN116981247B_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure provide a preparation method of a semiconductor structure, the preparation method comprising: providing a structure to be processed, the structure to be processed comprising a semiconductor substrate, a plurality of semiconductor fins extending along a first direction on the semiconductor substrate, and a first filling layer filling gaps between the semiconductor fins; forming a first protective layer on the structure to be processed, and patterning the first protective layer; taking the patterned first protective layer as a mask, etching the semiconductor fins and the first filling layer along a second direction intersecting the first direction, so as to etch the semiconductor fins into a plurality of semiconductor columns and connecting ridges connecting adjacent semiconductor columns, wherein an upper surface of the connecting ridges is higher than upper surfaces of the first filling layers located on both sides of the connecting ridges.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of semiconductor technology, and in particular to a semiconductor structure and its fabrication method. Background Technology

[0002] As the integration density in semiconductor manufacturing processes continues to increase, improving the integration density of memory has become a trend. Consequently, the size of integrated circuits is gradually shrinking, which increases the difficulty of memory fabrication. In the manufacturing process of advanced dynamic random access memory (DRAM), the process technology level of the bit lines directly affects the conductivity of the bit lines, thereby affecting the chip's conduction capability and even seriously affecting the electrical performance and reliability of the chip in later stages.

[0003] However, there are still shortcomings in the current bit line manufacturing technology. How to optimize the bit line manufacturing technology is a technical problem that urgently needs to be solved at this stage. Summary of the Invention

[0004] This disclosure provides a method for fabricating a semiconductor structure, comprising: providing a structure to be processed, the structure to be processed including a semiconductor substrate, a plurality of semiconductor fins extending along a first direction on the semiconductor substrate, and a first filling layer filling the gaps between the semiconductor fins; forming a first protective layer on the structure to be processed, and patterning the first protective layer; using the patterned first protective layer as a mask, etching the semiconductor fins and the first filling layer along a second direction intersecting the first direction, so as to etch the semiconductor fins into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge.

[0005] In some embodiments, patterning the first protective layer includes: forming a first mask layer over the first protective layer; etching the first mask layer and the first protective layer to pattern the first mask layer and the first protective layer into a plurality of strip structures extending along a second direction; and removing the first mask layer.

[0006] In some embodiments, etching the first mask layer and the first protective layer includes: forming a second mask layer over the first mask layer; patterning the second mask layer to form a plurality of initial strip structures extending along the second direction, forming spacers with vertical sidewall morphology on the sidewalls of the initial strip structures; removing the initial strip structures; and etching the first mask layer and the first protective layer using the spacers as a mask.

[0007] In some embodiments, after etching the semiconductor fin and the first filler layer along the second direction, the method further includes: forming a second protective layer that at least covers the sidewalls of the semiconductor pillar and the top and sidewalls of the connecting ridge; and removing the second protective layer covering the top and sidewalls of the connecting ridge to expose the top and sidewalls of the connecting ridge.

[0008] In some embodiments, after removing the second protective layer covering the top and sidewalls of the connecting ridge, the method further includes: performing ion implantation to form doped regions on the exposed top and sidewalls of the connecting ridge and the lower portion of the semiconductor pillar, wherein the doped regions formed on the top and sidewalls of the connecting ridge and the lower portion of the semiconductor pillar are connected and extend along a first direction.

[0009] In some embodiments, after ion implantation, the method further includes: depositing a metal layer covering the exposed top and sidewalls of the doped region; performing a heat treatment to cause the metal layer to react with the doped region to form metal silicides on the top and sidewalls of the doped region, the metal silicides extending in a first direction as bit lines in the semiconductor structure; and removing the unreacted metal layer.

[0010] In some embodiments, after removing the unreacted metal layer, the method further includes forming a second filler layer that fills the gap between adjacent bit lines and covers the top and sidewalls of the bit lines.

[0011] In some embodiments, using the first protective layer as a mask, the semiconductor fin and the first filling layer are etched along a second direction intersecting the first direction to etch the semiconductor fin into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars. The upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge. This includes controlling the etching selectivity ratio of the semiconductor fin to the first filling layer, such that the etching rate of the first filling layer is greater than the etching rate of the semiconductor fin, so that after etching, the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge is 20-30 nm.

[0012] In some embodiments, the semiconductor fins and the first filler layer are etched along a second direction intersecting the first direction to etch the semiconductor fins into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filler layer located on both sides of the connecting ridge, including: controlling the etching conditions such that the height difference between the upper surface of the connecting ridge and the upper surface of the first filler layer located on both sides of the connecting ridge reaches 0.5 times to 1 times the thickness of the first protective layer.

[0013] This disclosure also provides a semiconductor structure, including: a semiconductor substrate; a plurality of semiconductor fins extending along a first direction on the semiconductor substrate, each semiconductor fin including a plurality of semiconductor pillars and a connecting ridge connecting adjacent semiconductor pillars, the upper surface of the connecting ridge being lower than the upper surface of the semiconductor pillar; a doped region extending along the first direction, the doped region being located at the top and sidewalls of the connecting ridge and the lower part of the semiconductor pillar; and a bit line extending along the first direction, the bit line covering a portion of the top and sidewalls of the doped region.

[0014] In some embodiments, the semiconductor structure further includes: a first filling layer that at least partially fills the gap between adjacent semiconductor fins, the upper surface of the connecting ridge being higher than the upper surface of the first filling layer located on both sides of the connecting ridge, and the top and sidewalls of the bit line being exposed from the first filling layer.

[0015] In some embodiments, the semiconductor structure further includes a second filling layer that fills the gaps between adjacent bit lines and covers the top and sidewalls of the bit lines.

[0016] In some embodiments, the first filler layer and the semiconductor fin have a high etch selectivity.

[0017] In some embodiments, the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge is 20-30 nm.

[0018] In some embodiments, the semiconductor structure further includes a first protective layer located above the semiconductor pillar.

[0019] In some embodiments, the ratio of the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge to the thickness of the first protective layer is 0.5-1.

[0020] In this embodiment, after etching the semiconductor fins and the first filler layer, the upper surface of the connecting ridge is made higher than the upper surface of the first filler layer located on both sides of the connecting ridge, thereby exposing the three surfaces of the connecting ridge: the sidewalls and the top. During the subsequent formation of the metal silicide, the metal can react with the substrate not only from the top of the connecting ridge but also from the sidewalls. This increases the contact area between the metal and the substrate, making it easier to form high-quality interconnected metal silicides. Furthermore, because the three surfaces of the connecting ridge—the sidewalls and the top—are simultaneously exposed, sufficient metal is ensured to participate in the reaction to form the metal silicide, solving the problem of insufficient metal content in the metal silicide reaction.

[0021] Additional aspects and advantages of this disclosure will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this disclosure. Attached Figure Description

[0022] To more clearly illustrate the technical solutions in the embodiments of this disclosure or in the conventional art, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 A flowchart illustrating a method for fabricating a semiconductor structure according to an embodiment of this disclosure;

[0024] Figure 2 This is a top view schematic diagram of a semiconductor structure provided in an embodiment of the present disclosure;

[0025] Figures 3a-18a For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken by line AA';

[0026] Figures 3b-18b For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken from line BB';

[0027] Figures 3c-18c For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken by line CC';

[0028] Figures 3d-18d For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken from line DD'.

[0029] Figure label:

[0030] 201-Semiconductor substrate; 203-Semiconductor substrate; 203-Semiconductor fin; 207-First filler layer; 209-Temperature oxide layer; 210-Strip structure; 211-First protective layer; 212-Bottom first mask layer; 213-First mask layer; 214-Top first mask layer; 215-Second mask layer; 215'-Initial strip structure; 216-Bottom second mask layer; 217-Spacer; 218-Top second mask layer; 219-Semiconductor pillar; 220-Photoresist layer; 221-Connecting ridge; 223-Second protective layer; 225-Doped region; 227-Metal layer; 229-Bit line; 231-Second filler layer;

[0031] The height difference between the upper surface of the H-connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge. Detailed Implementation

[0032] Exemplary embodiments of the present disclosure will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present disclosure are shown in the drawings, it should be understood that the present disclosure may be implemented in various forms and should not be limited to the specific embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.

[0033] In the accompanying drawings, for clarity, the dimensions of layers, areas, and elements, as well as their relative dimensions, may be exaggerated. The same reference numerals denote the same elements throughout.

[0034] It should be understood that when an element or layer is referred to as "on," "adjacent to," "connected to," or "coupled to" other elements or layers, it may be directly on, adjacent to, connected to, or coupled to other elements or layers, or there may be intervening elements or layers. Conversely, when an element is referred to as "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or portions, these elements, components, areas, layers, and / or portions should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or portion from another element, component, area, layer, or portion. Therefore, without departing from the teachings of this disclosure, the first element, component, area, layer, or portion discussed below may be referred to as a second element, component, area, layer, or portion. And the discussion of a second element, component, area, layer, or portion does not imply that the first element, component, area, layer, or portion necessarily exists in this disclosure.

[0035] Spatial relation terms such as “below,” “under,” “below,” “under,” “above,” “above,” etc., are used herein for convenience of description to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of the device in use and operation. For example, if the device in the figure is flipped, then the element or feature described as “below,” “under,” or “below” other elements or features will be oriented “above” other elements or features. Therefore, the exemplary terms “below” and “under” can include both above and below orientations. The device may be otherwise oriented (rotated 90 degrees or otherwise) and the spatial descriptive terms used herein will be interpreted accordingly.

[0036] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “comprise” and / or “comprising,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.

[0037] As the cell size of semiconductor devices (such as DRAM, Dynamic Random Access Memory) continues to shrink, the industry has adopted DRAM with a vertical transistor layout using a 4F2 architecture. In DRAM with a vertical transistor layout, the bit lines of the vertical transistors are typically located at the bottom of the semiconductor pillars. When forming bit lines at the bottom of the semiconductor pillars, metal can be deposited in the gaps between the pillars, and a silicide reaction occurs between the metal and the substrate, thus forming metal silicide bit lines at the bottom of the semiconductor pillars. Traditional metal silicide bit line fabrication processes struggle to form high-quality, fully interconnected metal silicides.

[0038] Based on this, the present disclosure provides a method for fabricating a semiconductor structure, as shown in the attached figure. Figure 1 The forming method includes:

[0039] Step 101: Provide a structure to be processed, the structure to be processed including a semiconductor substrate, a plurality of semiconductor fins extending along a first direction on the semiconductor substrate, and a first filling layer filling the gaps between the semiconductor fins.

[0040] Step 102: Form a first protective layer on the structure to be processed, and pattern the first protective layer.

[0041] Step 103: Using the patterned first protective layer as a mask, etch the semiconductor fin and the first filling layer along a second direction intersecting the first direction to etch the semiconductor fin into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge.

[0042] In this embodiment, after etching the semiconductor fins and the first filler layer, the upper surface of the connecting ridge is made higher than the upper surface of the first filler layer located on both sides of the connecting ridge, thereby exposing the three surfaces of the connecting ridge: the sidewalls and the top. During the subsequent formation of the metal silicide, the metal can react with the substrate not only from the top of the connecting ridge but also from the sidewalls. This increases the contact area between the metal and the substrate, making it easier to form high-quality interconnected metal silicides. Furthermore, because the three surfaces of the connecting ridge—the sidewalls and the top—are simultaneously exposed, sufficient metal is ensured to participate in the reaction to form the metal silicide, solving the problem of insufficient metal content in the metal silicide reaction.

[0043] Figure 2 This is a top view schematic diagram of a semiconductor structure provided in an embodiment of the present disclosure; Figures 3a-18a For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken by line AA'. Figures 3b-18b For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken from line BB'. Figures 3c-18c For each process step along Figure 2 A schematic diagram of the cross-sectional structure taken by line CC'. Figures 3d-18d For each process step along Figure 2 A cross-sectional structural diagram taken from line DD'. The manufacturing method of the semiconductor structure provided in the embodiments of this disclosure will be further described in detail below with reference to the accompanying drawings. In detailing the embodiments of this disclosure, for ease of explanation, the schematic diagrams may be partially enlarged without adhering to general proportions, and the schematic diagrams are merely examples and should not limit the scope of protection of this application.

[0044] First, as attached Figures 3a-3d As shown in 4a-4d and 5a-5d, step 101 is performed to provide a structure to be processed, the structure to be processed including a semiconductor substrate 203, a plurality of semiconductor fins 205 extending along a first direction on the semiconductor substrate 203, and a first filling layer 207 filling the gaps between the semiconductor fins 205.

[0045] The semiconductor substrate 203 and the semiconductor fins 205 may comprise at least one elemental semiconductor material, at least one III-V compound semiconductor material, at least one II-VI compound semiconductor material, at least one organic semiconductor material, or other semiconductor materials known in the art. In one specific embodiment, the semiconductor substrate is a silicon substrate, which may be doped or undoped. The material of the semiconductor fins 205 may be the same as the material of the semiconductor substrate 203. The material of the first filling layer 207 includes, but is not limited to, oxides, such as silicon oxide.

[0046] In some embodiments, as shown in the appendix Figures 3a-3dAs shown in 4a-4d and 5a-5d, the provision of the structure to be processed includes: providing a semiconductor substrate 201; etching the upper part of the semiconductor substrate 201 along a first direction to form a plurality of semiconductor fins 205 extending along the first direction, the lower part of the unetched semiconductor substrate 201 becoming a semiconductor substrate 203; filling the gap between adjacent semiconductor fins 205 with a first filling layer 207, the upper surface of the first filling layer 207 being flush with the upper surface of the semiconductor fins 205; thermally oxidizing the semiconductor fins 205 to form a thermally oxidized layer 209 on the upper surface of the semiconductor fins 205.

[0047] For details, see attached. Figures 3a-3d As shown, firstly: a semiconductor substrate 201 is provided. The semiconductor substrate may include at least one elemental semiconductor material (e.g., a silicon (Si) substrate, a germanium (Ge) substrate), at least one III-V compound semiconductor material, at least one II-VI compound semiconductor material, at least one organic semiconductor material, or other semiconductor materials known in the art.

[0048] Next, as attached Figures 4a-4d As shown, the upper part of the semiconductor substrate 201 is etched along a first direction to form a plurality of semiconductor fins 205 extending along the first direction, and the lower part of the unetched semiconductor substrate 201 becomes the semiconductor substrate 203. Here, a dry etching process can be used for the upper part of the semiconductor substrate, including physical etching, chemical etching, reactive ion etching, etc.

[0049] Next, as attached Figures 5a-5d As shown, a first filling layer 207 is used to fill the gap between adjacent semiconductor fins 205. The upper surface of the first filling layer 207 is flush with the upper surface of the semiconductor fins 205. The semiconductor fins 205 are thermally oxidized to form a thermal oxide layer 209 on the upper surface of the semiconductor fins 205. The first filling layer 207 can be filled using processes such as atomic layer deposition (ALD) or chemical vapor deposition (CVD). Optionally, after filling the gap between adjacent semiconductor fins 205 with the first filling layer 207, a planarization process, such as chemical mechanical polishing (CMP) and / or etching, can be used to make the upper surface of the first filling layer 207 coplanar with the upper surface of the semiconductor fins 205. The thermal oxide layer can be formed by in-situ thermal oxidation of the semiconductor fins 205, for example, it can be silicon oxide. The thermal oxide layer can protect the semiconductor pillars in subsequent processes.

[0050] In one embodiment, after forming a plurality of semiconductor fins 205 extending along a first direction, the method further includes: performing ion implantation on the semiconductor fins 205 to form a first source / drain doped region (not shown) and a second source / drain doped region (not shown) at the top and bottom of the semiconductor fins 205, respectively. In other embodiments, ion implantation may be performed on the semiconductor substrate 201 after providing the semiconductor substrate 201 to form a first doped region and a second doped region. After subsequently forming a plurality of semiconductor fins extending along the first direction, the first doped region is used to form the first source / drain doped region, and the second doped region is used to form the second source / drain doped region.

[0051] Next, proceed to step 102, see appendix. Figures 6a-6d Appendix Figures 7a-7d Appendix Figures 8a-8d Appendix Figures 9a-9d Appendix Figures 10a-10d and attached Figures 11a-11d A first protective layer 211 is formed on the structure to be processed, and the first protective layer 211 is patterned. The material of the first protective layer 211 includes, but is not limited to, nitrides, such as silicon nitride. In practice, the first protective layer 211 can be formed on the structure to be processed using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD). The patterning process includes, but is not limited to, self-aligned double patterning (SADP) and self-aligned quadruple patterning (SAQP). By providing a first protective layer on top of the structure to be processed, the subsequently formed semiconductor pillars can be effectively protected from oxidation, nitriding, damage, or contamination in subsequent processes.

[0052] In some embodiments, see Appendix Figures 6a-6d Appendix Figures 7a-7d Appendix Figures 8a-8d Appendix Figures 9a-9d Appendix Figures 10a-10d and attached Figures 11a-11d Patterning the first protective layer 211 includes: forming a first mask layer 213 above the first protective layer 211; etching the first mask layer 213 and the first protective layer 211 to pattern the first mask layer 213 and the first protective layer 211 into a plurality of strip structures 210 extending along a second direction; and removing the first mask layer 213.

[0053] In some embodiments, see Appendix Figures 7a-7d Appendix Figures 8a-8d Appendix Figures 9a-9d and attached Figures 10a-10dEtching the first mask layer 213 and the first protective layer 211 includes: forming a second mask layer 215 above the first mask layer 213; patterning the second mask layer 215 to form a plurality of initial strip structures 215' extending along the second direction, and forming spacers 217 with vertical sidewall morphology on the sidewalls of the initial strip structures 215'; removing the initial strip structures 215'; and etching the first mask layer 213 and the first protective layer 211 using the spacers 217 as a mask.

[0054] For details, please see the appendix. Figures 6a-6d First, a first mask layer 213 is formed above the first protective layer 211. In actual operation, the first mask layer 213 may include a bottom first mask layer 212 and a top first mask layer 214 stacked together, with the top first mask layer 214 located above the bottom first mask layer 212. The bottom first mask layer may include, but is not limited to, polycrystalline silicon or amorphous carbon, and the top first mask layer may include, but is not limited to, silicon oxynitride. Using a multilayer mask layer structure can improve linewidth consistency and edge roughness.

[0055] Next, see Appendix Figures 7a-7d A second mask layer 215 is formed above the first mask layer 213. In practice, the second mask layer 215 may include a bottom second mask layer 216 and a top second mask layer 218 stacked together, with the top second mask layer 218 located above the bottom second mask layer 216. The bottom second mask layer 216 may include, but is not limited to, a hard mask material, and the top second mask layer 218 may include, but is not limited to, silicon oxynitride. Using a multi-layer mask structure can improve linewidth consistency and edge roughness.

[0056] Next, see the appendix. Figures 8a-8d The second mask layer 215 is patterned to form a plurality of initial strip structures 215' extending along the second direction, and spacers 217 having vertical sidewall morphology are formed on the sidewalls of the initial strip structures 215'. In some embodiments, patterning the second mask layer 215 to form a plurality of initial strip structures 215' extending along the second direction includes: forming a photoresist layer 220 above the second mask layer 215 (see Appendix). Figures 7a-7dThe photoresist layer is patterned, and the patterned photoresist layer is used as a mask to etch the second mask layer 215. In practice, the photoresist layer 220 may also include a Si-containing anti-reflective coating (SiARC), which covers the surface of the second mask layer 215. This absorbs reflected light from the lithography process, improving the linewidth resolution in the lithography process. In some embodiments, a plurality of initial strip structures 215' are arranged in parallel at equal intervals, and the height and width of the plurality of initial strip structures may be the same. The width of the spacer may be, but is not limited to, half the width of the initial strip structure. The material of the spacer 217 may include, but is not limited to, oxides. In practice, a spacer layer covering the surface of the initial strip structure may be formed, the spacer layer covering the surface of the first mask layer and the spacer layer on the top of the initial strip structure may be removed, and the spacer layer on the sidewall of the initial strip structure may be retained to form a spacer with a vertical sidewall morphology.

[0057] Next, see Appendix Figures 9a-9d The initial strip structure 215' is removed. This removal can be achieved through wet etching, dry etching, or a combination thereof.

[0058] Then, see appendix. Figures 10a-10d Using spacer 217 as a mask, the first mask layer 213 and the first protective layer 211 are etched to pattern the first mask layer 213 and the first protective layer 211 into a plurality of strip structures 210 extending along the second direction. The first mask layer 213 and the first protective layer 211 can be patterned using wet etching or dry etching. In some embodiments, the plurality of strip structures 210 are arranged in parallel at equal intervals, and the height and width of the plurality of strip structures can be the same. The width of the strip structure 210 can be, but is not limited to, half the width of the initial strip structure. This effectively reduces the linewidth of the spacer, achieving a doubling of spatial pattern density, which can increase the density of subsequently formed semiconductor pillars, forming a more refined and accurate pattern, and improving registration accuracy.

[0059] Next, see Appendix Figures 11a-11d Remove the first mask layer 213. This can be done by wet etching, dry etching, or a combination thereof.

[0060] Then, proceed to step 103, see appendix. Figures 12a-12dUsing the patterned first protective layer 211 as a mask, the semiconductor fin 205 and the first filling layer 207 are etched along a second direction intersecting the first direction to etch the semiconductor fin 205 into a plurality of semiconductor pillars 219 and connecting ridges 221 connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge 221 is higher than the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221.

[0061] In some specific embodiments, using the first protective layer 211 as a mask, the semiconductor fin 205 and the first filling layer 207 are etched along a second direction intersecting the first direction to etch the semiconductor fin 205 into a plurality of semiconductor pillars 219 and connecting ridges 221 connecting adjacent semiconductor pillars. The upper surface of the connecting ridge 221 is higher than the upper surface of the first filling layer 207 located on both sides of the connecting ridge. This includes controlling the etching selectivity ratio of the semiconductor fin 205 to the first filling layer 207, such that the etching rate of the first filling layer 207 is greater than the etching rate of the semiconductor fin 205, so that after etching, the height difference H between the upper surface of the connecting ridge 221 and the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221 is 20-30 nm. For example, the height difference H between the upper surface of the connecting ridge 221 and the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221 can be, for example, 21 nm, 25 nm, or 28 nm. Thus, by utilizing the different etching rates of the first filling layer 207 and the semiconductor fin 205 during etching, the upper surface of the connecting ridge can be made higher than the upper surfaces of the filling layers on both sides of the connecting ridge in one step with high efficiency. If the height difference is too large, difficulties will arise in subsequent filling processes. If the height difference is too small, the area of ​​the exposed sides of the connecting ridge will be too small, which is not conducive to the subsequent formation of high-quality interconnected metal silicides.

[0062] In some embodiments, the semiconductor fin 205 and the first filler layer 207 are etched along a second direction intersecting the first direction to etch the semiconductor fin 205 into a plurality of semiconductor pillars 219 and connecting ridges 221 connecting adjacent semiconductor pillars 219, wherein the upper surface of the connecting ridge 221 is higher than the upper surface of the first filler layer 207 located on both sides of the connecting ridge 221. This includes controlling the etching conditions such that the height difference between the upper surface of the connecting ridge 221 and the upper surface of the first filler layer 207 located on both sides of the connecting ridge 221 reaches 0.5 to 1 times the thickness of the first protective layer 211. For example, the multiple by which the height difference between the upper surface of the connecting ridge 221 and the upper surface of the first filler layer 207 located on both sides of the connecting ridge 221 reaches the thickness of the first protective layer 211 can be, for example, 0.7, 0.8, or 0.9 times. If the multiple is too large, it is difficult to control the height difference between the connecting ridge and the filler layers on both sides. If the multiplier is too small, it will lead to low efficiency and will be difficult to achieve the desired height difference due to the limitation of the thickness of the first protective layer.

[0063] In some embodiments, see Appendix Figures 13a-13d and attached Figures 14a-14d After etching the semiconductor fin 205 and the first filler layer 207 along the second direction, the method further includes: forming a second protective layer 223, the second protective layer 223 at least covering the sidewalls of the semiconductor pillar 219 and the top and sidewalls of the connecting ridge 221; removing the second protective layer 223 covering the top and sidewalls of the connecting ridge 221, exposing the top and sidewalls of the connecting ridge 221. The material of the second protective layer 223 can be an oxide, specifically silicon oxide. The second protective layer can effectively protect the sidewalls of the semiconductor pillar, preventing the semiconductor pillar from being affected by subsequent ion implantation and by the metal and substrate silicide reaction.

[0064] In practice, the second protective layer 223 can be formed using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD) to cover the surface of the first filling layer 207, the semiconductor pillar 219, and the top and sidewalls of the connecting ridge 221. A reverse etching process can be used to remove the second protective layer 223 covering the top of the semiconductor pillar 219, the surface of the first filling layer 207, and the top and sidewalls of the connecting ridge 221.

[0065] In some embodiments, as shown in the appendix Figures 15a-15dAs shown, after removing the second protective layer 223 covering the top and sidewalls of the connecting ridge 221, the method further includes performing ion implantation to form doped regions 225 on the exposed top and sidewalls of the connecting ridge 221 and the lower portion of the semiconductor pillar 219. The doped regions 225 formed on the top and sidewalls of the connecting ridge 221 and the lower portion of the semiconductor pillar are connected and extend along a first direction. In other embodiments, the doped regions 225 may also be formed by a diffusion process.

[0066] In some embodiments, as shown in the appendix Figures 16a-16d and attached Figures 17a-17d As shown, after ion implantation, the method further includes: depositing a metal layer 227 covering the exposed top and sidewalls of the doped region 225; performing heat treatment to react the metal layer 227 with the doped region 225 to form metal silicides on the top and sidewalls of the doped region 225, the metal silicides extending along a first direction and serving as bit lines 229 in the semiconductor structure; and removing unreacted metal layers. The metal layer includes, but is not limited to, cobalt, titanium, or nickel. The metal silicides include, but are not limited to, cobalt silicide, titanium silicide, or nickel silicide. In practical operation, for energy consumption and yield considerations, the heat treatment temperature can be 600℃~700℃, for example, 630℃, 670℃, or 690℃. Metal silicides can effectively reduce contact resistance and improve bit line signal transmission rate. In this embodiment, the metal can react with the substrate not only from the top of the connecting ridge but also from the sidewalls, which increases the contact area between the metal and the substrate, making it easier to form high-quality interconnected metal silicides. Furthermore, by simultaneously exposing the three surfaces of the sidewalls and top of the connecting ridge, sufficient metal can participate in the reaction to form metal silicides, thus solving the problem of insufficient metal content in the metal silicide reaction.

[0067] In some embodiments, as shown in the appendix Figures 18a-18d As shown, after removing the unreacted metal layer, the process further includes forming a second filler layer 231. The second filler layer 231 fills the gaps between adjacent bit lines 229, covering the top and sidewalls of the bit lines. The material of the second filler layer 231 includes, but is not limited to, oxides, such as silicon oxide. The second filler layer serves as isolation and protection between bit lines. In practice, the second filler layer 231 can be formed using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD).

[0068] In some embodiments, after forming the second fill layer, the method further includes: removing the second protective layer to form a gate dielectric layer covering the sidewalls of the semiconductor pillar; forming a word line material layer on the second fill layer; and etching the word line material layer along a second direction to form a plurality of word lines extending along the second direction, the word lines enclosing the gate dielectric layer. In practice, the gate dielectric layer can be formed by converting a portion of the semiconductor pillar into an oxide through in-situ thermal oxidation. The material of the word lines includes, but is not limited to, tungsten, copper, titanium, tantalum, titanium nitride, tantalum nitride, metal silicides, metal alloys, or any combination thereof.

[0069] This disclosure also provides a semiconductor structure, as shown in the attached figure. Figures 18a-18d The structure includes: a semiconductor substrate 203; a plurality of semiconductor fins 205 extending along a first direction on the semiconductor substrate 203, each semiconductor fin 205 including a plurality of semiconductor pillars 219 and a connecting ridge 221 connecting adjacent semiconductor pillars 219, the upper surface of the connecting ridge 221 being lower than the upper surface of the semiconductor pillar 219; a doped region 225 extending along the first direction, the doped region being located at the top and sidewalls of the connecting ridge 221 and the lower part of the semiconductor pillars 219; and a bit line 229 extending along the first direction, the bit line 229 covering a portion of the top and sidewalls of the doped region 225. In some embodiments, the material of the bit line includes metal silicides, including but not limited to cobalt silicide, titanium silicide, or nickel silicide. This disclosure provides a semiconductor structure that improves the quality of bit lines, optimizes the connectivity of bit lines, reduces the contact resistance of bit lines, and improves the bit line signal transmission rate.

[0070] In some embodiments, the semiconductor structure further includes: a first filling layer 207, which at least partially fills the gap between adjacent semiconductor fins 205; the upper surface of the connecting ridge 221 is higher than the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221; and the top and sidewalls of the bit line 229 are exposed from the first filling layer 207. The material of the first filling layer 207 includes, but is not limited to, oxides, such as silicon oxide. The upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge, exposing the three surfaces of the connecting ridge: the sidewalls and the top. During the formation of the metal silicide, the metal can react with the substrate not only from the top of the connecting ridge but also from the sidewalls, which increases the contact area between the metal and the substrate, making it easier to form high-quality interconnected metal silicides. Furthermore, since the three surfaces of the connecting ridge—the sidewalls and the top—are exposed simultaneously, sufficient metal can participate in the reaction to form metal silicides, solving the problem of insufficient metal content in the metal silicide reaction.

[0071] In some embodiments, the semiconductor structure further includes a second fill layer 231, which fills the gaps between adjacent bit lines 229 and covers the top and sidewalls of the bit lines 229. The material of the second fill layer 231 includes, but is not limited to, oxides, such as silicon oxide. The second fill layer serves for isolation and protection between bit lines.

[0072] In some embodiments, the materials of the first filler layer 207 and the semiconductor fin 205 have a high etch selectivity. By utilizing the difference in etching rates between the first filler layer 207 and the semiconductor fin 205, the upper surface of the connecting ridge can be made higher than the upper surfaces of the filler layers on both sides of the connecting ridge in one step with high efficiency.

[0073] In some embodiments, the height difference between the upper surface of the connecting ridge 221 and the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221 is 20-30 nm. If the height difference is too large, difficulties will arise in subsequent filling processes. If the height difference is too small, the area of ​​the exposed sides of the connecting ridge will be too small, which is not conducive to the formation of high-quality interconnected metal silicides.

[0074] In some embodiments, the semiconductor structure further includes a first protective layer 211, which is located above the semiconductor pillar 219. By providing a first protective layer above the structure to be processed, the semiconductor pillars formed subsequently can be effectively protected from oxidation, nitriding, damage, or contamination in subsequent processes.

[0075] In some embodiments, the ratio of the height difference between the upper surface of the connecting ridge 221 and the upper surface of the first filling layer 207 located on both sides of the connecting ridge 221 to the thickness of the first protective layer 211 is 0.5-1. If the ratio is too large, it is difficult to control the height difference between the connecting ridge and the filling layers on both sides. If the ratio is too small, it will lead to low efficiency and is not conducive to achieving the desired height difference under the limitation of the thickness of the first protective layer.

[0076] In some embodiments, the semiconductor structure further includes a plurality of word lines extending along a second direction intersecting the first direction, the word lines being located above the second filler layer and enclosing the sidewalls of the semiconductor pillar. The material of the word lines includes, but is not limited to, tungsten, copper, titanium, tantalum, titanium nitride, tantalum nitride, metal silicides, metal alloys, or any combination thereof.

[0077] In some embodiments, the semiconductor structure further includes a gate dielectric layer located between the word line and the semiconductor pillar.

[0078] In summary, in this embodiment, after etching the semiconductor fins and the first filler layer, the upper surface of the connecting ridge is made higher than the upper surface of the first filler layer located on both sides of the connecting ridge, thereby exposing the three surfaces of the connecting ridge: the sidewalls and the top. During the subsequent formation of the metal silicide, the metal can react with the substrate not only from the top of the connecting ridge but also from the sidewalls. This increases the contact area between the metal and the substrate, making it easier to form high-quality interconnected metal silicides. Furthermore, because the three surfaces of the connecting ridge—the sidewalls and the top—are exposed simultaneously, sufficient metal is ensured to participate in the reaction to form the metal silicide, solving the problem of insufficient metal quantity in the metal silicide reaction.

[0079] It should be noted that the semiconductor structure, its formation method, and manufacturing apparatus provided in this disclosure can be applied to any integrated circuit including this structure. The technical features described in each embodiment can be arbitrarily combined without conflict. Those skilled in the art can change the order of the above-described formation method steps without departing from the scope of protection of this disclosure. In the embodiments of this disclosure, some steps can be executed simultaneously or sequentially without conflict.

[0080] The above description is merely a preferred embodiment of this disclosure and is not intended to limit the scope of protection of this disclosure. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure.

Claims

1. A method for fabricating a semiconductor structure, characterized in that, include: A structure to be processed is provided, the structure to be processed including a semiconductor substrate, a plurality of semiconductor fins extending along a first direction on the semiconductor substrate, and a first filling layer filling the gaps between the semiconductor fins; A first protective layer is formed on the structure to be processed, and the first protective layer is patterned. Using the patterned first protective layer as a mask, the semiconductor fin and the first filling layer are etched along a second direction intersecting the first direction to etch the semiconductor fin into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge. A second protective layer is formed, which at least covers the sidewalls of the semiconductor pillar and the top and sidewalls of the connecting ridge; Remove the second protective layer covering the top and sidewalls of the connecting ridge to expose the top and sidewalls of the connecting ridge; Ion implantation is performed to form doped regions on the top and sidewalls of the exposed connecting ridges, the doped regions formed on the top and sidewalls of the connecting ridges being connected and extending along a first direction; A metal layer is deposited, which covers the top and sidewalls of the doped region exposed. Heat treatment is performed to cause the metal layer to react with the doped region, thereby forming metal silicides on the top and sidewalls of the doped region. The metal silicides extend along a first direction and serve as bit lines in the semiconductor structure. Remove unreacted metal layers.

2. The preparation method according to claim 1, characterized in that, Patterning the first protective layer includes: A first mask layer is formed above the first protective layer; The first mask layer and the first protective layer are etched to pattern the first mask layer and the first protective layer into a plurality of strip structures extending along the second direction; Remove the first mask layer.

3. The preparation method according to claim 2, characterized in that, Etching the first mask layer and the first protective layer includes: A second mask layer is formed above the first mask layer; The second mask layer is patterned to form a plurality of initial strip structures extending along the second direction, and spacers with vertical sidewall morphology are formed on the sidewalls of the initial strip structures; Remove the initial strip structure; The first mask layer and the first protective layer are etched using the spacer as a mask.

4. The preparation method according to claim 1, characterized in that, After removing the unreacted metal layer, the process also includes: A second filler layer is formed, which fills the gap between adjacent bit lines and covers the top and sidewalls of the bit lines.

5. The preparation method according to claim 1, characterized in that, Using the patterned first protective layer as a mask, the semiconductor fins and the first filling layer are etched along a second direction intersecting the first direction to etch the semiconductor fins into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filling layer located on both sides of the connecting ridge, including: The etching selectivity ratio between the semiconductor fin and the first filling layer is controlled such that the etching rate of the first filling layer is greater than the etching rate of the semiconductor fin, so that the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge after etching is 20-30nm.

6. The preparation method according to claim 1, characterized in that, The semiconductor fins and the first filler layer are etched along a second direction intersecting the first direction to etch the semiconductor fins into a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars, wherein the upper surface of the connecting ridge is higher than the upper surface of the first filler layer located on both sides of the connecting ridge, including: The etching conditions are controlled such that the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge reaches 0.5 to 1 times the thickness of the first protective layer.

7. A semiconductor structure, characterized in that, include: Semiconductor substrate; A plurality of semiconductor fins extending along a first direction are located on the semiconductor substrate, each semiconductor fin including a plurality of semiconductor pillars and connecting ridges connecting adjacent semiconductor pillars; A doped region extending along a first direction, the doped region being located at the top and sidewalls of the connecting ridge; A bit line extending along a first direction, the bit line covering part of the top and sidewalls of the doped region; A first filler layer at least partially fills the gap between adjacent semiconductor fins, the upper surface of the connecting ridge is higher than the upper surface of the first filler layer located on both sides of the connecting ridge, and the top and sidewalls of the bit line are exposed from the first filler layer.

8. The semiconductor structure according to claim 7, characterized in that, The semiconductor structure also includes: A second filler layer fills the gaps between adjacent bit lines and covers the top and sidewalls of the bit lines.

9. The semiconductor structure according to claim 7, characterized in that, The first filling layer has a high etch selectivity with the semiconductor fin material.

10. The semiconductor structure according to claim 7, characterized in that, The height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge is 20-30 nm.

11. The semiconductor structure according to claim 7, characterized in that, The semiconductor structure also includes: A first protective layer is located above the semiconductor pillar.

12. The semiconductor structure according to claim 11, characterized in that, The ratio of the height difference between the upper surface of the connecting ridge and the upper surface of the first filling layer located on both sides of the connecting ridge to the thickness of the first protective layer is 0.5-1.

Citation Information

Patent Citations

  • Semiconductor structure and manufacturing method thereof

    CN107346759A

  • Semiconductor device and preparation method thereof

    CN111211170A