Silicon-carbon material, preparation method and application thereof

By depositing silicon and carbon in graphite to form a three-dimensional carbon framework structure, silicon-carbon materials have solved the problems of volume expansion and poor cycle performance of silicon-carbon materials in lithium-ion batteries, achieving a performance improvement of high initial efficiency and low expansion.

CN116995196BActive Publication Date: 2026-11-20CARBON ONE NEW ENERGY GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211032683.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2026-11-20
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

Existing silicon-carbon materials in lithium-ion batteries suffer from problems such as large volume expansion, easy capacity reduction, and poor cycle performance. In particular, silicon and carbon materials are prone to separation, leading to loss of conductivity and repeated damage to the SEI film.

Method used

By mixing graphite with an oxidant and an intercalating agent and then expanding it, silicon and carbon are deposited in the pores, between layers and on the outer surface of the graphite using chemical vapor deposition to form a three-dimensional carbon skeleton conductive hollow structure. The tightly bonded silicon-carbon material is then formed by pressing and crushing, and active lithium is added in conjunction with a lithium plating step.

Benefits of technology

It improves the cycle stability of silicon-carbon materials, suppresses volume expansion, enhances conductivity, improves the capacity and cycle performance of lithium-ion batteries, reduces damage to the SEI film, and improves the first coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003817742120000231
    Figure BDA0003817742120000231
Patent Text Reader

Abstract

The application discloses a silicon-carbon material and a preparation method and application thereof, wherein, graphite, an oxidizing agent and an intercalation agent are mixed to obtain intercalated expanded graphite, and the intercalated expanded graphite is calcined to obtain expanded graphite; in an inert atmosphere, silicon is deposited on the surface of the expanded graphite by using a chemical vapor deposition method to obtain a first composite material; in an inert atmosphere, carbon is deposited on the surface of the first composite material by using a chemical vapor deposition method to obtain a second composite material; and the second composite material is pressed and crushed to obtain the silicon-carbon material. The application realizes complete coating of the carbon material on the silicon nanoparticles by depositing a large amount of silicon nanoparticles in the pores and interlayers of the carbon material, so that the coating structure of carbon-silicon-carbon and the three-dimensional carbon skeleton conductive hollow structure effect are exerted, which is favorable for inhibiting expansion of the silicon-carbon material, reducing internal resistance, and significantly improving the capacity and cycle performance of a lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to materials for lithium-ion batteries, specifically to a silicon-carbon material, its preparation method, and its applications. Background Technology

[0002] Lithium-ion batteries are currently widely used in consumer electronics, electric vehicles, and large-scale energy storage, and their application markets are gradually expanding to areas such as medical electronics, power tools, drones, data centers, and national security. The rapid development of these different fields has played a significant role in promoting the development of high-energy-density batteries.

[0003] Since the beginning of the 21st century, the development of portable electronic information products has been rapid, placing increasingly stringent demands on the capacity of energy storage batteries. Traditional lithium-ion batteries are nearing their energy density limits, making it difficult to meet the needs of 3C products. Silicon, with a specific capacity of 4200 mAh / g, can significantly improve the energy density of lithium batteries when used as the negative electrode material.

[0004] However, silicon-containing silicon-carbon materials suffer from significant volume expansion, easily reduced capacity, and deteriorated cycle performance. When silicon expands, it can easily detach from the carbon material, forming "dead silicon," which loses its conductivity and leads to reduced capacity. When silicon comes into direct contact with the electrolyte, a solid electrolyte interface (SEI) film is formed. During expansion, the SEI film is easily and repeatedly damaged, leading to continuous consumption and dissolution of silicon, resulting in a decrease in the capacity of silicon-containing lithium-ion batteries.

[0005] WO2021179219A1 discloses an anode electrode and its preparation method, as well as a battery and electronic device using the electrode. The anode electrode includes a current collector and an active layer. The active layer includes a porous carbon framework and silicon nanoparticles and lithium metal located within the porous carbon framework. Regarding the preparation method of the anode electrode, a porous carbon framework sheet is placed in a CVD apparatus, and a silane-containing gas is introduced to deposit silicon nanoparticles, resulting in a deposited porous carbon framework sheet. Under a protective gas atmosphere, molten lithium metal is brought into contact with the deposited porous carbon framework sheet, causing the lithium metal to fill the pores of the deposited porous carbon framework sheet, thus obtaining the active layer. The active layer is placed on the current collector, and hot-pressed to bond the active layer and the current collector together, thus obtaining the anode electrode. However, in this method, the porosity and open porosity of the porous carbon may be insufficient, causing most of the nano-silicon particles to be deposited on the outer surface of the porous carbon material. That is, most of the nano-silicon particles may not exist in the pores or interlayers of the porous carbon material. This results in most of the lithium metal reacting with the nano-silicon particles on the outer surface of the porous carbon material and being deposited on the outer surface of the carbon material, rather than being completely covered by the carbon material. In addition, due to the viscosity and surface tension of molten lithium metal, it is difficult for lithium metal to enter the pores of the porous carbon material.

[0006] Chinese patent CN101339987 discloses a silicon-carbon composite anode material for lithium-ion batteries and its preparation method. This silicon-carbon composite anode material is a core-shell structure material, with elemental silicon accounting for 0.01-10% and carbon accounting for 90.99%. The silicon-carbon composite anode material is prepared by mixing silicon powder or polymer-coated material with graphite, followed by high-energy milling, then adding asphalt or polymer-coated material and ball milling, carbonization, and finally pulverization. However, because silicon mainly coats the outer surface of graphite, the bonding between silicon and carbon is weak. Furthermore, the silicon content is limited, which is detrimental to improving battery performance. Summary of the Invention

[0007] The technical problem to be solved by the present invention is: to provide a method for preparing silicon-carbon materials, thereby improving the cycle stability of silicon-carbon materials applied to lithium-ion batteries, reducing the volume expansion of lithium-ion batteries, and increasing the capacity of lithium-ion batteries.

[0008] The purpose of this invention is to provide a silicon-carbon material and its preparation method, wherein the silicon-carbon material has the properties of high initial efficiency, long cycle life, and low expansion.

[0009] The objective of this invention can be achieved using the following technical solutions:

[0010] This invention provides a method for preparing silicon-carbon materials, comprising the following steps:

[0011] (1) Graphite, oxidant and intercalating agent are mixed to obtain intercalated expanded graphite, and the intercalated expanded graphite is calcined to obtain expanded graphite; wherein the particle size Dn50 of the graphite is 5.0 to 100.0 μm, and the mass ratio of graphite, oxidant and intercalating agent is 1:(0.1 to 3.0):(1.0 to 10.0);

[0012] (2) In an inert atmosphere, silicon is deposited on the pores, interlayers, defects and outer surface of the expanded graphite prepared in step (1) by chemical vapor deposition to obtain the first composite material.

[0013] (3) In an inert atmosphere, carbon is deposited on the pores, interlayers, defects and outer surface of the first composite material prepared in step (2) by chemical vapor deposition to obtain the second composite material.

[0014] (4) The second composite material obtained in step (3) is pressed and crushed to obtain silicon-carbon material.

[0015] Preferably, the pressing pressure in step (4) is 150-450 MPa, and the pressing time is preferably 1.0-10.0 min.

[0016] Preferably, in the above-mentioned method for preparing silicon-carbon materials, after step (2) and before step (3), a lithium plating step (2a) is included: lithium vapor is deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain a first composite material with deposited lithium, which serves as the raw material for carbon deposition in step (3).

[0017] That is, the present invention also provides a method for preparing silicon-carbon materials, comprising the following steps:

[0018] (1) Graphite, oxidant and intercalating agent are mixed to obtain intercalated expanded graphite, and the intercalated expanded graphite is calcined to obtain expanded graphite.

[0019] (2) In an inert atmosphere, silicon is deposited on the pores, interlayers, defects and outer surface of the expanded graphite prepared in step (1) by chemical vapor deposition to obtain the first composite material.

[0020] (2a) Lithium vapor is deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain a first composite material with deposited lithium;

[0021] (3) In an inert atmosphere, carbon is deposited on the pores, interlayers, defects and outer surface of the first composite material with deposited lithium prepared in step (2a) by chemical vapor deposition to obtain the second composite material.

[0022] (4) The second composite material obtained in step (3) is pressed and crushed to obtain silicon-carbon material.

[0023] Preferably, in step (2a), lithium vapor is introduced into a vacuum evaporation furnace containing the first composite material, and the vacuum evaporation furnace is rotated at the same time, so that the lithium vapor comes into full and uniform contact with the first composite material, thereby depositing the lithium vapor in the pores, interlayers, defects and outer surface of the first composite material.

[0024] Preferably, the temperature of the lithium vapor is 1350–1800°C; or,

[0025] Preferably, the rotation speed of the vacuum evaporation furnace is 5.0–20.0 rpm; or,

[0026] Preferably, the vacuum degree of the vacuum evaporation is 0.01–0.09 MPa, more preferably 0.01–0.05 MPa; or,

[0027] In step (2a), the lithium plating content of the first composite material is 1 to 30 wt%, preferably 1 to 10 wt%.

[0028] Preferably, the temperature of the chemical vapor deposition method in step (2) is 400–1400°C, more preferably 400–1000°C; preferably, the heating rate of the chemical vapor deposition method is 1–15°C / min; more preferably, the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, the rotation speed of the furnace chamber is 0.5–10.0 rpm, preferably the rotation time is 0.5–20.0 h, more preferably 1.0–10.0 h; or,

[0029] In step (2), the silicon source gas is silane or silane; preferably, the silicon source gas charging rate is 10-100 L / h, more preferably the silicon source gas charging time is 0.5-20.0 h, and more preferably 1.0-10.0 h; or,

[0030] In step (2), the silicon content of the first composite material is 10-40 wt%, preferably 20-35 wt%.

[0031] Preferably, the temperature of the chemical vapor deposition method in step (3) is 400–1000°C; preferably, the heating rate of the chemical vapor deposition method is 1–15°C / min; more preferably, the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, the rotation speed of the furnace chamber is 0.5–10.0 rpm, and preferably the rotation time is 0.5–2.0 h; or,

[0032] In step (3), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, or propane; preferably, the carbon source gas charging rate is 5–50 L / h, and more preferably, the carbon source gas charging time is 0.5–2.0 h; or,

[0033] In step (3), the carbon coating content of the second composite material is 0.5 to 10 wt%, preferably 0.5 to 8 wt%.

[0034] Preferably, the graphite is one or more of natural graphite, artificial graphite, spherical graphite, and graphitic mesophase; preferably, the particle size Dn50 of the graphite is 5.0–100.0 μm; more preferably, it is 20.0–90.0 μm; or,

[0035] The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid, preferably potassium permanganate or potassium perchlorate; or,

[0036] The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and glacial acetic acid, preferably sulfuric acid or perchloric acid; or,

[0037] The mass ratio of graphite, oxidant and intercalating agent is 1:(0.1-3.0):(2.0-10.0).

[0038] Preferably, in step (1), the mixing is a stirring mixture, the stirring temperature is 10–60°C, preferably, the stirring time is 0.5–24.0 h, more preferably, the stirring speed is 100–3000 rpm; or,

[0039] The drying temperature is 30–80℃, and the drying time is 6.0–24.0 h; or,

[0040] The heating rate of the calcination is 1-20℃ / min, preferably 5-10℃ / min, and the holding temperature of the calcination is 500-850℃, preferably 0.3-6.0h, and the holding time is 0.5-2.0h.

[0041] Preferably, step (1) further includes a step of washing the intercalated expanded graphite before calcination, wherein the washing includes washing the intercalated expanded graphite with deionized water until the pH of the filtrate is 5-7; preferably, the washing further includes a drying step.

[0042] The present invention also provides a silicon-carbon material, which is prepared by the above-described method for preparing silicon-carbon material; preferably, the silicon content in the silicon-carbon material is 10-40 wt%, more preferably 20-35%; more preferably, the particle size Dn50 of the silicon-carbon material is 1-60 μm, preferably 5-30 μm, more preferably 7.0-25.0 μm, and even more preferably 7.5-24.7 μm.

[0043] The present invention also provides a negative electrode active material comprising the aforementioned silicon-carbon material.

[0044] The present invention also provides a lithium-ion battery negative electrode, which comprises the above-mentioned negative electrode active material, conductive agent and binder.

[0045] The present invention also provides a lithium-ion battery comprising the above-described lithium-ion battery negative electrode.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) In this invention, ordinary carbon materials such as graphite are expanded by modification and high-temperature treatment, which increases the interlayer space or pore size inside the carbon material and improves the porosity of the pores inside the carbon material, which is beneficial for subsequent vapor deposition steps. Then, silicon source gas is introduced for high-temperature pyrolysis, and various process conditions are strictly controlled. Vapor deposition of nano-silicon particles is carried out, which allows a large amount of silicon source gas and / or nano-silicon particles to enter the pores, interlayers and defects of the expanded graphite and other carbon materials for dense and uniform deposition, rather than just being deposited on the outer surface of ordinary graphite and other carbon materials. This is beneficial for improving the binding effect of silicon and carbon in silicon-carbon materials, so that silicon nanoparticles are stored inside the pores or interlayers of carbon materials. This three-dimensional carbon skeleton conductive hollow structure is beneficial for suppressing the expansion of silicon-containing anode materials and improving conductivity, and reducing internal resistance. This process is beneficial for improving battery capacity and cycle performance. Then, a carbon source gas is introduced for high-temperature pyrolysis, allowing for the vapor deposition of carbon nanoparticles into the expanded carbon material already deposited with silicon nanoparticles. This also allows a large amount of carbon source gas and / or carbon nanoparticles to enter the pores, interlayers, and defects of the expanded carbon material for deposition, completely coating the already deposited silicon nanoparticles. Simultaneously, carbon nanoparticles naturally deposit on the outer surface of the expanded carbon material, completely coating the silicon nanoparticles deposited on the outer surface. Finally, a pressing step is used, applying high pressure to make the bonding between silicon and carbon nanoparticles tighter and to close the pores or interlayer openings of the graphite material. This reduces the contact between silicon nanoparticles and the electrolyte, lowering silicon consumption and reducing repeated damage to the SEI film. By compressing and densifying the expanded voids and interlayer spaces of expanded graphite, the compaction density of silicon-carbon materials can be increased, achieving a comprehensive coating effect of carbon materials on silicon materials. This helps to suppress the expansion of silicon materials and reduce the internal resistance of the battery, thereby improving the cycle performance and capacity utilization of the battery. It also helps to avoid direct contact between silicon particles and electrolyte to prevent the formation of SEI film, thus avoiding or mitigating the dissolution and consumption of silicon, preventing excessive capacity reduction, and significantly improving the cycle performance of silicon-containing anode lithium batteries.

[0048] (2) Furthermore, by performing a lithium plating step after the silicon plating step (2) and before the carbon plating step (3), i.e., pre-replenishing the silicon-carbon material with lithium, it is possible to replenish the active lithium consumed or lost due to side reactions during the formation of the SEI film in the first charge-discharge cycle and during the long-term charge-discharge cycle, which is beneficial to improving the first coulombic efficiency of the lithium-ion battery and alleviating the capacity reduction.

[0049] (3) Compared with existing silicon-carbon materials with carbon-coated silicon structures, the silicon-carbon material of the present invention has a "sandwich" type carbon-silicon-carbon structure and a three-dimensional carbon skeleton conductive hollow structure. The silicon-carbon material of the present invention utilizes graphite materials and carbon nanoparticles to achieve complete coating of silicon nanoparticles or lithium silicon nanoparticles, leveraging the spatial effect of the three-dimensional carbon skeleton conductive hollow structure. This allows for buffering or self-absorption of the volume expansion effect of silicon particles during charging and discharging, alleviating or suppressing the expansion of the silicon-carbon material, preventing silicon particles from pulverizing and detaching from the carbon material surface to form "dead silicon," improving the charge-discharge cycle performance of lithium batteries containing the silicon-carbon material of the present invention, increasing the capacity of lithium batteries, improving the conductivity of silicon-containing anode materials, and mitigating the capacity reduction of silicon-containing anode lithium batteries during cycling. Detailed Implementation

[0050] In this specification, unless otherwise specified, the symbols, units, abbreviations, and terms have the following meanings. For example, when using ~ or - to indicate a numerical range, they include both endpoints, and the units are common. For example, 5~25% means more than 5% and less than 25%.

[0051] In this invention, Dn50 refers to the particle size corresponding to a cumulative particle size distribution percentage of 50% in a sample.

[0052] In this invention, the percentage of silicon coating on the first composite material refers to the percentage of the mass difference between the first composite material obtained by silicon coating on expanded graphite and the expanded graphite, relative to the mass of the first composite material.

[0053] In this invention, the carbon plating percentage of the second composite material refers to the percentage of the mass difference between the second composite material obtained by carbon plating the first composite material and the first composite material.

[0054] In this invention, the lithium plating percentage of the first composite material for lithium deposition refers to the percentage of the mass difference between the first composite material for lithium deposition obtained by lithium plating treatment and the first composite material itself, relative to the mass of the first composite material for lithium deposition.

[0055] In one specific embodiment of the present invention, a method for preparing silicon-carbon material is provided, comprising the following steps:

[0056] (1) Intercalated expanded graphite is obtained by mixing graphite, oxidant and intercalating agent, and expanded graphite is obtained by calcining the intercalated expanded graphite; wherein the particle size Dn50 of the graphite is 5.0 to 100.0 μm, and the mass ratio of graphite, oxidant and intercalating agent is 1:(0.1 to 3.0):(1.0 to 10.0), preferably 1:(0.1 to 3.0):(2.0 to 10.0);

[0057] (2) In an inert atmosphere, silicon is deposited on the surface of the expanded graphite obtained in step (1) by chemical vapor deposition. Preferably, silicon nanoparticles are deposited in the pores, interlayers, defects and outer surface of the expanded graphite to obtain the first composite material.

[0058] (3) In an inert atmosphere, carbon is deposited on the surface of the first composite material obtained in step (2) by chemical vapor deposition. Preferably, carbon nanoparticles are deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain the second composite material.

[0059] (4) The second composite material obtained in step (3) is pressed and crushed to obtain silicon-carbon material.

[0060] In a preferred embodiment of the present invention, after step (2) and before step (3), a lithium plating step (2a) is included: lithium vapor is deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain a first composite material with deposited lithium.

[0061] In step (2a), high-temperature lithium vapor is introduced into a vacuum evaporation furnace containing the first composite material, while the vacuum evaporation furnace is rotated to ensure that the lithium vapor comes into full and uniform contact with the first composite material, thereby depositing lithium vapor into the pores, interlayers, defects and outer surface of the first composite material to obtain a first composite material with deposited lithium.

[0062] Preferably, the temperature of the lithium vapor introduced into the vacuum evaporation process is 1350–1800°C, and more preferably 1350–1450°C.

[0063] Setting the temperature above 1350°C helps lithium vapor remain in a vapor state for a certain period before contacting the first composite material in the vacuum vapor deposition furnace. This allows sufficient lithium vapor to penetrate into the fully open pores, interlayer voids, or defects inside the expanded graphite, enabling adequate contact and reaction with the silicon nanoparticles already deposited inside the expanded graphite. Similarly, lithium vapor will also have adequate contact and reaction with the silicon nanoparticles already deposited on the outer surface of the expanded graphite. Setting the temperature below 1800°C, preferably below 1450°C, avoids excessive heat conduction to the silicon nanoparticles already deposited on the inner and outer surfaces, preventing the silicon particles from melting and liquefying, preventing the silicon nanocrystals from growing larger or agglomerating, and promoting uniform contact and alloying reaction between the silicon deposited particles and lithium nanoparticles.

[0064] Preferably, the vacuum evaporation is performed in a vacuum evaporation furnace.

[0065] Regarding the rotation speed of the vacuum evaporation furnace, there is no particular limitation as long as the lithium vapor can be fully mixed and contacted with the first negative electrode material. For example, it can be 5.0 to 20.0 rpm. If the rotation speed is too low, the bottom material may not be able to fully contact the lithium vapor, resulting in uneven lithium plating. If the rotation speed is too high, it may cause the rotation speed to be too fast and cause the material to stick to the wall, or it may affect the permeability of the lithium vapor in the furnace, resulting in uneven contact.

[0066] Regarding the vacuum level of the vacuum evaporation furnace, there is no particular limitation as long as it is conducive to the deposition reaction of lithium vapor in the vacuum evaporation furnace, for example, it is 0.01 to 0.09 MPa, preferably 0.01 to 0.05 MPa. Regarding the temperature of the vacuum evaporation furnace, there is no particular limitation as long as it is conducive to the deposition reaction of lithium vapor in the vacuum evaporation furnace and does not cause the deposited silicon nanoparticles to melt and agglomerate or the particle size of silicon nanocrystals to increase, for example, it can be 80 to 1000°C, preferably 80 to 800°C, more preferably 80 to 400°C.

[0067] By performing lithium vapor deposition after the silicon plating step, lithium can be pre-replenished on the negative electrode material, avoiding the loss of lithium due to lithium consumption during the formation or destruction of the SEI film. This is beneficial for improving the initial coulombic efficiency of lithium-ion batteries and enhancing the capacity retention rate of the battery during cycling.

[0068] For example, the first composite material is placed in a vapor deposition furnace, filled with an inert protective gas, and after replacing it with an inert protective atmosphere, a vacuum is drawn. The temperature is then increased to 80–400°C at a rate of 5–15°C / min. Lithium vapor at 1350–1800°C is then slowly and uniformly introduced at this temperature, while the furnace chamber is rotated at a speed of 5.0–20.0 rpm. After a given amount of lithium vapor has been introduced, the pressure is slowly restored to atmospheric pressure, and the temperature is lowered to room temperature (25°C). Under the protection of an inert atmosphere, the first composite material with deposited lithium is obtained. By strictly selecting specific process conditions and leveraging synergistic effects, the deposition efficiency of lithium vapor on the first composite material can be improved.

[0069] After the lithium plating step (2a), carbon vapor deposition is performed in an inert atmosphere, which can completely coat the deposited lithium nanoparticles or lithium-silicon alloy particles, thereby helping to avoid contact between the active lithium or lithium-silicon alloy and the organic solvent, and avoiding side reactions with the electrolyte.

[0070] Regarding the lithium plating percentage of the first composite material for lithium deposition in step (2a), it can be, for example, 1 to 30 wt%, preferably 2 to 10 wt%. If the lithium plating percentage is too low, it may not achieve the pre-lithiation effect; if the lithium plating percentage is too high, it may be difficult to achieve complete coating of lithium nanoparticles or lithium-silicon alloy particles by carbon materials, and it is easy for highly active lithium or lithium-silicon alloy to come into contact with the electrolyte, which can easily trigger side reactions, reduce battery performance, and also lead to higher costs.

[0071] The lithium vapor can be prepared, for example, from metallic lithium, crude lithium, or lithium salts.

[0072] Specifically, regarding the source of lithium vapor supply, there are no particular limitations as long as a uniform deposition of a specific amount of lithium can be achieved. For example, lithium vapor can be prepared by heating and melting metallic lithium in a crucible in an inert atmosphere and then evaporating it; alternatively, crude lithium can be distilled in a vacuum distillation tank in an inert atmosphere, and after filtration and / or removal of impurities using vacuum distillation, the lithium vapor can be condensed and collected, stored in a lithium storage tank, and then the lithium blocks in the storage tank can be heated and evaporated to prepare lithium vapor; alternatively, a thermal reduction method can be used, using one or more reducing agents selected from silicon powder, aluminum powder, iron powder, and carbon powder to reduce one or more lithium salts such as lithium carbonate, lithium hydroxide, or lithium oxide to generate lithium vapor, which can then be directly introduced into a vapor deposition tank after filtration and dust removal; the lithium vapor can also be further vacuum distilled to remove impurities before being introduced into a vapor deposition tank; or the lithium vapor after dust removal or impurity removal can be condensed and collected, stored in a lithium storage tank, and then heated and evaporated in a crucible in an inert atmosphere to prepare lithium vapor.

[0073] Regarding the vacuum degree of the distillation vessel, there is no particular limitation as long as it is conducive to introducing the lithium vapor generated in the distillation vessel into the vapor deposition furnace. For example, it can be greater than or equal to the vacuum degree of the vacuum vapor deposition furnace, for example, it can be 0.01 to 0.1 MPa, preferably 0.01 to 0.09 MPa.

[0074] The method of introducing lithium vapor is not particularly limited as long as the desired vapor deposition effect is achieved. For example, physical methods such as pressure difference or a fan can be used to introduce lithium vapor prepared in a distillation tank into the vapor deposition furnace. Regarding the amount of lithium vapor introduced, it is acceptable as long as the desired vapor deposition amount and effect are achieved. For example, as long as the lithium metal content accounts for 1-30% of the total mass of the lithium metal composite material, preferably 1-10%, more preferably 1.96-9.1%, there is no particular limitation. Considering physical losses such as wall adhesion losses, the amount of lithium vapor provided by the distillation tank is usually slightly greater than the given amount of lithium vapor introduced into the vapor deposition furnace, as long as it ensures that the given amount of lithium vapor is introduced and deposited on the first composite material.

[0075] The lithium vapor charging flow rate can be adjusted by adjusting the amount of lithium raw material input, or by adjusting the melting temperature or reaction temperature. In addition, by adjusting the temperature and rotation speed of the vapor deposition furnace, as well as the material dispersion state caused by the rotation, there is no particular limitation on the lithium vapor charging flow rate as long as the expected vapor deposition reaction effect can be achieved.

[0076] There is no particular limitation on the charging time of lithium vapor, as long as the expected deposition amount and evaporation effect can be achieved. For example, it can be 0.5 to 12.0 h, preferably 0.5 to 5.0 h, and preferably all the prepared lithium vapor is charged into the evaporation furnace.

[0077] There are no particular limitations on the inner liner of the distillation tank or the vapor deposition furnace, as long as the expected effect can be achieved. For example, it can be made of ceramic material or corundum material.

[0078] Optionally, by moderately performing vapor-phase lithium plating on the first composite material on which silicon has already been deposited, i.e., pre-lithiating the silicon-carbon material, it is beneficial to further improve the capacity of the silicon-carbon anode material. This can replenish the active lithium consumed due to the formation or destruction of the SEI film, slow down capacity decay, and improve the battery's initial coulombic efficiency, rate discharge performance, and cycle performance.

[0079] In another preferred embodiment of the present invention, in step (1), graphite, oxidant and intercalating agent are mixed to obtain a mixture, the mixture is stirred to obtain intercalated expanded graphite, the intercalated expanded graphite is repeatedly washed with deionized water until the pH of the filtrate is between 5 and 7, the washed intercalated expanded graphite is dried, and then calcined in an inert atmosphere to obtain expanded graphite.

[0080] In the above-described method for preparing expanded graphite, mixing and stirring are performed to ensure that the intercalating agent and oxidizing agent fully impregnate the pores and interlayers of the graphite carbon material. Excess oxidizing agent and intercalating agent are removed through repeated washing, for example, 2 to 10 times. The washing process continues until the pH of the filtrate is 5 to 7. If the pH is too low after washing, the expansion degree may be too large; if the pH is too high, the intercalating agent may excessively detach from the carbon material, resulting in insufficient subsequent expansion. The moisture in the intercalated expanded graphite is removed by drying, followed by calcination, which oxidizes the intercalating agent to generate gas, causing the graphite to expand and modify, thus obtaining expanded graphite.

[0081] In the above-mentioned method for preparing expanded graphite, the stirring temperature is 10-60℃, the stirring time is 0.5-24.0h, and the stirring speed is 100-3000rpm. As long as the desired stirring effect can be achieved, the stirring conditions are not particularly limited.

[0082] The drying temperature of the washed intercalated expanded graphite is 30-80℃, and the drying time is 6.0-24.0h. As long as the predetermined drying effect can be achieved, the drying conditions are not particularly limited.

[0083] The heating rate of the calcination is 1-20℃ / min, preferably 5-10℃ / min, the holding temperature of the calcination is 500-850℃, and the holding time is 0.3-6.0h, preferably 0.5-2.0h.

[0084] Regarding the calcination and holding temperature and time, there are no particular limitations as long as the graphite can expand sufficiently, resulting in a significant opening of the graphite pore space and a significant widening of the interlayer spacing. For example, the holding temperature can be 500–850℃. If the calcination and holding temperature is too low, the expansion may be insufficient, and the modification effect obtained by the oxide intercalation may be inadequate. If the temperature is too high, the expansion may be excessive, resulting in too many breakages and defects, making it difficult to control the process reaction, easily causing various side reactions, introducing too many impurity atoms, and hindering subsequent vapor-phase silicon deposition.

[0085] The graphite is one or more of natural graphite, artificial graphite, spherical graphite, and graphite mesophase. The particle size Dn50 of the graphite is 5.0-100.0 μm, preferably 20.0-90.0 μm, and more preferably 20.0-60.0 μm. When the particle size is too small, the particle size of the final product obtained after pressing and crushing is too small, and the specific surface area is too large, which is not conducive to the performance of battery capacity. When the particle size is too large, the slurry preparation process is difficult to control, and uneven particle distribution is likely to occur in the coating process.

[0086] The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid, preferably potassium permanganate and potassium perchlorate;

[0087] The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid and glacial acetic acid, preferably sulfuric acid or perchloric acid;

[0088] The mass ratio of graphite to oxidant to intercalating agent is 1:(0.1-3.0):(1.0-10.0), preferably 1:(0.1-3.0):(2.0-10.0), and more preferably 1:(0.1-2.0):(2.0-5.0). The amount of intercalating agent is, for example, 1-10 times the amount of graphite. If the amount of intercalating agent is too small, it is difficult to stir and mix evenly, making intercalation difficult and resulting in poor expansion and modification effects. If the amount of intercalating agent is too large, it increases process costs, prolongs drying time, and may cause excessive expansion. The amount of oxidant is, for example, 0.1-3.0 times the amount of graphite. If the amount of oxidant is too small, the expansion degree is too low, resulting in insufficient modification. If the amount of oxidant is too large, the expansion may become excessive, increasing preparation costs and impurities.

[0089] The strong acid treatment causes a certain degree of etching on the graphite surface, resulting in structural defects and uneven morphology, which is beneficial for the deposition of silicon in subsequent processes and enhances the strong adsorption between carbon and silicon.

[0090] By utilizing the aforementioned oxide intercalation modification and high-temperature calcination treatments, the oxygen-containing groups inserted or introduced between the graphite layers undergo pyrolysis, causing the graphite material to expand significantly. This expands the graphite sheets, facilitating subsequent vapor-phase deposition. The expansion rate of graphite can be several times or even more than ten times, resulting in significantly higher porosity and interlayer spacing compared to current porous carbon materials.

[0091] In another preferred embodiment of the present invention, in step (2), the expanded graphite material is placed in a chemical vapor deposition furnace, a vacuum is drawn, an inert protective gas is introduced at a rate of 10 to 100 L / h, and the temperature is raised to 400 to 1400°C, preferably 400 to 1000°C, at a rate of 1 to 15°C / min; then a silicon source gas is introduced at a rate of 10 to 100 L / h, the cavity of the chemical vapor deposition furnace is rotated at a speed of 0.5 to 10.0 rpm, and the temperature is maintained and rotated for 0.5 to 20.0 h, preferably 1.0 to 10.0 h, and then the introduction of silicon source gas is stopped and the temperature is lowered to room temperature to obtain a first composite material in which silicon nanoparticles are deposited in the pores, interlayers, defects and outer surface of the expanded graphite.

[0092] The inert protective gas is one or more of argon, helium, xenon, radon, and neon.

[0093] The silicon source gas is silane or ethyl silane.

[0094] By depositing silicon nanoparticles (hereinafter also referred to as silicon plating) on ​​the inner and outer surfaces of graphite, the battery capacity of the final product can be increased. Regarding the proportion of silicon plating in step (2), from the viewpoint of suppressing silicon expansion and improving battery performance, the proportion of silicon plating in the first composite material is 10-40%, preferably 20-35%, and more preferably 21.13-33.24%. If the amount of silicon plating is too large, it may be difficult to achieve complete coating of silicon particles by carbon materials or carbon nanoparticles, and the spatial effect of the carbon-silicon-carbon "sandwich" type coating structure cannot be fully utilized. This can easily lead to excessively large particle size of silicon particles and excessively thick silicon layer on the surface, making it difficult to suppress the expansion of silicon, causing repeated damage to the SEI film and excessive consumption of lithium ions, thereby affecting the cycle performance of the battery. If the amount of silicon plating is too small, it may result in insufficient capacity and fail to take advantage of the capacity of silicon-carbon materials.

[0095] Regarding the temperature of the chemical vapor deposition furnace in the silicon chemical vapor deposition step, it can be, for example, 400–1400°C, preferably 400–1000°C. If the temperature is too low, the silicon source gas will not be sufficiently decomposed, which may lead to poor silicon vapor deposition effect, especially the inability to fully deposit in the internal pores or interlayer of the expanded graphite. If the temperature is too high, it will increase the difficulty of process control and the energy consumption cost will be higher. When the temperature is close to or exceeds the melting point of silicon, 1410°C, the silicon nanoparticles deposited on the surface of the carbon material will melt and stick together, which may form a mass. This is not conducive to the formation of a good bond between carbon and silicon, resulting in poor expansion inhibition effect and cycle performance.

[0096] In another preferred embodiment of the present invention, in step (3), the first composite material is placed in a chemical vapor deposition furnace in an inert protective gas atmosphere, a vacuum is drawn, and the temperature is raised to 400-1000°C, preferably 500-900°C, at a rate of 1-15°C / min. Then, carbon source gas is introduced at a rate of 5-50L / h, and the cavity of the chemical vapor deposition furnace is rotated at a speed of 0.5-10.0rpm. The furnace is kept warm and rotated for 0.5-2.0h, and then the introduction of carbon source gas is stopped and the temperature is lowered to room temperature to obtain a second composite material with carbon further coated on the surface of silicon.

[0097] The carbon source gas includes one or more of methane, ethylene, acetylene, propylene, or propane;

[0098] The inert protective gas is one or more of argon, helium, xenon, radon, and neon.

[0099] Carbon plating on the first composite material where silicon has already been deposited helps protect the deposited silicon nanoparticles. This is because silicon reacts with the electrolyte, causing it to dissolve and be lost, thus reducing battery capacity. Carbon plating also increases the conductivity of the final product, reduces silicon expansion, and minimizes unwanted side reactions.

[0100] Carbon deposition of the first composite material using a vapor-phase coating method leverages the extremely small particle size and strong penetrating power of the gaseous carbon source gas or carbon nanoparticles. This allows for easy entry into the pores and interlayers of the carbon material for carbon deposition, facilitating comprehensive and uniform coating of the first composite material and promoting the reaction or adsorption coating between silicon nanoparticles and carbon nanoparticles. In contrast, solid-phase or liquid-phase coating methods, using common coating agents such as asphalt, resin, or organic solutions with large particle sizes or viscosity, are less effective at penetrating the fine pores and interlayers of the carbon material, especially deep within the pores. This makes comprehensive and uniform coating of the first composite material difficult to achieve and therefore less preferable than vapor-phase coating.

[0101] Regarding the temperature of the chemical vapor deposition furnace during carbon plating, for example, it can be 400-1000℃. If the temperature is too low, the carbon source gas will not be fully decomposed, which may lead to poor carbon vapor deposition effect, especially the inability to fully deposit carbon in the internal pores or interlayers of the first composite material. If the temperature is too high, it will increase the difficulty of process control and increase energy consumption costs.

[0102] Regarding the chemical vapor deposition furnace in step (3), the chemical vapor deposition furnace that has undergone silicon plating in step (2) can also be used without affecting the effect of the invention, so as to improve the continuity of production.

[0103] Regarding the carbon plating percentage of the second composite material in step (3), from the viewpoint of suppressing silicon expansion and improving battery performance, the carbon plating percentage of the second composite material is preferably 0.5-10%, more preferably 0.5-8%, and even more preferably 1-7%. If the carbon plating amount is too high, the carbon content in the silicon-carbon material will increase, the energy density will decrease, the battery capacity will decrease, and the carbon layer coated on the silicon will be too thick, which may hinder the passage of lithium ions. If the carbon plating amount is too low, the deposited silicon nanoparticles cannot be completely coated, which may lead to the contact between the silicon particles and the electrolyte and side reactions, resulting in silicon consumption and capacity reduction.

[0104] In another preferred embodiment of the present invention, in step (4), the second composite material obtained in step (3) is pressed and crushed to obtain silicon-carbon material.

[0105] This invention employs an extruder or isostatic press for pressing. The pressing pressure can be, for example, 150–450 MPa, and the pressing time can be, for example, 1–10 minutes. Setting a higher pressure during pressing helps to achieve a tighter bond between silicon and carbon nanoparticles and closes the pores or interlayer openings of the graphite material. This reduces the contact between silicon nanoparticles and the electrolyte, decreasing silicon consumption and repeated damage to the SEI film. By compressing and densifying the expanded voids and interlayer spaces of the expanded graphite, the compaction density of the silicon-carbon material is increased.

[0106] This invention employs commonly used pulverizing machines such as mechanical pulverizers, air jet mills, ball mills, or grinding mills for uniform pulverization. The compressed, block-shaped material is thoroughly and uniformly pulverized, preferably to a particle size smaller than that of the raw graphite. Regarding pulverization time and conditions, there are no particular limitations as long as the particle size Dn50 after grinding is ensured to be 1–60 μm, preferably 5–30 μm, more preferably 7.0–25.0 μm, and even more preferably 7.5–24.7 μm. The pulverization time can be, for example, 0.5–5.0 h, preferably 1.0–3.0 h. Various pulverizing machines or methods can be used, including, for example, jaw crushers, mechanical pulverizers, air jet mills, ball mills, or grinding mills.

[0107] After the pressing and crushing steps, further post-processing such as grading, sieving, and demagnetization can be carried out before packaging and discharge.

[0108] The present invention also provides a silicon-carbon material, which is prepared by the above-described method for preparing silicon-carbon materials.

[0109] In the aforementioned silicon-carbon material, the silicon content is 10-40%, preferably 20-35%. Specifically, the silicon content in the first composite material is 10-40%, preferably 20-35%. Since the mass difference between the second composite material and the first composite material is relatively small, the fluctuation of the mass percentage of each component after the carbon plating step can be basically ignored; that is, the silicon content in the second composite material can be considered to be 10-40%, preferably 20-35%. Further, the mass percentage of silicon in the silicon-carbon material can be considered to be 10-40%, preferably 20-35%.

[0110] Among the aforementioned silicon-carbon materials, the specific surface area measured using a BET surface area analyzer ranges from 0.5 to 5.0 m². 2 / g.

[0111] The particle size Dn50 of the silicon-carbon material is, for example, 1–60 μm, preferably 5–30 μm, more preferably 7.0–25.0 μm, and even more preferably 7.5–24.7 μm. If the particle size is too small, the specific surface area will be too large, which may lead to an increase in side reactions in the electrolyte and a decrease in capacity; if the particle size is too large, large particles and unevenness are likely to occur during slurry preparation, making the coating process difficult to control, resulting in poor ion conduction and hindering the performance of lithium battery cycle life.

[0112] The present invention also provides a negative electrode active material comprising the above-mentioned silicon-carbon material.

[0113] The present invention also provides an active negative electrode for a lithium-ion battery, which comprises the above-mentioned negative electrode material, a conductive agent and a binder.

[0114] The present invention also provides a lithium-ion battery, wherein it comprises the above-described lithium-ion battery negative electrode.

[0115] To better understand the above technical solution, the present invention will be further described in detail below.

[0116] All raw materials and reagents used in this invention were purchased from mainstream manufacturers on the market. Those without a specified manufacturer or concentration are all analytical grade raw materials or reagents that are routinely available. There are no particular restrictions as long as they achieve the intended effect. For example, natural graphite was purchased from BTR Corporation; silane and other reagents were purchased from Guangzhou Spectrum Gas Co., Ltd.; acetylene and other reagents were purchased from Shenzhen Huataipeng Special Gas Co., Ltd.; potassium permanganate, concentrated sulfuric acid, and other reagents were purchased from Aladdin Reagent Network.

[0117] The mixer, drying equipment, chemical vapor deposition furnace, isostatic press, pulverizer, and other instruments and equipment used in this embodiment were all purchased from major manufacturers on the market. As long as they can achieve the expected results, there are no particular limitations. For example, the chemical vapor deposition (CVD) furnace was purchased from Shenzhen Kejing Zhida Technology Co., Ltd.

[0118] Unless otherwise specified in this embodiment, the techniques or conditions described in the literature in this field or in accordance with the product manual shall apply.

[0119] The present invention will now be described in more detail with reference to examples and comparative examples, but the scope of the present invention is not limited to these examples. It should be noted that, unless otherwise specified, all percentages, parts, and ratios used in the present invention are based on mass.

[0120] Example 1

[0121] (I) Preparation of Expanded Graphite

[0122] 100.0g of natural graphite (particle size Dn50 of 20.0μm), 10.0g of potassium permanganate, and 200.0g of sulfuric acid (98wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 10℃ for 24.0h at a stirring speed of 100rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 5.0. The washed intercalated expanded graphite was then dried at 30℃ for 24.0h, and then calcined at 500℃ for 2.0h under a nitrogen atmosphere at a heating rate of 5℃ / min to obtain 94.4g of expanded graphite.

[0123] (II) Preparation of the first composite material

[0124] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.01MPa, and argon was introduced at a rate of 10L / h. The temperature was increased to 400℃ at a rate of 1℃ / min, and then silane was introduced at a rate of 10L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 0.5rpm and kept at the temperature for 10.0h. Then the introduction of silane was stopped, and the temperature was lowered to 25℃ to obtain 63.4g of the first composite material with silicon coated on the surface of the expanded graphite.

[0125] The silicon content of the first composite material is calculated to be 21.13% according to the following formula.

[0126] Silicon plating percentage = (mass of first composite material - mass of expanded graphite) / mass of first composite material * 100%.

[0127] (III) Preparation of the second composite material

[0128] In an argon atmosphere, 50.0 g of the first composite material was placed in another chemical vapor deposition furnace. The furnace was evacuated to 0.01 MPa and heated to 500 °C at a rate of 1 °C / min. Acetylene was then introduced at a rate of 5 L / h, and the furnace chamber was rotated at 0.5 rpm. The furnace was kept at this temperature and rotated for 2.0 h. Then, the acetylene introduction was stopped, and the temperature was lowered to 25 °C, yielding 50.5 g of a second composite material further coated with carbon on the surface of the first composite material. The carbon content of the second composite material was calculated to be 0.99% according to the following formula.

[0129] Carbon coating percentage = (mass of second composite material - mass of first composite material) / mass of second composite material * 100%.

[0130] (iv) Preparation of silicon-carbon materials

[0131] The second composite material was pressed at 150 MPa for 10.0 min using an isostatic press, and then pulverized for 3.0 h using a pulverizer at a speed of 300 rpm, a ball-to-material ratio of 5:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 7.5 μm using a laser particle size analyzer.

[0132] Example 2

[0133] (I) Preparation of Expanded Graphite

[0134] 100.0 g of natural graphite (particle size Dn50 of 90.0 μm), 300.0 g of potassium permanganate, and 1000.0 g of sulfuric acid (98 wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 60 °C for 0.5 h at a stirring speed of 3000 rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 7.0. The washed intercalated expanded graphite was then dried at 80 °C for 6.0 h, and then calcined at 850 °C for 0.5 h in a nitrogen atmosphere at a heating rate of 10 °C / min to obtain 92.3 g of expanded graphite.

[0135] (II) Preparation of the first composite material

[0136] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.05MPa, and argon gas was introduced at a rate of 100L / h. The temperature was increased to 1000℃ at a rate of 15℃ / min, and then silane was introduced at a rate of 100L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 10.0rpm and kept at this temperature for 1.0h. Then, the introduction of silane was stopped, and the temperature was lowered to 25℃ to obtain 69.8g of a first composite material with silicon coated on the surface of the expanded graphite. The silicon coating percentage of the first composite material was calculated to be 28.4% according to the formula in Example 1.

[0137] (III) Preparation of the second composite material

[0138] In an argon atmosphere, 50.0g of the first composite material was placed in another chemical vapor deposition furnace, evacuated to 0.05MPa, heated to 900℃ at a rate of 15℃ / min, and then acetylene was introduced at a rate of 50L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 10.0rpm, and the furnace was kept at the temperature and rotated for 0.5h. Then, the acetylene introduction was stopped, and the temperature was lowered to 25℃ to obtain 52.9g of a second composite material with carbon further coated on the surface of the first composite material.

[0139] The carbon content of the second composite material is calculated to be 5.5% according to the formula in Example 1.

[0140] (iv) Preparation of silicon-carbon materials

[0141] The second composite material was pressed at 450 MPa for 1.0 min using an isostatic press, and then pulverized for 1.0 h using a pulverizer at a speed of 500 rpm, a ball-to-material ratio of 10:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 24.7 μm using a laser particle size analyzer.

[0142] Example 3

[0143] (I) Preparation of Expanded Graphite

[0144] 100.0 g of natural graphite (particle size Dn50 of 50.0 μm), 100.0 g of potassium permanganate, and 500.0 g of sulfuric acid (98 wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 30 °C for 12.0 h at a stirring speed of 1500 rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 6.0. The washed intercalated expanded graphite was then dried at 50 °C for 15.0 h, and then calcined at 700 °C for 1.0 h in a nitrogen atmosphere at a heating rate of 8 °C / min to obtain 93.6 g of expanded graphite.

[0145] (II) Preparation of the first composite material

[0146] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.02MPa, and argon gas was introduced at a rate of 50L / h. The temperature was increased to 700℃ at a rate of 10℃ / min, and then silane was introduced at a rate of 50L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 5.0rpm and kept at this temperature for 3.0h. Then, the introduction of silane was stopped, and the temperature was lowered to 25℃ to obtain 74.9g of a first composite material with silicon coated on the surface of the expanded graphite. The silicon coating percentage of the first composite material was calculated to be 33.24% according to the formula in Example 1.

[0147] (III) Preparation of the second composite material

[0148] In an argon atmosphere, 50.0 g of the first composite material was placed in another chemical vapor deposition furnace, evacuated to 0.02 MPa, and heated to 700 °C at a rate of 5 °C / min. Acetylene was then introduced at a rate of 30 L / h, and the furnace chamber was rotated at 0.5 rpm. The furnace was kept at this temperature and rotated for 1.5 h. Then, the acetylene introduction was stopped, and the temperature was lowered to 25 °C, yielding 53.8 g of a second composite material further coated with carbon on the surface of the first composite material. The carbon content of the second composite material was calculated to be 7.06% according to the formula in Example 1.

[0149] (iv) Preparation of silicon-carbon materials

[0150] The second composite material was pressed at 300 MPa for 5.0 min using an isostatic press, and then pulverized for 2.0 h using a pulverizer at a speed of 450 rpm, a ball-to-material ratio of 7:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 14.1 μm using a laser particle size analyzer.

[0151] Example 4

[0152] (I) Preparation of Expanded Graphite

[0153] 100.0 g of artificial graphite (particle size Dn50 of 60.0 μm), 50.0 g of potassium perchlorate, and 700.0 g of sulfuric acid (98 wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 40 °C for 10.0 h at a stirring speed of 500 rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 6.0. The washed intercalated expanded graphite was then dried at 60 °C for 10.0 h, and then calcined at 600 °C for 1.0 h in a nitrogen atmosphere at a heating rate of 20 °C / min to obtain 93.0 g of expanded graphite.

[0154] (II) Preparation of the first composite material

[0155] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.01MPa, and argon gas was introduced at a rate of 10L / h. The temperature was increased to 850℃ at a rate of 5℃ / min, and then silane was introduced at a rate of 50L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 5.0rpm and kept at this temperature for 2.0h. Then, the introduction of silane was stopped, and the temperature was lowered to 25℃ to obtain 74.2g of a first composite material with silicon coated on the surface of the expanded graphite. The silicon content of the first composite material was calculated to be 32.61% according to the formula in Example 1.

[0156] (III) Preparation of the second composite material

[0157] In an argon atmosphere, 50.0 g of the first composite material obtained in step (2) was placed in another chemical vapor deposition furnace, evacuated to 0.01 MPa, heated to 800 °C at a rate of 10 °C / min, and then charged with ethylene at a rate of 25 L / h. The chamber of the chemical vapor deposition furnace was rotated at a speed of 5.0 rpm, and the furnace was kept at this temperature for 1.0 h. Then, the ethylene charging was stopped, and the temperature was lowered to 25 °C to obtain 52.0 g of a second composite material further coated with carbon on the surface of the first composite material. The carbon coating percentage of the second composite material was calculated to be 3.84% according to the formula in Example 1.

[0158] (iv) Preparation of silicon-carbon materials

[0159] Using an isostatic press, the second composite material obtained in step (3) was pressed at 150 MPa for 10.0 min, and then crushed for 2.0 h using a pulverizer at a speed of 450 rpm, a ball-to-material ratio of 5:1, and a ball diameter of 5.0 mm. After crushing, it was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 15.2 μm using a laser particle size analyzer.

[0160] Example 5

[0161] In Example 1, after step (ii) and before step (iii), the following step (iia) is performed, and then the first composite material with deposited lithium is subjected to carbon plating step (iii). Otherwise, the operation steps and condition parameters are basically the same as in Example 1.

[0162] (ii) Preparation of the first composite material for lithium deposition

[0163] In an argon atmosphere, 50.0g of the first composite material was placed in a vacuum evaporation furnace. Argon was introduced to replace the material, creating an inert protective atmosphere. The furnace was then evacuated to 0.01MPa, and the temperature was increased to 400℃ at a rate of 15℃ / min. At this temperature, 1.0g of lithium vapor at 1350℃ was slowly introduced into the vacuum evaporation furnace over 0.5 hours, while simultaneously rotating the furnace chamber at 5.0rpm to ensure thorough mixing and reaction between the lithium vapor and the material. After the lithium vapor introduction was complete, argon gas was slowly introduced to restore atmospheric pressure, and the material was allowed to cool naturally to room temperature (25℃). Under an inert atmosphere, 51g of the first composite material with deposited lithium was obtained. The lithium deposition rate of the first composite material was calculated to be 1.96% according to the following formula.

[0164] The percentage of lithium plating on the first composite material for lithium deposition = (mass of the first composite material for lithium deposition - mass of the first composite material) / mass of the first composite material for lithium deposition * 100%.

[0165] Regarding the source of lithium vapor, it is prepared by heating and melting a specific amount of metallic lithium in a crucible under an argon atmosphere in a distillation tank, and then evaporating the vapor, which is then fed into a vacuum evaporation furnace.

[0166] Example 6

[0167] In Example 2, after step (ii) and before step (iii), the following step (iia) is performed, and then the first composite material with deposited lithium is subjected to carbon plating step (iii). Otherwise, the operation steps and condition parameters are basically the same as in Example 2.

[0168] (ii) Preparation of the first composite material for lithium deposition

[0169] In an argon atmosphere, 50.0g of the first composite material was placed in a vacuum evaporation furnace. Argon gas was introduced to replace the material, creating an inert protective atmosphere. The furnace was then evacuated to 0.09MPa, and heated to 80°C at a rate of 5°C / min. At this temperature, 5.0g of lithium vapor at 1450°C was slowly introduced into the vacuum evaporation furnace over 5.0h, while simultaneously rotating the furnace chamber at 20.0rpm to ensure thorough mixing and reaction between the lithium vapor and the material. After the lithium vapor introduction was complete, argon gas was slowly introduced to restore atmospheric pressure, and the material was allowed to cool naturally to room temperature (25°C). Under an inert atmosphere, 55g of the first composite material with deposited lithium was obtained. The lithium plating percentage of the first composite material with deposited lithium was calculated to be 9.1% according to the formula in Example 5.

[0170] Regarding the source of lithium vapor, it is prepared by heating and melting a specific amount of metallic lithium in a crucible under an argon atmosphere in a distillation tank, and then evaporating the vapor, which is then fed into a vacuum evaporation furnace.

[0171] Comparative Example 1

[0172] In Example 3, step (1) was not used, that is, the natural graphite of Example 3 was not subjected to oxidation intercalation modification and high temperature treatment, and the natural graphite of Example 3 was directly subjected to silicon plating in step (2); otherwise, the operation steps and condition parameters of steps (2), (3) and (4) were the same as those of Example 3.

[0173] Comparative Example 2

[0174] In Example 3, step (3) was not used, that is, the first composite material with silicon coated on the surface of expanded graphite obtained by step (2) was not carbon coated, and step (4) was directly applied to the first composite material. Otherwise, the operation steps and condition parameters of steps (1), (2) and (4) were the same as those in Example 3.

[0175] Comparative Example 3

[0176] The difference from Example 3 is that the particle size Dn50 of the natural graphite used to prepare the expanded graphite is 1.0 μm. Otherwise, the other operating steps and parameter conditions are the same as in Example 3.

[0177] Comparative Example 4

[0178] The difference from Example 3 is that the particle size Dn50 of the natural graphite used to prepare the expanded graphite is 150.0 μm. Otherwise, the other operating steps and parameter conditions are the same as in Example 3.

[0179] Comparative Example 5

[0180] The difference from Example 3 is that the pressing and crushing step (4) is not performed. Instead, the second composite material is directly screened and demagnetized to obtain silicon-carbon material. Apart from this, the other operation steps and parameter conditions are the same as in Example 3.

[0181] The following section introduces the battery manufacturing and testing process.

[0182] 1. Preparation of liquid lithium-ion batteries

[0183] (1) Preparation of positive electrode

[0184] A positive electrode slurry (70% solid content) was prepared by mixing lithium nickel cobalt manganese oxide (NCM811), conductive agent SuperP, carbon nanotubes, and binder polyvinylidene fluoride (PVDF) in a mass ratio of 97:1:0.5:1.5 with N-methylpyrrolidone (NMP). The slurry was coated onto aluminum foil as a current collector, dried at 70°C, and then cold-pressed at room temperature at 4 MPa. After trimming, cutting, and slitting, tabs were welded to form the positive electrode sheet.

[0185] (2) Preparation of negative electrode

[0186] Under an inert protective atmosphere, the silicon-carbon material of the embodiments of the present invention or the comparative material of the comparative example is thoroughly mixed with natural graphite (particle size D50 = 15 μm, purchased from BTR Corporation) at a ratio of 1:9 to obtain a negative electrode active material. The negative electrode active material, conductive agent SuperP, binder PVDF and NMP are mixed at a mass ratio of 97.5:1.0:1.5 to prepare a negative electrode slurry (solid content of 50%), which is coated on the current collector copper foil, dried at 100°C, cold pressed at 4MPa at room temperature, and then trimmed, cut, and slit before welding tabs to form a negative electrode sheet.

[0187] (3) Assembly of lithium-ion batteries

[0188] Using a porous PE polymer film as a separator, the prepared positive electrode, separator, and negative electrode are stacked sequentially, with the separator positioned between the positive and negative electrodes, and then wound to obtain a bare battery cell. The bare battery cell is placed in an aluminum-plastic shell package and subjected to a relative vacuum pressure of -0.95 × 10⁻⁶. 5 At Pa, the cells are dried at 100°C until the moisture content is below 100 ppm. The electrolyte, composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1) and LiPF6 (concentration 1.0M), is injected into the dried bare cells. The cells are then encapsulated, allowed to stand, formed (0.02C constant current charging for 2 hours, 0.1C constant current charging for 2 hours), shaped, and capacity tested (capacity grading) to produce a soft-pack lithium-ion battery.

[0189] 2. Testing of lithium-ion batteries

[0190] 2.1 First Coulomb efficiency test:

[0191] The batteries prepared above were formed and capacity tested using a battery testing cabinet. The formation step consisted of charging at a constant current of 0.05C for 2.0 hours, followed by charging at a constant current of 0.15C for 2.5 hours. The capacity testing step consisted of charging at a constant current of 0.33C to 4.2V, then charging at a constant voltage of 4.2V to the cutoff current of 0.02C, and discharging at 0.33C to 2.5V. The sum of the above charging capacities and the discharge capacities were recorded as the first charging capacity and the first discharging capacity, and the first charging specific capacity, the first discharging specific capacity, and the first coulombic efficiency were calculated.

[0192] 2.2-rate discharge performance test:

[0193] At 25°C, the battery, after being formed and tested, was charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 0.33C at 25°C, and the 0.33C discharge capacity was recorded. The battery was then charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 3C, and the 3C discharge capacity was recorded.

[0194] 3C discharge capacity retention rate (%) = 3C discharge capacity / 0.33C discharge capacity × 100%

[0195] 2.3 Room temperature cycling performance test:

[0196] At 25°C, the formed and capacity-graded battery was charged to 4.2V at a constant current and constant voltage of 0.5C, with a cutoff current of 0.02C, and allowed to rest for 5 minutes. Then, it was discharged to 2.5V at a constant current of 1C and allowed to rest for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was calculated using the following formula:

[0197] Capacity retention rate (%) after 500 cycles at room temperature = (Discharge capacity after 500 cycles / Discharge capacity after 1 cycle) × 100%.

[0198] 2.4 High-Temperature Cycling Performance Test:

[0199] First, at 25℃, the formed and capacity-securing batteries were charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, the batteries were discharged to 2.5V at 0.33C, and the initial discharge capacity was recorded. The batteries were then placed in a 45℃ high-temperature chamber and charged to 4.2V at a constant current and constant voltage of 0.33C, rested for 5 minutes, discharged to 2.5V at 0.33C, and rested for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was then calculated. The calculation formula is as follows:

[0200] High-temperature capacity retention rate after 500 cycles (%) = (500th cycle discharge capacity / 1st cycle discharge capacity) × 100%.

[0201] The specific results of various tests on liquid lithium-ion batteries are shown in Table 1.

[0202] Table 1 Test Results of Liquid Lithium-ion Batteries

[0203]

[0204] As shown in Table 1, the silicon-carbon materials in Examples 1 to 4 have an initial coulombic efficiency of over 91.7%, a 3C discharge capacity retention rate of over 90.1%, a capacity retention rate of over 81.4% after 500 cycles at room temperature, and a capacity retention rate of over 74.5% after 500 cycles at high temperature, demonstrating excellent application performance.

[0205] As shown in Table 1, the silicon-carbon materials in Examples 5 and 6 have an initial coulombic efficiency of over 94.6%, a 3C discharge capacity retention rate of over 91.7%, a capacity retention rate of over 84.2% after 500 cycles at room temperature, and a capacity retention rate of over 76.6% after 500 cycles at high temperature, demonstrating superior application performance.

[0206] As shown in Table 1, the analysis of the test results of Examples 1-6 and Comparative Example 1 shows that the first-effect and cycle performance of Comparative Example 1 are significantly worse. The possible reason is that in Comparative Example 1, the graphite was not subjected to oxidation intercalation and calcination expansion treatment. The space between layers and pores was not opened, and a large amount of silicon source gas and / or silicon nanoparticles and carbon source gas and / or carbon nanoparticles could not fully enter the interior of the graphite. Most of them may have been deposited on the outer surface of the graphite. The thickness of the silicon-containing layer on the outer surface is too high, which makes it easy for silicon material to expand. Furthermore, it is not possible to fully utilize the significant effects of the carbon-silicon-carbon "sandwich" type coating structure and the three-dimensional carbon skeleton conductive hollow structure. In addition, the binding of silicon and carbon is weak, and the coating of silicon is poor, making it difficult to suppress the expansion of silicon particles. Silicon is prone to contact with the electrolyte and side reactions occur, resulting in poor cycle performance.

[0207] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 2 shows that the first efficiency and cycle performance of Comparative Example 2 are significantly worse. The possible reason is that the gas phase carbon coating in step (3) was not carried out in Comparative Example 2, making it difficult to achieve complete coating of silicon material by carbon material. As a result, the silicon nanoparticles deposited in the pores, interlayers and outer surface of the first composite material are easily exposed to the electrolyte. During charge and discharge cycles, silicon expansion is likely to occur, leading to repeated damage and formation of the SEI film. Side reactions between silicon and electrolyte are likely to occur, resulting in excessive consumption of lithium ions and electrolyte, which leads to a decrease in first efficiency, a significant deterioration in cycle performance and a decrease in conductivity.

[0208] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 3 shows that the cycle performance of Comparative Example 3 is significantly worse. The possible reason is that the particle size of natural graphite is too small, and the particle size of the final product is even smaller, resulting in poor vapor deposition effect and various spatial effects. The specific surface area is too large, which leads to an excessive contact area with the electrolyte, consuming reversible lithium ions and hindering the utilization of battery capacity.

[0209] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 4 shows that the cycle performance of Comparative Example 4 is significantly worse. The possible reason is that the particle size of natural graphite is relatively large, which makes it easy to cause structural damage, which is not conducive to the uniformity of slurry preparation and coating consistency. In the coating process, it is easy to have uneven particle distribution, which in turn affects the cycle performance of the battery.

[0210] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 5 shows that the first-efficiency and cycle performance of Comparative Example 5 deteriorated. The possible reason is that no pressing step was performed, the bonding between silicon nanoparticles and carbon nanoparticles was relatively poor, the pores or interlayer openings of the expanded graphite were not closed, the compaction density was low, the specific surface area was large, the contact area with the electrolyte was too large, the side reactions and lithium consumption increased, resulting in poor cycle performance.

[0211] In this invention, graphite materials with a specific particle size range are selected and expanded to increase the interlayer space within ordinary carbon materials, thereby improving their porosity. This is followed by high-temperature pyrolysis and vapor deposition of silicon source gas, and then another high-temperature vapor deposition coating of carbon source gas. The reaction parameters and process conditions of each step are strictly controlled to precisely control the amount and effect of silicon and carbon vapor deposition. This successfully deposits silicon nanoparticles and carbon nanoparticles within the pores, interlayers, and defects of the expanded carbon material, achieving silicon deposition on carbon materials. Complete coating of nanoparticles reduces internal resistance. Furthermore, after the vapor deposition carbon coating step, pressing and pulverizing steps seal or reduce the pores or interlayer spaces inside the expanded graphite, reduce the specific surface area of ​​the material, increase the compaction density of the material, promote the bonding between silicon nanoparticles and carbon nanoparticles, and promote complete coating of silicon. This effectively leverages the close synergistic effect of each step, successfully suppressing the expansion of silicon and improving its conductivity, reducing the contact between silicon and electrolyte, avoiding or reducing the generation of side reactions, and thus improving battery capacity and cycle performance.

[0212] Furthermore, by pre-replenishing lithium in silicon-carbon materials, the active lithium consumed or lost due to side reactions during the formation of the SEI film in the first charge-discharge cycle and during long-term charge-discharge cycles can be replenished, which can further improve the first coulombic efficiency of lithium-ion batteries, improve battery cycle performance, and alleviate capacity reduction.

[0213] By leveraging the synergistic effect of each step and strictly controlling the process conditions of each step, this invention can fully utilize the carbon-silicon-carbon "sandwich" coating structure of the silicon-carbon material of this invention, and take advantage of the significant spatial effect of the three-dimensional carbon skeleton conductive hollow structure. This significantly suppresses the expansion of silicon-containing silicon-carbon anode materials, improves conductivity and specific capacity, avoids direct contact between silicon and electrolyte to prevent side reactions, avoids the dissolution and loss of silicon and lithium, and improves the initial coulombic efficiency and high and low temperature cycling performance of silicon-containing anode lithium batteries.

[0214] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. The specific examples used above to illustrate the present invention are only for the purpose of helping to understand the present invention and are not intended to limit the present invention. Those skilled in the art to which this invention pertains can make several simple deductions, modifications, substitutions, or combinations based on the concept of the present invention. These deductions, modifications, substitutions, or combinations also fall within the scope of the claims of the present invention.

Claims

1. A method for preparing a silicon-carbon material, characterized in that, Includes the following steps: (1) Intercalated expanded graphite is obtained by mixing graphite, oxidant and intercalating agent, and expanded graphite is obtained by calcining the intercalated expanded graphite; wherein the particle size Dn50 of the graphite is 5.0~100.0μm, the mass ratio of graphite, oxidant and intercalating agent is 1:(0.1~3.0):(1.0~10.0); the holding temperature of calcination is 500~850℃; (2) In an inert atmosphere, silicon is deposited on the pores, interlayers, defects and outer surface of the expanded graphite prepared in step (1) by chemical vapor deposition to obtain the first composite material; the silicon content of the first composite material is 10~40wt%; (3) In an inert atmosphere, carbon is deposited on the pores, interlayers, defects and outer surface of the first composite material prepared in step (2) using chemical vapor deposition to obtain the second composite material; the carbon content of the second composite material is 0.5~10wt%; (4) The second composite material obtained in step (3) is pressed and crushed to obtain silicon-carbon material.

2. The method for preparing silicon-carbon material according to claim 1, characterized in that, The pressing pressure in step (4) is 150~450MPa.

3. The method for preparing silicon-carbon material according to claim 2, characterized in that, The pressing time mentioned in step (4) is 1.0~10.0 min.

4. The method for preparing silicon-carbon material according to claim 1, characterized in that, After step (2) and before step (3), the following lithium plating step (2a) is included: lithium vapor is deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain the first composite material with lithium deposition, which serves as the raw material for carbon deposition in step (3).

5. The method for preparing silicon-carbon material according to claim 2, characterized in that, After step (2) and before step (3), the following lithium plating step (2a) is included: lithium vapor is deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain the first composite material with lithium deposition, which serves as the raw material for carbon deposition in step (3).

6. The method for preparing silicon-carbon material according to claim 4, characterized in that, In step (2a), lithium vapor is introduced into a vacuum evaporation furnace containing the first composite material, and the vacuum evaporation furnace is rotated to ensure that the lithium vapor comes into full and uniform contact with the first composite material, thereby depositing the lithium vapor into the pores, interlayers, defects and outer surface of the first composite material.

7. The method for preparing silicon-carbon material according to claim 6, characterized in that, In step (2a), the temperature of the lithium vapor is 1350~1800℃; or, The rotation speed of the vacuum evaporation furnace is 5.0~20.0 rpm; or, The vacuum degree of the vacuum evaporation is 0.01~0.09 MPa; or, The lithium plating content of the first composite material for lithium deposition in step (2a) is 1 to 30 wt%.

8. The method for preparing silicon-carbon material according to claim 7, characterized in that, In step (2a), the vacuum degree of the vacuum evaporation is 0.01~0.05 MPa; or, The lithium plating content of the first composite material for lithium deposition in step (2a) is 1~10wt%.

9. The preparation method according to claim 1, characterized in that, The temperature for the chemical vapor deposition method described in step (2) is 400~1400℃; or, In step (2), the silicon source gas is silane or ethylsilane; or, In step (2), the silicon content of the first composite material is 20-35 wt%.

10. The preparation method according to claim 2, characterized in that, The temperature for the chemical vapor deposition method described in step (2) is 400~1400℃; or, In step (2), the silicon source gas is silane or ethylsilane; or, In step (2), the silicon content of the first composite material is 20-35 wt%.

11. The preparation method according to claim 4, characterized in that, The temperature for the chemical vapor deposition method described in step (2) is 400~1400℃; or, In step (2), the silicon source gas is silane or ethylsilane; or, In step (2), the silicon content of the first composite material is 20-35 wt%.

12. The preparation method according to claim 9, characterized in that, The temperature for chemical vapor deposition in step (2) is 400~1000℃; or, In step (2), the rate of silicon source gas filling is 10~100L / h.

13. The preparation method according to claim 9, characterized in that, The heating rate of the chemical vapor deposition method is 1~15℃ / min; Alternatively, the silicon source gas can be introduced over a period of 0.5 to 20.0 hours.

14. The preparation method according to claim 9, characterized in that, The chemical vapor deposition method is carried out in a chemical vapor deposition furnace, and the rotational speed of the furnace chamber is 0.5~10.0 rpm; Alternatively, the silicon source gas can be introduced over a period of 1 to 10 hours.

15. The preparation method according to claim 14, characterized in that, The rotation time is 0.5~20.0h.

16. The preparation method according to claim 14, characterized in that, The rotation time is 1.0~10.0h.

17. The method for preparing silicon-carbon material according to any one of claims 1-16, characterized in that, The temperature for chemical vapor deposition in step (3) is 400~1000℃; or, In step (3), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, or propane; or, In step (3), the carbon content of the second composite material is 0.5~8wt%.

18. The method for preparing silicon-carbon material according to claim 17, characterized in that, The heating rate of the chemical vapor deposition method described in step (3) is 1~15℃ / min; or, In step (3), the carbon source gas is introduced at a rate of 5~50 L / h.

19. The method for preparing silicon-carbon material according to claim 18, characterized in that, The chemical vapor deposition method described in step (3) is carried out in a chemical vapor deposition furnace, wherein the rotational speed of the furnace chamber is 0.5~10.0 rpm; or, The carbon source gas is introduced in step (3) for 0.5 to 2.0 hours.

20. The method for preparing silicon-carbon material according to claim 19, characterized in that, The chemical vapor deposition method described in step (3) is carried out in a chemical vapor deposition furnace, and the rotation time of the chemical vapor deposition furnace cavity is 0.5~2.0h.

21. The preparation method according to any one of claims 1-16, characterized in that, The graphite is one or more of the following: natural graphite, artificial graphite, spherical graphite, and graphitic intermediate phase; or... The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid; or, The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and glacial acetic acid; or, The mass ratio of graphite, oxidant and intercalating agent is 1:(0.1~3.0):(2.0~10.0).

22. The preparation method according to claim 17, characterized in that, The graphite is one or more of the following: natural graphite, artificial graphite, spherical graphite, and graphitic intermediate phase; or... The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid; or, The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and glacial acetic acid; or, The mass ratio of graphite, oxidant and intercalating agent is 1:(0.1~3.0):(2.0~10.0).

23. The preparation method according to claim 21, characterized in that, The graphite has a particle size Dn50 of 20.0~90.0 μm.

24. The preparation method according to any one of claims 1-16, characterized in that, In step (1), the mixing is a stirring mixture, and the stirring temperature is 10~60℃; or, The heating rate of the calcination is 1~20℃ / min.

25. The preparation method according to claim 17, characterized in that, In step (1), the mixing is a stirring mixture, and the stirring temperature is 10~60℃; or, The heating rate of the calcination is 1~20℃ / min.

26. The preparation method according to claim 21, characterized in that, In step (1), the mixing is a stirring mixture, and the stirring temperature is 10~60℃; or, The heating rate of the calcination is 1~20℃ / min.

27. The preparation method according to claim 24, characterized in that, In step (1), the mixing is a stirring mixture, and the stirring time is 0.5~24.0 h; or, The heating rate of the calcination is 5~10℃ / min.

28. The preparation method according to claim 27, characterized in that, In step (1), the mixing is a stirring mixture at a speed of 100-3000 rpm; or, The calcination holding time is 0.3~6.0h.

29. The preparation method according to claim 28, characterized in that, The calcination holding time is 0.5~2h.

30. The preparation method according to any one of claims 1-16, characterized in that, Step (1) before calcination also includes a step of washing the intercalated expanded graphite, wherein the washing includes washing the intercalated expanded graphite with deionized water until the pH of the filtrate is 5-7.

31. The preparation method according to claim 30, characterized in that, The washing process also includes a drying step.

32. The preparation method according to claim 31, characterized in that, The drying temperature is 30~80℃.

33. The preparation method according to claim 32, characterized in that, The drying time is 6.0~24.0h.

34. A silicon-carbon material, characterized in that, It is prepared by any one of claims 1-33.

35. The silicon-carbon material according to claim 34, characterized in that, The silicon content in the silicon-carbon material is 10~40wt%.

36. The silicon-carbon material according to claim 34, characterized in that, The silicon content in the silicon-carbon material is 20-35 wt%.

37. The silicon-carbon material according to any one of claims 34-36, characterized in that, The particle size Dn50 of the silicon-carbon material is 1~60μm.

38. The silicon-carbon material according to claim 37, characterized in that, The particle size Dn50 of the silicon-carbon material is 5~30μm.

39. A negative electrode active material, characterized in that, It contains the silicon-carbon material as described in any one of claims 34-38.

40. A lithium-ion battery negative electrode, characterized in that, It comprises the negative electrode active material, conductive agent, and binder as described in claim 39.

41. A lithium-ion battery, characterized in that, It comprises the lithium-ion battery negative electrode as described in claim 40.

Citation Information

Patent Citations

  • Anode plate and manufacturing method therefor, battery using anode plate, and electronic apparatus

    WO2021179219A1

  • Lithium ion battery silicon-carbon negative electrode material and preparation method thereof

    CN113964307A

  • Expanded graphite nano-silicon composite negative electrode material for lithium ion battery and preparation method of expanded graphite nano-silicon composite negative electrode material

    CN114497476A

  • Lithium metal composite material, modified material thereof, preparation methods of lithium metal composite material and modified material, and battery

    CN114824218A