Silicon-carbon material, preparation method thereof and lithium ion battery

By depositing silicon and carbon in expanded graphite to form a three-dimensional carbon framework structure, combined with high-temperature pressing and pulverization processes, the problems of volume expansion and poor cycle performance of silicon-carbon materials in lithium-ion batteries were solved, thereby improving the battery's capacity and conductivity.

CN116995197BActive Publication Date: 2026-11-20CARBON ONE NEW ENERGY GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211033374.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2026-11-20
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

Existing silicon-carbon materials in lithium-ion batteries suffer from problems such as large volume expansion, easy capacity reduction, and poor cycle performance. In particular, silicon and carbon materials are prone to separation, leading to loss of conductivity and repeated damage to the SEI film.

Method used

Silicon and carbon are deposited in the pores, interlayers and outer surface of expanded graphite by chemical vapor deposition to form a three-dimensional carbon framework conductive hollow structure. High-temperature pressing and pulverization processes are used to achieve a tight bond between silicon nanoparticles and carbon nanoparticles, which inhibits the expansion of silicon and improves conductivity.

Benefits of technology

It effectively suppressed the volume expansion of silicon-carbon materials, improved the cycle performance and capacity of lithium-ion batteries, enhanced conductivity, and reduced silicon consumption and SEI film damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003817968170000181
    Figure BDA0003817968170000181
Patent Text Reader

Abstract

The application discloses a silicon-carbon material, a preparation method thereof and a lithium ion battery, wherein silicon and carbon are co-deposited on the surface of expanded graphite by using a chemical vapor deposition method to obtain a first composite material; carbon is deposited on the surface of the first composite material by using the chemical vapor deposition method in an inert atmosphere to obtain a second composite material; and then the silicon-carbon material is obtained by pressing and crushing. In the application, the gas phase cracking reaction of a small amount of carbon source gas and the co-deposition of carbon nanoparticles are simultaneously carried out in the process of the gas phase cracking of the silicon source gas and the deposition of silicon nanoparticles, which is beneficial to inhibiting the excessive growth of silicon nanocrystalline grains and reducing the particle size of the silicon nanocrystalline grains, thereby relieving or inhibiting the swelling of the silicon particles in the charge-discharge cycle. Then, the high-temperature gas phase cracking deposition coating of the carbon source gas is carried out again, the silicon nanoparticles are completely coated by the carbon material, the internal resistance is reduced, and the battery capacity and the cycle performance are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to materials for lithium-ion batteries, specifically to a silicon-carbon material, its preparation method, and a lithium-ion battery. Background Technology

[0002] Lithium-ion batteries are currently widely used in consumer electronics, electric vehicles, and large-scale energy storage, and their application markets are gradually expanding to areas such as medical electronics, power tools, drones, data centers, and national security. The rapid development of these different fields has played a significant role in promoting the development of high-energy-density batteries.

[0003] Since the beginning of the 21st century, the development of portable electronic information products has been rapid, placing increasingly stringent demands on the capacity of energy storage batteries. Traditional lithium-ion batteries are nearing their energy density limits, making it difficult to meet the needs of 3C products. Silicon, with a specific capacity of 4200 mAh / g, can significantly improve the energy density of lithium batteries when used as the negative electrode material.

[0004] However, silicon-containing silicon-carbon materials suffer from significant volume expansion, easily reduced capacity, and deteriorated cycle performance. When silicon expands, it can easily detach from the carbon material, forming "dead silicon," which loses its conductivity and leads to reduced capacity. When silicon comes into direct contact with the electrolyte, a solid electrolyte interface (SEI) film is formed. During expansion, the SEI film is easily and repeatedly damaged, leading to continuous consumption and dissolution of silicon, resulting in a decrease in the capacity of silicon-containing lithium-ion batteries.

[0005] WO2021179219A1 discloses an anode electrode and its preparation method, as well as a battery and electronic device using the electrode. The anode electrode includes a current collector and an active layer. The active layer includes a porous carbon framework and silicon nanoparticles and lithium metal located within the porous carbon framework. Regarding the preparation method of the anode electrode, a porous carbon framework sheet is placed in a CVD apparatus, and a silane-containing gas is introduced to deposit silicon nanoparticles, resulting in a deposited porous carbon framework sheet. Under a protective gas atmosphere, molten lithium metal is brought into contact with the deposited porous carbon framework sheet, causing the lithium metal to fill the pores of the deposited porous carbon framework sheet, thus obtaining the active layer. The active layer is placed on the current collector, and hot-pressed to bond the active layer and the current collector together, thus obtaining the anode electrode. However, in this method, the porosity and open porosity of the porous carbon may be insufficient, causing most of the nano-silicon particles to be deposited on the outer surface of the porous carbon material. That is, most of the nano-silicon particles may not exist in the pores or interlayers of the porous carbon material. This results in most of the lithium metal reacting with the nano-silicon particles on the outer surface of the porous carbon material and being deposited on the outer surface of the carbon material, rather than being completely covered by the carbon material. In addition, due to the viscosity and surface tension of molten lithium metal, it is difficult for lithium metal to enter the pores of the porous carbon material.

[0006] Chinese patent CN101339987 discloses a silicon-carbon composite anode material for lithium-ion batteries and its preparation method. This silicon-carbon composite anode material is a core-shell structure material, with elemental silicon accounting for 0.01-10% and carbon accounting for 90.99%. The silicon-carbon composite anode material is prepared by mixing silicon powder or polymer-coated material with graphite, followed by high-energy milling, then adding asphalt or polymer-coated material and ball milling, carbonization, and finally pulverization. However, because silicon mainly coats the outer surface of graphite, the bonding between silicon and carbon is weak. Furthermore, the silicon content is limited, which is detrimental to improving battery performance. Summary of the Invention

[0007] The technical problem to be solved by the present invention is: to provide a method for preparing silicon-carbon materials, thereby improving the cycle stability of silicon-carbon materials applied to lithium-ion batteries, reducing the volume expansion of lithium-ion batteries, and increasing the capacity of lithium-ion batteries.

[0008] The purpose of this invention is to provide a silicon-carbon material and its preparation method, wherein the silicon-carbon material has the properties of high initial efficiency, long cycle life, and low expansion.

[0009] The objective of this invention can be achieved using the following technical solutions:

[0010] This invention provides a method for preparing silicon-carbon materials, comprising the following steps:

[0011] (1) In an inert atmosphere, silicon and carbon are deposited in the pores, interlayers, defects and outer surface of expanded graphite by chemical vapor deposition to obtain a first composite material.

[0012] (2) In an inert atmosphere, carbon is deposited on the pores, interlayers, defects and outer surface of the first composite material prepared in step (1) by chemical vapor deposition to obtain the second composite material.

[0013] (3) The second composite material obtained in step (2) is pressed and crushed to obtain silicon-carbon material.

[0014] Preferably, the temperature of the chemical vapor deposition method in step (1) is 400-1000℃; preferably, the heating rate of the chemical vapor deposition method is 1-15℃ / min; more preferably, the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, the rotation speed of the furnace chamber is 0.5-10.0 rpm, preferably the rotation time is 0.5-20.0 h, more preferably 1.0-10.0 h; or,

[0015] In step (1), the silicon source gas is silane or silane; preferably, the silicon source gas charging rate is 10–100 L / h, and preferably, the silicon source gas charging time is 1.0–10.0 h; or,

[0016] In step (1), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; preferably, the carbon source gas charging rate is 1–10 L / h, and preferably, the carbon source gas charging time is 1.0–10.0 h; or,

[0017] The ratio of the silicon source gas charging rate to the carbon source gas charging rate is 1:0.01 to 0.4, preferably 1:0.05 to 0.2; or,

[0018] In step (1), the amount of silicon-coated carbon in the first composite material is 10-40 wt%, preferably 20-30 wt%, and more preferably 22.56-28.88 wt%.

[0019] Preferably, the temperature of the chemical vapor deposition method in step (2) is 400–1000°C; preferably, the heating rate of the chemical vapor deposition method is 1–15°C / min; more preferably, the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, the rotation speed of the furnace chamber is 0.5–10.0 rpm, and preferably the rotation time is 0.5–2.0 h; or,

[0020] In step (2), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; preferably, the carbon source gas charging rate is 5–50 L / h, and more preferably, the carbon source gas charging time is 0.5–2.0 h; or,

[0021] In step (2), the carbon coating content of the second composite material is 0.5-10 wt%, preferably 1-6 wt%.

[0022] Preferably, the pressing pressure in step (3) is 150-450 MPa, and the pressing time is preferably 1.0-10.0 min.

[0023] Preferably, the expanded graphite in step (1) is prepared by the following steps: mixing graphite, oxidant and intercalating agent to obtain intercalated expanded graphite, and calcining the intercalated expanded graphite to obtain expanded graphite.

[0024] Preferably, in the above-mentioned method for preparing expanded graphite, the step of washing the intercalated expanded graphite before calcination is further included, wherein the washing includes washing the intercalated expanded graphite with deionized water until the pH of the filtrate is 5-7; preferably, the step of drying is further included after washing.

[0025] Preferably, the graphite is one or more of the following: natural graphite, artificial graphite, spherical graphite, and graphite intermediate phase; or,

[0026] The graphite has a particle size Dn50 of 5.0–100.0 μm, preferably 20.0–90.0 μm; or,

[0027] The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid, preferably potassium permanganate or potassium perchlorate; or,

[0028] The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and glacial acetic acid, preferably sulfuric acid or perchloric acid; or,

[0029] The mass ratio of graphite to oxidant to intercalating agent is 1:(0.1-3.0):(1.0-10.0), preferably 1:(0.1-3.0):(2.0-10.0).

[0030] Preferably, in the above-described method for preparing expanded graphite, the mixing is a stirring mixture, the stirring temperature is 10-60℃, preferably, the stirring time is 0.5-24.0 h, and more preferably, the stirring speed is 100-3000 rpm; or,

[0031] The drying temperature is 30-80℃, and the drying time is 6.0-24.0h; or,

[0032] The heating rate of the calcination is 1-20℃ / min, preferably 5-10℃ / min, the holding temperature of the calcination is 500-850℃, and the holding time is 0.5-2.0h.

[0033] The present invention also provides a silicon-carbon material, which is prepared by the above preparation method; preferably, the silicon-carbon content in the silicon-carbon material is 10-40 wt%, more preferably 20-30 wt%; more preferably, the particle size Dn50 of the silicon-carbon material is 1-60 μm, more preferably 5-25 μm.

[0034] The present invention also provides a negative electrode active material comprising the aforementioned silicon-carbon material.

[0035] The present invention also provides a lithium-ion battery negative electrode, which comprises the above-mentioned negative electrode active material, conductive agent and binder.

[0036] The present invention also provides a lithium-ion battery comprising the above-described lithium-ion battery negative electrode.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) In this invention, ordinary carbon materials such as graphite are expanded by modification and high-temperature treatment, which can increase the interlayer space or pore size inside the carbon material and improve the porosity of the pores inside the carbon material, which is beneficial for subsequent vapor deposition steps; then, silicon source gas and carbon source gas are simultaneously introduced for high-temperature pyrolysis, and various process conditions are strictly controlled. Vapor deposition of nano-silicon particles is carried out, which can make a large amount of silicon source gas and / or nano-silicon particles and a relatively small amount of carbon source gas and / or nano-carbon particles. The particles penetrate into the pores, interlayers, and defects of expanded graphite and other carbon materials for dense and uniform deposition, rather than simply depositing on the outer surface of ordinary graphite and other carbon materials. This is beneficial for improving the binding effect of silicon and carbon in silicon-carbon materials, allowing silicon nanoparticles and carbon nanoparticles to be stored inside the pores or interlayers of the carbon material. By simultaneously carrying out a relatively small amount of carbon source gas vapor phase pyrolysis and co-deposition of carbon nanoparticles during the vapor phase pyrolysis of silicon source gas and the deposition of silicon nanoparticles, it is beneficial for suppressing the excessive growth of silicon nanocrystals and reducing the silicon nanocrystal density. The particle size is optimized to suppress silicon particle expansion during charge-discharge cycles. This three-dimensional carbon skeleton conductive hollow structure helps suppress the expansion of silicon-containing anode materials and improve conductivity, reducing internal resistance and improving battery capacity and cycle performance. Then, carbon source gas is introduced again for high-temperature pyrolysis to perform vapor-phase deposition of carbon nanoparticles on the expanded carbon material that has already deposited silicon and carbon nanoparticles. This allows a large amount of carbon source gas and / or carbon nanoparticles to enter the pores, interlayers, and defects of the expanded carbon material for deposition, completely coating the already deposited silicon nanoparticles. At the same time, carbon nanoparticles will also naturally deposit on the outer surface of the expanded carbon material, completely coating the silicon nanoparticles deposited on the outer surface of the expanded carbon material. Finally, a pressing step is used to press the material at high pressure, which helps to make the bonding between silicon and carbon nanoparticles tighter and close the pores or interlayer openings of the graphite material, thereby reducing the contact between silicon nanoparticles and electrolyte, reducing silicon consumption and repeated damage to the SEI film. By compressing and densifying the expanded voids and interlayer spaces of expanded graphite, the compaction density of silicon-carbon materials can be increased, achieving a comprehensive coating effect of carbon materials on silicon materials. This helps to suppress the expansion of silicon materials and reduce the internal resistance of the battery, thereby improving the cycle performance and capacity utilization of the battery. It also helps to avoid direct contact between silicon particles and electrolyte to prevent the formation of SEI film, thus avoiding or mitigating the dissolution and consumption of silicon, preventing excessive capacity reduction, and significantly improving the cycle performance of silicon-containing anode lithium batteries.

[0039] (2) Compared with existing silicon-carbon materials with carbon-coated silicon structures, the silicon-carbon material of the present invention has a "sandwich" type carbon-silicon-carbon structure and a three-dimensional carbon skeleton conductive hollow structure. The silicon-carbon material of the present invention utilizes graphite materials and carbon nanoparticles to achieve complete coating of silicon nanoparticles or silicon-carbon nanoparticles, leveraging the spatial effect of the three-dimensional carbon skeleton conductive hollow structure. This buffers or self-absorbs the volume expansion effect of silicon particles during charging and discharging, alleviates or suppresses the expansion of silicon-carbon materials, prevents silicon particles from pulverizing and falling off the surface of carbon materials to form "dead silicon," improves the charge-discharge cycle performance of lithium batteries containing the silicon-carbon material of the present invention, increases the capacity of lithium batteries, improves the conductivity of silicon-containing anode materials, and improves the capacity reduction of silicon-containing anode lithium batteries during cycling. Detailed Implementation

[0040] In this specification, unless otherwise specified, the symbols, units, abbreviations, and terms have the following meanings. For example, when using ~ or - to indicate a numerical range, they include both endpoints, and the units are common. For example, 5~25% means more than 5% and less than 25%.

[0041] In this invention, particle size Dn50 refers to the particle size corresponding to a cumulative particle size distribution percentage of 50% in a sample.

[0042] In this invention, the percentage of silicon-carbon plating in the first composite material refers to the percentage of the mass difference between the first composite material obtained by silicon-carbon plating of expanded graphite and the expanded graphite, relative to the mass of the first composite material.

[0043] In this invention, the carbon plating percentage of the second composite material refers to the percentage of the mass difference between the second composite material obtained by carbon plating the first composite material and the first composite material.

[0044] In one specific embodiment of the present invention, a method for preparing silicon-carbon material is provided, comprising the following steps:

[0045] (1) In an inert atmosphere, silicon and carbon are deposited on the surface of expanded graphite by chemical vapor deposition. Preferably, silicon nanoparticles are deposited in the pores, interlayers, defects and outer surface of expanded graphite to obtain a first composite material.

[0046] (2) In an inert atmosphere, carbon is deposited on the surface of the first composite material obtained in step (1) by chemical vapor deposition. Preferably, carbon nanoparticles are deposited in the pores, interlayers, defects and outer surface of the first composite material to obtain the second composite material.

[0047] (3) The second composite material obtained in step (2) is pressed and crushed to obtain silicon-carbon material.

[0048] In a preferred embodiment of the present invention, in step (1), the expanded graphite material is placed in a chemical vapor deposition furnace, a vacuum is drawn, an inert protective gas is introduced at a rate of 10-100 L / h, and the temperature is raised to 400-1000°C, preferably 500-900°C, at a rate of 1-15°C / min; then a silicon source gas is introduced at a rate of 10-100 L / h, the cavity of the chemical vapor deposition furnace is rotated at a speed of 0.5-10.0 rpm, and the temperature is maintained and rotated for 0.5-20.0 h, preferably 1.0-10.0 h, and then the introduction of silicon source gas is stopped and the temperature is lowered to room temperature to obtain a first composite material in which silicon nanoparticles are deposited in the pores, interlayers, defects and outer surface of the expanded graphite.

[0049] The chemical vapor deposition method is carried out in a chemical vapor deposition furnace, wherein the rotation speed of the furnace chamber is 0.5 to 10.0 rpm, preferably 0.5 to 20.0 h, and more preferably 1.0 to 10.0 h;

[0050] In step (1), the silicon source gas is silane or silane; preferably, the silicon source gas charging rate is 10 to 100 L / h, and preferably, the silicon source gas charging time is 1.0 to 10.0 h.

[0051] In step (1), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; preferably, the carbon source gas charging rate is 1 to 10 L / h, more preferably 2 to 5 L / h, and preferably, the carbon source gas charging time is 1.0 to 10.0 h.

[0052] By simultaneously performing chemical vapor deposition of silicon source gas and carbon source gas in step (1), it is beneficial to suppress the excessive growth of silicon nanocrystals. By generating silicon-carbon bonds to suppress or interfere with the growth of silicon nanocrystals, the particle size of the deposited silicon grains can be effectively reduced. By generating amorphous carbon around the silicon nanocrystals, the volume expansion of silicon nanoparticles can be further buffered or suppressed, thereby improving the cycle characteristics of the anode material.

[0053] The ratio of the silicon source gas charging rate to the carbon source gas charging rate can be, for example, 1:0.01 to 0.4, preferably 1:0.05 to 0.2. If the proportion of carbon source gas charging to silicon source gas charging is too low, it may be difficult to suppress the growth of silicon nanocrystals, improve the expansion of silicon particles, and consequently, improve the cycle performance of silicon-carbon materials. If the proportion of carbon source gas charging to silicon source gas charging is too high, it will lead to a decrease in the overall capacity of the silicon-carbon material, failing to achieve the intended effect of increasing battery capacity. Furthermore, it may generate carbon microspheres, resulting in a reduction in initial efficiency.

[0054] The inert protective gas is one or more of argon, helium, xenon, radon, and neon.

[0055] By depositing silicon nanoparticles and carbon nanoparticles (hereinafter also referred to as silicon-carbon plating) on ​​the inner and outer surfaces of graphite, the battery capacity of the final product can be increased. Regarding the proportion of silicon-carbon plating in the first composite material in step (1), from the viewpoint of suppressing silicon expansion and improving battery performance, the proportion of silicon-carbon plating in the first composite material is, for example, 10-40%, preferably 20-30%, and more preferably 22.56-28.88 wt%. If the amount of silicon-carbon plating is too large, it may be difficult to achieve complete coating of silicon-carbon particles by carbon materials or carbon nanoparticles, and the spatial effect of the carbon-silicon-carbon "sandwich" type coating structure cannot be fully utilized. This can easily lead to an excessively thick silicon-carbon layer on the surface, making it difficult to suppress the expansion of silicon, causing repeated damage to the SEI film and excessive consumption of lithium ions, thereby affecting the cycle performance of the battery. If the amount of silicon-carbon plating is too small, it may result in insufficient capacity and fail to take advantage of the capacity of silicon-carbon materials.

[0056] Regarding the temperature of the chemical vapor deposition furnace in the silicon-carbon chemical vapor deposition step, for example, it can be 400-1000℃, preferably 500-900℃. If the temperature is too low, the decomposition of silicon source gas and carbon source gas will be insufficient, which may lead to poor vapor deposition effect of silicon and carbon, especially the inability to fully deposit in the internal pores or interlayer of the expanded graphite. If the temperature is too high, it will increase the difficulty of process control and the energy consumption cost will be higher. When the temperature is close to or exceeds the melting point of silicon, 1410℃, the silicon nanoparticles deposited on the surface of the carbon material will melt and stick together, which may form a block, which is not conducive to the formation of good bonding between carbon and silicon, resulting in poor expansion inhibition effect and cycle performance.

[0057] In another preferred embodiment of the present invention, in step (2), the first composite material is placed in a chemical vapor deposition furnace in an inert protective gas atmosphere, a vacuum is drawn, and the temperature is raised to 400-1000°C, preferably 500-900°C, at a rate of 1-15°C / min. Then, carbon source gas is introduced at a rate of 5-50L / h, and the cavity of the chemical vapor deposition furnace is rotated at a speed of 0.5-10.0rpm. The furnace is kept warm and rotated for 0.5-2.0h, and then the introduction of carbon source gas is stopped and the temperature is lowered to room temperature to obtain a second composite material with carbon further coated on the surface of silicon.

[0058] The carbon source gas includes one or more of methane, ethylene, acetylene, propylene, and propane;

[0059] The inert protective gas is one or more of argon, helium, xenon, radon, and neon.

[0060] Carbon plating on a first composite material containing deposited silicon nanoparticles and a small amount of carbon nanoparticles provides excellent protection for the deposited silicon nanoparticles. This is because direct contact between silicon and the electrolyte can lead to a reaction that causes silicon to dissolve and be lost, reducing battery capacity. Carbon plating also increases the conductivity of the final product, inhibits silicon expansion, and reduces unwanted side reactions.

[0061] Carbon deposition of the first composite material using a vapor-phase coating method is advantageous because the carbon source gas or carbon nanoparticles in the vapor phase have extremely small particle sizes and strong penetrating power, allowing them to easily enter the pores and interlayers of the carbon material for carbon deposition. This facilitates comprehensive and uniform coating of the first composite material and promotes the reaction or adsorption coating between silicon nanoparticles and carbon nanoparticles. In contrast, solid-phase or liquid-phase coating methods are less desirable than vapor-phase coating because commonly used coating agents such as asphalt, resin, or organic solutions have large particle sizes or high viscosity, making it difficult for them to penetrate the fine pores and interlayers of the carbon material, especially deep within the pores. Therefore, achieving comprehensive and uniform coating of the first composite material is challenging.

[0062] Regarding the temperature of the chemical vapor deposition furnace during carbon plating, for example, it can be 400-1000℃. If the temperature is too low, the carbon source gas will not be fully decomposed, which may lead to poor carbon vapor deposition effect, especially the inability to fully deposit carbon in the internal pores or interlayers of the first composite material. If the temperature is too high, it will increase the difficulty of process control and increase energy consumption costs.

[0063] Regarding the chemical vapor deposition furnace in step (2), the chemical vapor deposition furnace that has undergone silicon-carbon plating in step (1) can also be used without affecting the effect of the invention, so as to improve the continuity of production.

[0064] Regarding the carbon plating percentage of the second composite material in step (2), from the viewpoint of suppressing silicon expansion and improving battery performance, the carbon plating percentage of the second composite material is, for example, 0.5 to 10 wt%, preferably 1 to 6 wt%, and more preferably 1.19 to 5.3 wt%. If the carbon plating amount is too high, the carbon content in the silicon-carbon material will increase, the energy density will decrease, and the battery capacity will decrease. Furthermore, if the carbon layer coated on the silicon is too thick, it may hinder the passage of lithium ions. If the carbon plating amount is too low, the deposited silicon nanoparticles cannot be completely coated, which may lead to side reactions due to contact between the silicon particles and the electrolyte, resulting in silicon consumption and capacity reduction.

[0065] In another preferred embodiment of the present invention, in step (3), the second composite material obtained in step (2) is pressed and pulverized to obtain silicon-carbon material.

[0066] This invention employs an extruder or isostatic press for pressing. The pressing pressure can be, for example, 150–450 MPa, and the pressing time can be, for example, 1–10 minutes. Setting a higher pressure during pressing helps to achieve a tighter bond between silicon and carbon nanoparticles and closes the voids or interlayer openings in the graphite material. This reduces the contact between silicon nanoparticles and the electrolyte, decreasing silicon consumption and repeated damage to the SEI film. By compressing and densifying the expanded voids and interlayer spaces of the expanded graphite, the compaction density of the silicon-carbon material is increased.

[0067] This invention employs commonly used pulverizing machines such as mechanical pulverizers, air jet mills, ball mills, or grinding mills for uniform pulverization. The compressed, block-shaped material is thoroughly and uniformly pulverized, preferably to a particle size smaller than that of the raw graphite. Regarding pulverization time and conditions, there are no particular limitations as long as the particle size Dn50 after grinding is ensured to be 1–60 μm, preferably 5–25 μm, and more preferably 6.7–24.3 μm. The pulverization time can be, for example, 0.5–5.0 h, preferably 1.0–3.0 h. Various pulverizing machines or methods can be used, including, for example, jaw crushers, mechanical pulverizers, air jet mills, ball mills, or grinding mills.

[0068] After the pressing and crushing steps, further post-processing such as grading, sieving, and demagnetization can be carried out before packaging and discharge.

[0069] In another preferred embodiment of the present invention, the expanded graphite in step (1) can be commercially available expanded graphite, as long as it meets the requirements of vapor deposition, there is no particular limitation. The expanded graphite in step (1) is prepared by the following steps: mixing graphite, oxidant and intercalating agent to obtain intercalated expanded graphite, and calcining the intercalated expanded graphite to obtain expanded graphite.

[0070] In the above-mentioned method for preparing expanded graphite, graphite, oxidant, and intercalating agent are mixed to obtain a mixture, the mixture is stirred to obtain intercalated expanded graphite, the intercalated expanded graphite is repeatedly washed with deionized water until the pH of the filtrate is between 5 and 7, the washed intercalated expanded graphite is dried, and then calcined in an inert atmosphere to obtain expanded graphite.

[0071] In the above-described method for preparing expanded graphite, mixing and stirring are performed to ensure that the intercalating agent and oxidizing agent fully impregnate the pores and interlayers of the graphite carbon material. Excess oxidizing agent and intercalating agent are removed through repeated washing, for example, 2 to 10 times. The washing process continues until the pH of the filtrate is 5 to 7. If the pH is too low after washing, the expansion degree may be too large; if the pH is too high, the intercalating agent may excessively detach from the carbon material, resulting in insufficient subsequent expansion. The moisture in the intercalated expanded graphite is removed by drying, followed by calcination, which oxidizes the intercalating agent to generate gas, causing the graphite to expand and modify, thus obtaining expanded graphite.

[0072] In the above-mentioned method for preparing expanded graphite, the stirring temperature is 10-60℃, the stirring time is 0.5-24.0h, and the stirring speed is 100-3000rpm. As long as the desired stirring effect can be achieved, the stirring conditions are not particularly limited.

[0073] The drying temperature of the washed intercalated expanded graphite is 30-80℃, and the drying time is 6.0-24.0h. As long as the predetermined drying effect can be achieved, the drying conditions are not particularly limited.

[0074] The heating rate of the calcination is 1-20℃ / min, preferably 5-10℃ / min, the holding temperature of the calcination is 500-850℃, and the holding time is 0.3-6.0h, preferably 0.5-2.0h.

[0075] Regarding the calcination and holding temperature and time, there are no particular limitations as long as the graphite can expand sufficiently, resulting in a significant opening of the graphite pore space and a significant widening of the interlayer spacing. For example, the holding temperature can be 500–850℃. If the calcination and holding temperature is too low, the expansion may be insufficient, and the modification effect obtained by the oxide intercalation may be inadequate. If the temperature is too high, the expansion may be excessive, resulting in too many breakages and defects, making it difficult to control the process reaction, easily causing various side reactions, introducing too many impurity atoms, and hindering subsequent vapor-phase silicon deposition.

[0076] The graphite is one or more of natural graphite, artificial graphite, spherical graphite, and graphite mesophase. The particle size Dn50 of the graphite is 5.0-100.0 μm, preferably 20.0-90.0 μm, and more preferably 20.0-60.0 μm. When the particle size is too small, the particle size of the final product obtained after pressing and crushing is too small, and the specific surface area is too large, which is not conducive to the performance of battery capacity. When the particle size is too large, the slurry preparation process is difficult to control, and uneven particle distribution is likely to occur in the coating process.

[0077] The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid, preferably potassium permanganate and potassium perchlorate;

[0078] The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid and glacial acetic acid, preferably sulfuric acid or perchloric acid;

[0079] The mass ratio of graphite to oxidant to intercalating agent is 1:(0.1-3.0):(1.0-10.0), preferably 1:(0.1-3.0):(2.0-10.0), and more preferably 1:(0.1-2.0):(2.0-5.0). The amount of intercalating agent is, for example, 1-10 times the amount of graphite. If the amount of intercalating agent is too small, it is difficult to stir and mix evenly, making intercalation difficult and resulting in poor expansion and modification effects. If the amount of intercalating agent is too large, it increases process costs, prolongs drying time, and may cause excessive expansion. The amount of oxidant is, for example, 0.1-3.0 times the amount of graphite. If the amount of oxidant is too small, the expansion degree is too low, resulting in insufficient modification. If the amount of oxidant is too large, the expansion may become excessive, increasing preparation costs and impurities.

[0080] The strong acid treatment causes a certain degree of etching on the graphite surface, resulting in structural defects and uneven morphology, which is beneficial for the deposition of silicon in subsequent processes and enhances the strong adsorption between carbon and silicon.

[0081] By utilizing the aforementioned oxide intercalation modification and high-temperature calcination treatments, the oxygen-containing groups inserted or introduced between the graphite layers undergo pyrolysis, causing the graphite material to expand significantly. This expands the graphite sheets, facilitating subsequent vapor-phase deposition. The expansion rate of graphite can be several times or even more than ten times, resulting in significantly higher porosity and interlayer spacing compared to current porous carbon materials.

[0082] The present invention also provides a silicon-carbon material, which is prepared by the above-described method for preparing silicon-carbon materials.

[0083] In the aforementioned silicon-carbon material, the proportion of silicon-carbon plating is 10–40 wt%, preferably 20–30 wt%. Specifically, the proportion of silicon-carbon plating in the first composite material is 10–40 wt%, preferably 20–30 wt%. Since the mass difference between the second composite material and the first composite material is relatively small, the fluctuation of the mass percentage of each component after the carbon plating step can be basically ignored; that is, the proportion of silicon-carbon plating in the second composite material can be considered to be 10–40 wt%, preferably 20–30 wt%. Further, the proportion of silicon-carbon plating in the silicon-carbon material can be considered to be 10–40 wt%, preferably 20–30 wt%.

[0084] In the aforementioned silicon-carbon materials, the specific surface area, measured using a BET surface area analyzer, ranges from 0.5 to 5.0 m². 2 / g.

[0085] The particle size Dn50 of the silicon-carbon material is, for example, 1-60 μm, preferably 5-25 μm, and more preferably 6.7-24.3 μm. If the particle size is too small, the specific surface area will be too large, which may lead to an increase in side reactions in the electrolyte and a decrease in capacity. If the particle size is too large, the coating process will be difficult to control, resulting in poor ion conduction and hindering the performance of lithium battery cycle.

[0086] The present invention also provides a negative electrode active material comprising the above-mentioned silicon-carbon material.

[0087] The present invention also provides a lithium-ion battery negative electrode, which comprises the above-mentioned negative electrode active material, conductive agent and binder.

[0088] The present invention also provides a lithium-ion battery, wherein it comprises the above-described lithium-ion battery negative electrode.

[0089] To better understand the above technical solution, the present invention will be further described in detail below.

[0090] All raw materials and reagents used in this invention were purchased from mainstream manufacturers on the market. Those without a specified manufacturer or concentration are all analytical grade raw materials or reagents that are routinely available. There are no particular restrictions as long as they achieve the intended effect. For example, natural graphite was purchased from BTR Corporation; silane and other reagents were purchased from Guangzhou Spectrum Gas Co., Ltd.; acetylene and other reagents were purchased from Shenzhen Huataipeng Special Gas Co., Ltd.; potassium permanganate, concentrated sulfuric acid, and other reagents were purchased from Aladdin Reagent Network.

[0091] The mixer, drying equipment, chemical vapor deposition furnace, isostatic press, pulverizer, and other instruments and equipment used in this embodiment were all purchased from major manufacturers on the market. As long as they can achieve the expected results, there are no particular limitations. For example, the chemical vapor deposition (CVD) furnace was purchased from Shenzhen Kejing Zhida Technology Co., Ltd.

[0092] Unless otherwise specified in this embodiment, the techniques or conditions described in the literature in this field or in accordance with the product manual shall apply.

[0093] The present invention will now be described in more detail with reference to examples and comparative examples, but the scope of the present invention is not limited to these examples. It should be noted that, unless otherwise specified, all percentages, parts, and ratios used in the present invention are based on mass.

[0094] Example 1

[0095] (I) Preparation of Expanded Graphite

[0096] 100.0g of natural graphite (particle size Dn50 of 20.0μm), 10.0g of potassium permanganate, and 200.0g of sulfuric acid (98wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 10℃ for 24.0h at a stirring speed of 100rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 5.0. The washed intercalated expanded graphite was then dried at 30℃ for 24.0h, and then calcined at 500℃ for 2.0h in a nitrogen atmosphere at a heating rate of 5℃ / min to obtain 93.9g of expanded graphite.

[0097] (II) Preparation of the first composite material

[0098] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.01MPa, and argon was introduced at a rate of 10L / h. The temperature was increased to 500℃ at a rate of 1℃ / min, and then silane was introduced at a rate of 100L / h and acetylene at a rate of 5L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 0.5rpm and kept at the temperature for 1.0h. Then the introduction of silane and acetylene was stopped, and the temperature was lowered to 25℃ to obtain 64.57g of the first composite material with silicon coated on the surface of the expanded graphite.

[0099] The silicon-carbon content of the first composite material is calculated to be 22.56% according to the following formula.

[0100] Silicon carbon content ratio = (mass of first composite material - mass of expanded graphite) / mass of first composite material * 100%.

[0101] (III) Preparation of the second composite material

[0102] In an argon atmosphere, 50.0g of the first composite material was placed in another chemical vapor deposition furnace, evacuated to 0.01MPa, heated to 500℃ at a rate of 1℃ / min, and then acetylene was introduced at a rate of 5L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 0.5rpm and kept at the temperature for 2.0h. Then, the acetylene introduction was stopped and the temperature was lowered to 25℃ to obtain 50.6g of a second composite material with carbon further coated on the surface of the first composite material.

[0103] The carbon coating percentage is calculated to be 1.19% according to the following formula.

[0104] Carbon coating percentage = (Mass of second composite material - Mass of first composite material) / Mass of second composite material * 100%

[0105] (iv) Preparation of silicon-carbon materials

[0106] The second composite material was pressed at 150 MPa for 10.0 min using an isostatic press, and then pulverized for 3.0 h using a pulverizer at a speed of 300 rpm, a ball-to-material ratio of 5:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 6.7 μm using a laser particle size analyzer.

[0107] Example 2

[0108] (I) Preparation of Expanded Graphite

[0109] 100.0 g of natural graphite (particle size Dn50 of 90.0 μm), 300.0 g of potassium permanganate, and 1000.0 g of sulfuric acid (98 wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 60 °C for 0.5 h at a stirring speed of 3000 rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 7.0. The washed intercalated expanded graphite was then dried at 80 °C for 6.0 h, and then calcined at 850 °C for 0.5 h in a nitrogen atmosphere at a heating rate of 10 °C / min to obtain 92.4 g of expanded graphite.

[0110] (II) Preparation of the first composite material

[0111] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.05MPa, and argon was introduced at a rate of 100L / h. The temperature was increased to 900℃ at a rate of 15℃ / min, and then silane was introduced at a rate of 10L / h and acetylene at a rate of 2L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 5.0rpm and kept at the temperature for 10.0h. Then the introduction of silane and acetylene was stopped, and the temperature was lowered to 25℃ to obtain 70.3g of the first composite material with silicon coated on the surface of the expanded graphite.

[0112] The carbon content in the silicon plating is calculated to be 28.88% according to the following formula.

[0113] Silicon carbon content ratio = (mass of first composite material - mass of expanded graphite) / mass of first composite material * 100%.

[0114] (III) Preparation of the second composite material

[0115] In an argon atmosphere, 50.0g of the first composite material was placed in another chemical vapor deposition furnace, evacuated to 0.05MPa, heated to 900℃ at a rate of 15℃ / min, and then acetylene was introduced at a rate of 50L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 10.0rpm, and the furnace was kept at the temperature and rotated for 0.5h. Then, the acetylene introduction was stopped, and the temperature was lowered to 25℃ to obtain 52.8g of a second composite material with carbon further coated on the surface of the first composite material.

[0116] The carbon coating percentage is calculated to be 5.3% according to the following formula.

[0117] Carbon coating percentage = (Mass of second composite material - Mass of first composite material) / Mass of second composite material * 100%

[0118] (iv) Preparation of silicon-carbon materials

[0119] The second composite material was pressed at 450 MPa for 1.0 min using an isostatic press, and then pulverized for 1.0 h using a pulverizer at a speed of 500 rpm, a ball-to-material ratio of 10:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 24.3 μm using a laser particle size analyzer.

[0120] Example 3

[0121] (I) Preparation of Expanded Graphite

[0122] 100.0g of natural graphite (particle size Dn50 of 50.0μm), 100.0g of potassium permanganate, and 500.0g of sulfuric acid (98wt%) were thoroughly mixed to obtain a mixture. The mixture was stirred at 30℃ for 12.0h at a stirring speed of 1500rpm to obtain intercalated expanded graphite. The intercalated expanded graphite was repeatedly washed with deionized water until the pH of the filtrate was 6.0. The washed intercalated expanded graphite was then dried at 50℃ for 15.0h, and then calcined at 700℃ for 1.0h in a nitrogen atmosphere at a heating rate of 8℃ / min to obtain 93.2g of expanded graphite.

[0123] (II) Preparation of the first composite material

[0124] 50.0g of the expanded graphite obtained in step (1) was placed in a chemical vapor deposition furnace, evacuated to 0.02MPa, and argon was introduced at a rate of 50L / h. The temperature was increased to 700℃ at a rate of 10℃ / min, and then silane was introduced at a rate of 50L / h and acetylene at a rate of 5L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 5.0rpm and kept at the temperature for 2.0h. Then the introduction of silane and acetylene was stopped, and the temperature was lowered to 25℃ to obtain 67.1g of the first composite material with silicon coated on the surface of the expanded graphite.

[0125] The carbon content in the silicon plating is calculated to be 25.48% according to the following formula.

[0126] Silicon carbon content ratio = (mass of first composite material - mass of expanded graphite) / mass of first composite material * 100%.

[0127] (III) Preparation of the second composite material

[0128] In an argon atmosphere, 50.0g of the first composite material was placed in another chemical vapor deposition furnace, evacuated to 0.02MPa, heated to 700℃ at a rate of 5℃ / min, and then acetylene was introduced at a rate of 25L / h. The cavity of the chemical vapor deposition furnace was rotated at a speed of 0.5rpm, and the furnace was kept at the temperature and rotated for 1.0h. Then, the acetylene introduction was stopped, and the temperature was lowered to 25℃ to obtain 51.4g of a second composite material with carbon further coated on the surface of the first composite material.

[0129] The carbon coating percentage is calculated to be 2.72% according to the following formula.

[0130] Carbon coating percentage = (Mass of second composite material - Mass of first composite material) / Mass of second composite material * 100%

[0131] (iv) Preparation of silicon-carbon materials

[0132] The second composite material was pressed at 300 MPa for 5.0 min using an isostatic press, and then pulverized for 2.0 h using a pulverizer at a speed of 450 rpm, a ball-to-material ratio of 7:1, and a ball diameter of 5.0 mm. After pulverization, the material was graded, sieved, and demagnetized to obtain silicon-carbon material. The particle size Dn50 was measured to be 16.5 μm using a laser particle size analyzer.

[0133] Comparative Example 1

[0134] In Example 3, step (1) was not used, that is, the natural graphite of Example 3 was not subjected to oxidation intercalation modification and high temperature treatment, and the natural graphite of Example 3 was directly subjected to silicon carbide plating in step (2); otherwise, the operation steps and condition parameters of steps (2), (3) and (4) were the same as those of Example 3.

[0135] Comparative Example 2

[0136] In Example 3, step (3) was not used, that is, the first composite material obtained by step (2) with silicon and carbon coated on the surface of expanded graphite was not carbon coated, and step (4) was directly applied to the first composite material. Otherwise, the operation steps and condition parameters of steps (1), (2) and (4) were the same as those in Example 3.

[0137] Comparative Example 3

[0138] The difference from Example 3 is that the particle size Dn50 of the natural graphite used to prepare the expanded graphite is 1.0 μm. Otherwise, the other operating steps and parameter conditions are the same as in Example 3.

[0139] Comparative Example 4

[0140] The difference from Example 3 is that the particle size Dn50 of the natural graphite used to prepare the expanded graphite is 150.0 μm. Otherwise, the other operating steps and parameter conditions are the same as in Example 3.

[0141] Comparative Example 5

[0142] The difference from Example 3 is that the pressing and crushing step (4) is not performed. Instead, the second composite material is directly screened and demagnetized to obtain silicon-carbon material. Apart from this, the other operation steps and parameter conditions are the same as in Example 3.

[0143] The following section introduces the battery manufacturing and testing process.

[0144] 1. Preparation of liquid lithium-ion batteries

[0145] (1) Preparation of positive electrode

[0146] A positive electrode slurry (70% solid content) was prepared by mixing lithium nickel cobalt manganese oxide (NCM811), conductive agent SuperP, carbon nanotubes, and binder polyvinylidene fluoride (PVDF) in a mass ratio of 97:1:0.5:1.5 with N-methylpyrrolidone (NMP). The slurry was coated onto aluminum foil as a current collector, dried at 70°C, and then cold-pressed at room temperature at 4 MPa. After trimming, cutting, and slitting, tabs were welded to form the positive electrode sheet.

[0147] (2) Preparation of negative electrode

[0148] Under an inert protective atmosphere, the silicon-carbon material of the embodiments of the present invention or the comparative material of the comparative example is thoroughly mixed with natural graphite (particle size D50 = 15 μm, purchased from BTR Corporation) at a ratio of 1:9 to obtain a negative electrode active material. The negative electrode active material, conductive agent SuperP, binder PVDF and NMP are mixed at a mass ratio of 97.5:1.0:1.5 to prepare a negative electrode slurry (solid content of 50%), which is coated on the current collector copper foil, dried at 100°C, cold pressed at 4MPa at room temperature, and then trimmed, cut, and slit before welding tabs to form a negative electrode sheet.

[0149] (3) Assembly of lithium-ion batteries

[0150] Using a porous PE polymer film as a separator, the prepared positive electrode, separator, and negative electrode are stacked sequentially, with the separator positioned between the positive and negative electrodes, and then wound to obtain a bare battery cell. The bare battery cell is placed in an aluminum-plastic shell package and subjected to a relative vacuum pressure of -0.95 × 10⁻⁶. 5 At Pa, the cells are dried at 100°C until the moisture content is below 100 ppm. The electrolyte, composed of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1) and LiPF6 (concentration 1.0M), is injected into the dried bare cells. The cells are then encapsulated, allowed to stand, formed (0.02C constant current charging for 2 hours, 0.1C constant current charging for 2 hours), shaped, and capacity tested (capacity grading) to produce a soft-pack lithium-ion battery.

[0151] 2. Testing of lithium-ion batteries

[0152] 2.1 First Coulomb efficiency test:

[0153] The batteries prepared above were formed and capacity tested using a battery testing cabinet. The formation step consisted of charging at a constant current of 0.05C for 2.0 hours, followed by charging at a constant current of 0.15C for 2.5 hours. The capacity testing step consisted of charging at a constant current of 0.33C to 4.2V, then charging at a constant voltage of 4.2V to the cutoff current of 0.02C, and discharging at 0.33C to 2.5V. The sum of the above charging capacities and the discharge capacities were recorded as the first charging capacity and the first discharging capacity, and the first charging specific capacity, the first discharging specific capacity, and the first coulombic efficiency were calculated.

[0154] 2.2-rate discharge performance test:

[0155] At 25°C, the battery, after being formed and tested, was charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 0.33C at 25°C, and the 0.33C discharge capacity was recorded. The battery was then charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 3C, and the 3C discharge capacity was recorded.

[0156] 3C discharge capacity retention rate (%) = 3C discharge capacity / 0.33C discharge capacity × 100%

[0157] 2.3 Room temperature cycling performance test:

[0158] At 25°C, the formed and capacity-graded battery was charged to 4.2V at a constant current and constant voltage of 0.5C, with a cutoff current of 0.02C, and allowed to rest for 5 minutes. Then, it was discharged to 2.5V at a constant current of 1C and allowed to rest for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was calculated using the following formula:

[0159] Capacity retention rate (%) after 500 cycles at room temperature = (Discharge capacity after 500 cycles / Discharge capacity after 1 cycle) × 100%.

[0160] 2.4 High-Temperature Cycling Performance Test:

[0161] First, at 25℃, the formed and capacity-securing batteries were charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, the batteries were discharged to 2.5V at 0.33C, and the initial discharge capacity was recorded. The batteries were then placed in a 45℃ high-temperature chamber and charged to 4.2V at a constant current and constant voltage of 0.33C, rested for 5 minutes, discharged to 2.5V at 0.33C, and rested for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was then calculated. The calculation formula is as follows:

[0162] High-temperature capacity retention rate after 500 cycles (%) = (500th cycle discharge capacity / 1st cycle discharge capacity) × 100%.

[0163] The specific results of various tests on liquid lithium-ion batteries are shown in Table 1.

[0164] Table 1 Test Results of Liquid Lithium-ion Batteries

[0165]

[0166] As shown in Table 1, the silicon-carbon materials in Examples 1 to 3 have an initial coulombic efficiency of over 92.2%, a 3C discharge capacity retention rate of over 91.3%, a capacity retention rate of over 84.6% after 500 cycles at room temperature, and a capacity retention rate of over 77.1% after 500 cycles at high temperature, demonstrating excellent application performance.

[0167] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 1 shows that the first-effect and cycle performance of Comparative Example 1 are significantly worse. The possible reason is that in Comparative Example 1, the graphite was not subjected to oxidation intercalation and calcination expansion treatment. The space between layers and pores was not opened, and a large amount of silicon source gas and / or silicon nanoparticles and carbon source gas and / or carbon nanoparticles could not fully enter the interior of the graphite. Most of them may have been deposited on the outer surface of the graphite. The thickness of the silicon-containing layer on the outer surface is too high, which makes it easy for silicon material to expand. It is impossible to give full play to the significant effect of the carbon-silicon-carbon "sandwich" type coating structure and the three-dimensional carbon skeleton conductive hollow structure. In addition, the binding of silicon and carbon is weak, and the coating of silicon is poor, making it difficult to suppress the expansion of silicon particles. Silicon is easy to come into contact with the electrolyte and undergo side reactions, resulting in poor cycle performance.

[0168] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 2 shows that the first efficiency and cycle performance of Comparative Example 2 are significantly worse. The possible reason is that the gas phase carbon coating in step (3) was not carried out in Comparative Example 2, making it difficult to achieve complete coating of silicon material by carbon material. As a result, the silicon nanoparticles deposited in the pores, interlayers and outer surface of the first composite material are easily exposed to the electrolyte. During charge and discharge cycles, silicon expansion is likely to occur, leading to repeated damage and formation of the SEI film, resulting in excessive consumption of lithium ions, which in turn reduces the first efficiency, worsens the cycle performance and conductivity.

[0169] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 3 shows that the cycle performance of Comparative Example 3 is significantly worse. The possible reason is that the particle size of natural graphite is too small, the particle size of the final product is even smaller, various space effects are poor, the specific surface area is too large, resulting in an excessive contact area with the electrolyte, which consumes reversible lithium ions and is not conducive to the utilization of battery capacity.

[0170] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 4 shows that the cycle performance of Comparative Example 4 is significantly worse. The possible reason is that the particle size of natural graphite is too large, which makes it easy to cause structural damage, which is not conducive to uniform slurry preparation. Furthermore, it is easy to cause uneven particle distribution during the coating process, which in turn affects the cycle performance of the battery.

[0171] As shown in Table 1, the analysis of the test results of Example 3 and Comparative Example 5 shows that the first-efficiency and cycle performance of Comparative Example 5 deteriorated. The possible reason is that no pressing step was performed, the bonding between silicon nanoparticles and carbon nanoparticles was relatively poor, the pores or interlayer openings of the expanded graphite were not closed, the compaction density was low, the specific surface area was large, the contact area with the electrolyte was too large, the side reactions and lithium consumption increased, resulting in poor cycle performance.

[0172] In this invention, by expanding ordinary graphite material, the interlayer space within the ordinary carbon material is increased, improving its porosity. Then, high-temperature pyrolysis and vapor deposition of silicon and carbon source gases are simultaneously performed, which helps to suppress the excessive growth of silicon nanocrystals and reduce the silicon grain size, thereby alleviating or suppressing the expansion of silicon particles during charge-discharge cycles. Then, high-temperature vapor deposition coating of carbon source gas is performed again. The reaction parameters and process conditions of each step are strictly controlled to precisely control the amount and effect of silicon and carbon vapor deposition. This successfully deposits silicon and carbon nanoparticles within the pores, interlayers, and defects of the expanded carbon material, and suppresses… The excessive growth of silicon nanocrystals was prevented, the particle size of silicon nanocrystals was suppressed, and the expansion of silicon particles was inhibited. This achieved complete coating of silicon nanoparticles with carbon materials, reduced internal resistance, and, after the gas-phase carbon coating step, the pressing step was used to seal or reduce the pores or interlayer space inside the expanded graphite, reduce the specific surface area of ​​the material, increase the compaction density of the material, promote the bonding between silicon nanoparticles and carbon nanoparticles, and promote complete coating of silicon. This effectively leveraged the close synergistic effect of each step, successfully suppressed the expansion of silicon and improved its conductivity, reduced the contact between silicon and electrolyte, avoided or reduced the generation of side reactions, and was beneficial to improving battery capacity and cycle performance.

[0173] By leveraging the synergistic effects of each step and strictly controlling the process conditions of each step, this invention can fully utilize the significant effects of the carbon-silicon-carbon "sandwich" type coating structure and the three-dimensional carbon skeleton conductive hollow structure, significantly suppressing the expansion of silicon-carbon materials, improving conductivity and specific capacity, avoiding dissolution loss and capacity loss due to direct contact between silicon and electrolyte, and improving the initial coulombic efficiency and cycle performance of silicon-containing negative electrode lithium batteries.

[0174] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. The specific examples used above to illustrate the present invention are only for the purpose of helping to understand the present invention and are not intended to limit the present invention. Those skilled in the art to which this invention pertains can make several simple deductions, modifications, substitutions, or combinations based on the concept of the present invention. These deductions, modifications, substitutions, or combinations also fall within the scope of the claims of the present invention.

Claims

1. A method for preparing a silicon-carbon material, characterized in that, Includes the following steps: (1) In an inert atmosphere, silicon and carbon are deposited in the pores, interlayers, defects and outer surface of expanded graphite by chemical vapor deposition to obtain a first composite material; the ratio of the silicon source gas filling rate to the carbon source gas filling rate is 1:0.01~0.4; the silicon-carbon content of the first composite material is 10~40wt%; (2) In an inert atmosphere, carbon is deposited on the pores, interlayers, defects, and outer surface of the first composite material prepared in step (1) using chemical vapor deposition to obtain the second composite material; the carbon content of the second composite material is 0.5~10wt%; (3) The second composite material obtained in step (2) is pressed and crushed to obtain silicon-carbon material; The expanded graphite is prepared by the following steps: mixing graphite, oxidant and intercalating agent to obtain intercalated expanded graphite, and calcining the intercalated expanded graphite to obtain expanded graphite; the mass ratio of graphite to oxidant to intercalating agent is 1:(0.1~3.0):(1.0~10.0); the particle size Dn50 of graphite is 5.0~100.0μm.

2. The preparation method according to claim 1, characterized in that, The temperature for chemical vapor deposition in step (1) is 400-1000℃; or, In step (1), the silicon source gas is silane or silane; or, in step (1), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; or, the ratio of the silicon source gas charging rate to the carbon source gas charging rate is 1:0.05-0.2; or, Step (2) The silicon carbon content of the first composite material is 20-30 wt%.

3. The preparation method according to claim 2, characterized in that, In step (1), the heating rate of the chemical vapor deposition method is 1~15℃ / min; or, In step (1), the silicon source gas is introduced at a rate of 10~100 L / h; or, In step (1), the carbon source gas is introduced at a rate of 1~10 L / h.

4. The preparation method according to claim 3, characterized in that, In step (1), the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, and the rotational speed of the furnace chamber is 0.5~10.0 rpm; or, In step (1), the silicon source gas charging time is 1.0~10.0 h; or, In step (1), the carbon source gas is introduced for 1.0~10.0 h.

5. The preparation method according to claim 4, characterized in that, In step (1), the chemical vapor deposition method is carried out in a chemical vapor deposition furnace for a rotation time of 0.5 to 20.0 h.

6. The preparation method according to claim 4, characterized in that, In step (1), the chemical vapor deposition method is carried out in a chemical vapor deposition furnace for a rotation time of 1.0~10.0h.

7. The preparation method according to claim 1, characterized in that, The temperature for the chemical vapor deposition method described in step (2) is 400–1000 °C; or, In step (2), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; or, In step (2), the carbon content of the second composite material is 1-6 wt%.

8. The preparation method according to claim 2, characterized in that, The temperature for the chemical vapor deposition method described in step (2) is 400–1000 °C; or, In step (2), the carbon source gas is one or more of methane, ethylene, acetylene, propylene, and propane; or, In step (2), the carbon content of the second composite material is 1-6 wt%.

9. The preparation method according to claim 7, characterized in that, In step (2), the heating rate of the chemical vapor deposition method is 1~15℃ / min; or, In step (2), the carbon source gas is introduced at a rate of 5~50 L / h.

10. The preparation method according to claim 7, characterized in that, In step (2), the chemical vapor deposition method is carried out in a chemical vapor deposition furnace, and the rotational speed of the furnace chamber is 0.5~10.0 rpm; or, In step (2), the carbon source gas is introduced for 0.5 to 2.0 hours.

11. The preparation method according to claim 10, characterized in that, The chemical vapor deposition method is carried out in a chemical vapor deposition furnace, and the rotation time of the chemical vapor deposition furnace cavity is 0.5~2.0h.

12. The preparation method according to any one of claims 1-11, characterized in that, The pressing pressure in step (3) is 150-450 MPa.

13. The preparation method according to claim 12, characterized in that, The compression time is 1.0 to 10.0 min.

14. The preparation method according to any one of claims 1-11, characterized in that, The graphite is one or more of the following: natural graphite, artificial graphite, spherical graphite, and graphitic intermediate phase; or... The graphite has a particle size Dn50 of 20.0–90.0 μm; or, The oxidant is one or more of potassium permanganate, potassium dichromate, chromium trioxide, potassium perchlorate, hydrogen peroxide, and nitric acid; or, The intercalating agent is one or more of sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and glacial acetic acid; or, The mass ratio of graphite to oxidant to intercalating agent is 1:(0.1-3.0):(2.0-10.0).

15. The preparation method according to any one of claims 1-11, characterized in that, The mixing is a stirring mixture, and the stirring temperature is 10-60℃; or, The step prior to calcination includes washing the intercalated expanded graphite with deionized water until the pH of the filtrate is 5-7; the step after washing also includes drying at a temperature of 30-80°C; or... The heating rate for calcination is 1-20℃ / min.

16. The preparation method according to claim 14, characterized in that, The mixing is a stirring mixture, and the stirring temperature is 10-60℃; or, The step prior to calcination includes washing the intercalated expanded graphite with deionized water until the pH of the filtrate is 5-7; the step after washing also includes drying at a temperature of 30-80°C; or... The heating rate for calcination is 1-20℃ / min.

17. The preparation method according to claim 15, characterized in that, The stirring time is 0.5-24.0 hours; or, The drying time is 6.0-24.0 hours; or, The heating rate for calcination is 5-10℃ / min.

18. The preparation method according to claim 15, characterized in that, The stirring speed is 100-3000 rpm; or, The calcination holding temperature is 500-850℃.

19. The preparation method according to claim 18, characterized in that, The heat preservation time is 0.3~6.0h.

20. The preparation method according to claim 18, characterized in that, The heat preservation time is 0.5~2.0h.

21. A silicon-carbon material, characterized in that, It is prepared by any one of claims 1-20.

22. The silicon-carbon material according to claim 21, characterized in that, The silicon-carbon material contains 10-40 wt% silicon-coated carbon.

23. The silicon-carbon material according to claim 21, characterized in that, The silicon-carbon content in the silicon-carbon material is 20-30 wt%.

24. The silicon-carbon material according to any one of claims 21-23, characterized in that, The particle size Dn50 of the silicon-carbon material is 1~60μm.

25. The silicon-carbon material according to claim 24, characterized in that, The particle size Dn50 of the silicon-carbon material is 5~25μm.

26. A negative electrode active material, characterized in that, It contains the silicon-carbon material as described in any one of claims 21-25.

27. A lithium-ion battery negative electrode, characterized in that, It comprises the negative electrode active material, conductive agent, and binder as described in claim 26.

28. A lithium-ion battery, characterized in that, It includes the lithium-ion battery negative electrode as described in claim 27.

Citation Information

Patent Citations

  • Anode plate and manufacturing method therefor, battery using anode plate, and electronic apparatus

    WO2021179219A1

  • Expanded graphite and nano-silicon composite material, preparation method thereof, electrode plate and battery

    CN105355870A

  • Silicon-carbon negative electrode material and preparation method thereof

    CN106602043A

  • Silicon carbon composite material and preparation method thereof

    CN110429262A