A modified carbon material, a method for preparing the same, a negative electrode material composition, and a lithium ion battery

By forming a uniform organic polymer microsphere coating layer on the surface of carbon materials and performing a three-stage calcination process involving boron-doped compounds, the initial coulombic efficiency and cycle performance issues of lithium-ion batteries were solved, thereby improving the energy density and high and low temperature performance of the batteries.

CN116995198BActive Publication Date: 2026-11-20CARBON ONE NEW ENERGY GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211073929.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-02
Publication Date
2026-11-20
Estimated Expiration
2042-09-02

AI Technical Summary

Technical Problem

The initial coulombic efficiency, rate cycle performance, and high and low temperature cycle performance of existing lithium-ion batteries are poor, and there is room for improvement.

Method used

Modified carbon materials with a core-shell structure are used, with a carbon core and an organic polymer pyrolytic carbon coating layer. Polymer microspheres are prepared by emulsion polymerization and a uniform carbonized or graphitized coating layer is formed on the surface of the carbon material. Combined with a three-stage calcination process, boron compounds are doped to promote graphitization.

Benefits of technology

It significantly improves the initial coulombic efficiency, rate discharge performance, and high and low temperature cycling performance of lithium-ion batteries, reduces internal resistance, and improves the lithium intercalation performance of carbon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116995198B_ABST
    Figure CN116995198B_ABST
Patent Text Reader

Abstract

The application discloses a modified carbon material, a preparation method thereof, a negative electrode material composition and a lithium ion battery. The preparation method of the modified carbon material comprises the following steps: mixing a carbon material with an emulsion, stirring and dispersing to obtain a slurry; drying the slurry to obtain a polymer-coated carbon material with a polymer coating layer on the surface of the carbon material; heating the polymer-coated carbon material under an inert atmosphere, carbonizing, and then sieving to obtain a modified carbon material, wherein the heating mode adopts a stepwise heating mode, and the emulsion is a high-molecular polymer microsphere emulsion. By applying the modified carbon material to a lithium ion battery, the first coulomb efficiency, the rate cycle performance and the high and low temperature cycle performance of the lithium ion battery can be improved, and the gram capacity of the carbon negative electrode material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of negative electrode materials for lithium-ion batteries, specifically to a modified carbon material and its preparation method, a negative electrode material composition, and a lithium-ion battery. Background Technology

[0002] Lithium-ion batteries have been widely used in portable electronic products and electric vehicles due to their advantages such as high operating voltage, long cycle life, no memory effect, low self-discharge, and environmental friendliness. Currently, commercially available lithium-ion battery anode materials mainly use carbon anode materials such as natural graphite, artificial graphite, soft carbon, and hard carbon. These materials offer advantages such as inexpensive and readily available raw materials, good conductivity, and high output voltage.

[0003] However, the aforementioned carbon anode materials have room for improvement in terms of specific capacity, initial coulombic efficiency, high-temperature storage capacity retention / recovery rate, rate cycling performance, and high and low temperature cycling performance, and cannot meet the high-performance requirements of future lithium-ion batteries. The charge-discharge power characteristics of carbon anode materials are closely related to the structure of their surface carbon layer. The coating layer of the anode material has a significant impact on its charge-discharge power characteristics and the performance of the solid electrolyte interphase (SEI) film.

[0004] With the development of the electric vehicle industry, higher requirements have been placed on the energy density, initial coulombic efficiency, rate cycling performance, and high and low temperature cycling performance of lithium-ion battery anode materials. Therefore, developing a low-cost and high-performance carbon anode material has become a hot research topic in the industry.

[0005] CN113422030A discloses an anode material, its preparation method, a battery anode, and a lithium-ion battery. The anode material comprises a core and a coating layer covering the core. The core comprises hard carbon, which includes multiple graphite microcrystals. The degree of crosslinking between the graphite microcrystals is 71%-100%, and the ratio of hydrogen atoms to carbon atoms in the anode material is less than 0.03. This technical solution can obtain a high-capacity, low-voltage anode material, but its initial coulombic efficiency and energy density are still not ideal.

[0006] CN101916846B discloses a lithium-ion battery anode composite material and its preparation method. The material uses graphite as a matrix, coated with an organic polymer and / or a conductive polymer. The preparation method involves purifying or graphitizing natural flake graphite, microcrystalline graphite, crystalline vein graphite, needle coke, or petroleum coke to obtain a graphite matrix. The graphite matrix is ​​then liquid-phase mixed with an organic polymer and / or a conductive polymer, spray-dried, and finally oven-dried to obtain the lithium-ion battery anode composite material. The organic polymer is one or more of polyvinyl alcohol, polyvinyl chloride, polyethylene glycol, polyethylene oxide, polyvinylidene fluoride, acrylic resin, and polyacrylonitrile. This method can improve the conductivity of the graphite material to a certain extent, but there is room for improvement in rate discharge performance and long-term cycle performance. Summary of the Invention

[0007] The technical problem solved by this invention is that the initial coulombic efficiency, rate cycle performance, and high and low temperature cycle performance of lithium-ion batteries in the prior art are poor, and there is still room for improvement.

[0008] To address the aforementioned technical problems, this invention provides a modified carbon material and its preparation method, an anode material composition, and a lithium-ion battery. When applied to a lithium-ion battery, the modified carbon material can improve the initial coulombic efficiency, rate cycle performance, and high and low temperature cycle performance of the lithium-ion battery, and can improve the specific capacity of the carbon anode material, etc.

[0009] The objective of this invention can be achieved using the following technical solutions:

[0010] In a first aspect, the present invention provides a modified carbon material having a core-shell structure, wherein the core contains carbon material and the coating layer contains organic polymer pyrolytic carbon.

[0011] The organic polymer pyrolysis carbon is obtained by carbonization treatment of organic polymer;

[0012] The organic polymer is prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, and an initiator using an emulsion polymerization method.

[0013] In some embodiments, based on 100 parts by dry weight of the composition, the styrene monomer comprises 10 to 75 parts, the acrylic hydrophobic monomer comprises 24 to 89 parts, and the initiator comprises 0.001 to 2.0 parts.

[0014] In some embodiments, the organic polymer is prepared by copolymerization of a composition comprising a styrene monomer, an acrylic hydrophobic monomer, a boron-containing compound, and an initiator using an emulsion polymerization method.

[0015] In some embodiments, based on 100 parts by dry weight of the composition, the styrene monomer comprises 10 to 75 parts, the acrylic hydrophobic monomer comprises 24 to 89 parts, the boron-containing compound comprises 0.01 to 5.0 parts, and the initiator comprises 0.001 to 2.0 parts.

[0016] In some embodiments, the boron-containing compound is any one or more of boric acid, metaboric acid, tetraphenylboric acid, sodium borate, sodium metaborate, sodium tetraphenylborate, calcium borate, and boron oxide.

[0017] In some embodiments, the polymer microspheres are prepared by copolymerization using an emulsion polymerization method from a composition comprising styrene monomers, acrylic hydrophobic monomers, water-soluble polymers, boron-containing compounds, and an initiator.

[0018] In some embodiments, based on 100 parts by dry weight of the composition, the styrene monomer comprises 10-48 parts, the acrylic hydrophobic monomer comprises 24-89 parts, preferably 24.5-89.28 parts, the water-soluble polymer comprises 0.5-25.0 parts, the boron-containing compound comprises 0.01-5.0 parts, preferably 0.1-5.0 parts, more preferably 0.2-2.0 parts, and the initiator comprises 0.001-2.0 parts, preferably 0.02-0.5 parts.

[0019] In some embodiments, the water-soluble polymer comprises one or more of chitosan, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylamide, and polyacrylic acid.

[0020] In some embodiments, the modified carbon material has a particle size D50 of 8–25 μm, preferably 10–20 μm, and a specific surface area of ​​2.0–4.0 m². 2 / g, preferably 2.5–3.5m 2 / g.

[0021] In some embodiments, the coating layer accounts for 0.1% to 10% of the total mass of the modified carbon material.

[0022] Secondly, the present invention provides a method for preparing the modified carbon material, comprising the following steps:

[0023] (1) The carbon material is mixed with the emulsion and stirred to disperse it, thus obtaining a slurry;

[0024] (2) The slurry is dried to obtain a polymer-coated carbon material with a polymer coating layer on the surface of the carbon material;

[0025] (3) The polymer-coated carbon material is heated in an inert atmosphere to carbonize it, and then sieved to obtain modified carbon material, wherein the heating method adopts a step heating method.

[0026] In some implementations, in step (1), water and carboxymethyl cellulose are first added and stirred to form a gel, and then emulsion and carbon materials are added and stirred to disperse to obtain a slurry;

[0027] In some embodiments, the stirring speed for mixing and applying the adhesive is 200–600 rpm, and the mixing and applying time is 20–60 min;

[0028] In some embodiments, the stirring speed for the stirring dispersion is 200–600 rpm, and the stirring dispersion time is 20–60 min;

[0029] In some embodiments, the solid content of the emulsion is 25-50%, preferably 30-40%;

[0030] In some embodiments, the solid content of the slurry is 10-60%, preferably 20-40%.

[0031] In some embodiments, the mass ratio of the carbon material to the carboxymethyl cellulose is 1:0.0005 to 0.002, or

[0032] The mass ratio of the carbon material to the dry weight of the emulsion is 1:0.05 to 0.30, preferably 1:0.05 to 0.20.

[0033] In some embodiments, the emulsion is a polymer microsphere emulsion;

[0034] In some embodiments, the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, and an initiator using an emulsion polymerization method;

[0035] In some embodiments, based on 100 parts by dry total mass of the composition, the styrene monomer is 10 to 75 parts, the acrylic hydrophobic monomer is 24 to 89 parts, and the initiator is 0.001 to 2.0 parts.

[0036] In some embodiments, the styrene monomer comprises one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene;

[0037] In some embodiments, the acrylic hydrophobic monomer comprises one or more of ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, nonyl heptaacrylate, octyl methacrylate, nonyl methacrylate, and decyl methacrylate.

[0038] In some embodiments, the initiator is a peroxide;

[0039] In some implementations, the water is pure water or deionized water;

[0040] In some embodiments, the carbon material is one or more of the following: natural graphite, artificial graphite, porous carbon, carbon fiber, mesophase carbon microspheres, hard carbon, soft carbon, graphite fiber, petroleum coke, needle coke, organic polymer pyrolysis carbon, resin carbon, carbon black, and amorphous carbon.

[0041] In some embodiments, the emulsion is a polymer microsphere emulsion, wherein the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, boron-containing compounds and an initiator using an emulsion polymerization method;

[0042] In some embodiments, based on 100 parts by dry weight of the composition, the styrene monomer comprises 10 to 75 parts, the acrylic hydrophobic monomer comprises 24 to 89 parts, the boron-containing compound comprises 0.01 to 5.0 parts, and the initiator comprises 0.001 to 2.0 parts.

[0043] In some embodiments, the boron-containing compound is any one or more of boric acid, metaboric acid, tetraphenylboric acid, sodium borate, sodium metaborate, sodium tetraphenylborate, calcium borate, and boron oxide.

[0044] In some embodiments, the emulsion is a polymer microsphere emulsion, wherein the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, water-soluble polymers, boron-containing compounds and initiators using an emulsion polymerization method;

[0045] In some embodiments, based on 100 parts by dry weight of the composition, the styrene monomer is 10 to 48 parts, the acrylic hydrophobic monomer is 24 to 89 parts, the water-soluble polymer is 0.5 to 25.0 parts, the boron-containing compound is 0.01 to 5.0 parts, and the initiator is 0.001 to 2.0 parts.

[0046] In some embodiments, the water-soluble polymer comprises one or more of chitosan, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylamide, and polyacrylic acid.

[0047] In some implementations, in step (2), the drying is carried out by spray drying, wherein the inlet temperature of the spray dryer is 150-400°C, preferably 200-300°C, and the outlet temperature is 70-150°C, preferably 90-130°C.

[0048] In some embodiments, in step (3), the polymer-coated carbon material is heated to 300-500°C, preferably 350-450°C, at a heating rate of 60-120°C / h under an inert atmosphere, and then held at that temperature for 2-5 hours.

[0049] Next, the temperature is increased to 800-2000℃, preferably 800-1300℃, and more preferably 1000-1200℃, at a heating rate of 60-120℃ / h, and held for 3-10 hours. Then, the temperature is allowed to drop naturally. After discharge, the material is broken up and sieved to obtain modified carbon material.

[0050] In some embodiments, in step (3), the polymer-coated carbon material is heated to 300-500°C, preferably 350-450°C, at a heating rate of 60-120°C / h under an inert atmosphere, and then held at that temperature for 2-5 hours.

[0051] Next, the temperature is increased to 800-2000°C at a heating rate of 60-120°C / h, preferably 800-1300°C, more preferably 1000-1200°C, and held for 3-10 hours;

[0052] Next, the temperature is increased to 2500-3500℃ at a heating rate of 60-120℃ / h and held for 1-5 hours; then it is cooled naturally, and after discharge, it is broken up and sieved to obtain modified carbon material.

[0053] In some embodiments, a modified carbon material is prepared by a method for preparing said modified carbon material.

[0054] Thirdly, the present invention provides a negative electrode material composition containing the modified carbon material or the modified carbon material prepared by the method for preparing the modified carbon material.

[0055] The composition comprises, by dry weight, 100% of the total mass of the negative electrode material composition, 95.0-98.0% of the modified carbon material, 0.5-2.0% of the conductive agent, and 1.0-3.0% of the binder.

[0056] Fourthly, the present invention provides a lithium-ion battery containing the aforementioned negative electrode material composition.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] (1) This invention first coats a layer of polymer microspheres on the surface of carbon materials. The polymer microspheres are formed by a unique polymer preparation composition. By precisely controlling the type and proportion of each monomer or compound in the composition, the compounding effect between the components is brought into play. By strictly controlling the reaction conditions of each process step, the synergistic effect between the steps is brought into play. Unexpectedly excellent polymer microsphere coating modification effect, excellent adhesion characteristics, and special spatial effect are obtained. Then, after drying and high temperature treatment, a carbonized coating layer or graphitized coating layer with uniform thickness distribution can be formed on the surface of carbon materials. It has excellent adhesion and coating effect as well as electrical and ion conduction properties, thereby improving the specific capacity of carbon materials, reducing internal resistance, which is conducive to the formation and stability of SEI film on the surface of carbon materials, and is conducive to improving rate performance and cycle performance.

[0059] (2) Furthermore, by adding a specific amount of boron-containing compound to the composition for preparing polymer microsphere emulsions and leveraging the synergistic effect of the three-stage calcination process, graphitization is significantly promoted, thereby significantly improving capacity and first-cycle efficiency, enhancing the lithium intercalation performance of carbon materials, and reducing internal resistance. Compared with existing technologies, this significantly improves rate performance and cycle performance, achieving unexpectedly significant results. After applying the negative electrode material of this invention, the first-cycle efficiency, high-temperature storage performance, rate discharge performance, and high and low temperature cycle performance of lithium-ion batteries can be improved. Attached Figure Description

[0060] Figure 1 This is a SEM image of the modified carbon material prepared in Example 6.

[0061] Figure 2 The image shows a SEM image of the polymer-coated carbon material powder with a polymer coating layer on the surface of the carbon material prepared in step (2) of Example 6. Detailed Implementation

[0062] In this specification, unless otherwise specified, notations, units, abbreviations, and terms have the following meanings. For example, when using ~ or - to indicate a range of values, they include both endpoints, and the units are common.

[0063] To better understand the above technical solution, the present invention will be further described in detail below.

[0064] In a first aspect, the present invention provides a method for preparing a modified carbon material, comprising the following steps:

[0065] (1) The carbon material is mixed with the emulsion and stirred to disperse it, thus obtaining a slurry;

[0066] (2) The slurry is dried to obtain a polymer-coated carbon material with a polymer coating layer on the surface of the carbon material;

[0067] (3) The polymer-coated carbon material is heated in an inert atmosphere to carbonize it, and then sieved to obtain modified carbon material, wherein the heating method adopts a step heating method.

[0068] Preferably, in step (1), water and carboxymethyl cellulose are added first, and the mixture is stirred and gelled. Then, emulsion and carbon materials are added, and the mixture is stirred and dispersed to obtain a slurry.

[0069] Pre-adding carboxymethyl cellulose (CMC) for gelling helps improve the dispersion stability of various materials in the slurry system. Before drying the slurry, it needs to be stored or transported to a dryer, requiring the maintenance of its stability. Adding an appropriate amount of CMC helps improve slurry stability, prevents slurry separation into liquid and solid phases, and avoids clumping or incomplete drying during the drying process.

[0070] Furthermore, by pre-adding carboxymethyl cellulose for sizing, a colloidal solution of a certain viscosity can be formed, which can act as a thickener, emulsifier, or suspender, helping to stabilize the morphology of the emulsion microspheres. When the composition for preparing emulsion polymer microspheres contains only two monomers, styrene-based monomers and acrylic hydrophobic monomers, the prepared microsphere emulsion is relatively unstable. By adding the freshly prepared polymer microsphere emulsion to the carboxymethyl cellulose sizing solution in the first half of the slurry preparation process, the stability of the microspheres in the polymer microsphere emulsion can be improved.

[0071] By thoroughly stirring and dispersing the microsphere emulsion-form polymer with carbon materials, polymer microspheres can be uniformly coated on the surface of carbon materials, leveraging the microstructural effect of microsphere coating. Compared with ordinary polymer coating, this method achieves superior coating effect, which is beneficial for promoting the formation of SEI film and improving rate performance and cycle performance.

[0072] A dispersion disc or a propeller-type agitator is preferably used in the stirring and dispersing process.

[0073] Preferably, the stirring speed for mixing and applying the adhesive is 200-600 rpm, and the stirring and applying time is 20-60 min; the stirring speed for mixing and dispersing is 200-600 rpm, and the mixing and dispersing time is 20-60 min.

[0074] Preferably, the solid content of the emulsion is 25-50%, more preferably 30-40%, taking into account the stability and applicability of the emulsion, as long as the expected effect can be achieved.

[0075] Preferably, the solid content of the slurry is 10-60%, more preferably 20-40%, more preferably 25-30%, and even more preferably 25.2-26.7%. This is to take into account the stability and applicability of the slurry, which is conducive to the uniform coating of carbon materials by emulsion microspheres. As long as the expected effect can be achieved, it is acceptable.

[0076] Regarding the solid content of the slurry, if the solid content is too low, the concentration of the slurry will be too low, and the emulsion microspheres may not easily adhere to and coat the carbon material, which may be detrimental to the cycle performance and put a burden on the subsequent drying process; if the solid content is too high, the concentration of the slurry will be too high, making it difficult to fully stir and disperse the carbon material, which is not conducive to uniformly coating the carbon material and is not conducive to subsequent dispersion and drying.

[0077] Preferably, the mass ratio of the carbon material to the carboxymethyl cellulose is 1:0.0005 to 0.002.

[0078] The mass ratio of the carbon material to the dry weight of the emulsion is 1:0.05 to 0.30, preferably 1:0.05 to 0.20.

[0079] Preferably, in the above-mentioned method for preparing modified carbon materials, the emulsion is a polymer microsphere emulsion, wherein the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, and an initiator using an emulsion polymerization method;

[0080] Of which, based on 100 parts of the total dry weight of the composition, styrene monomers comprise 10 to 75 parts; acrylic hydrophobic monomers comprise 24 to 89 parts, preferably 24.5 to 89.98 parts; and initiator comprises 0.001 to 2.0 parts, preferably 0.02 to 0.5 parts.

[0081] Preferably, the styrene monomer comprises one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene.

[0082] The styrene monomers can impart excellent adhesion and toughness to the polymer microspheres. The styrene monomers are copolymerized with other components such as hydrophobic acrylic monomers to form polymer microspheres, which improves the adhesion between the microspheres and carbon materials such as graphite, and helps to form a coating layer. After high-temperature treatment, the microspheres can form a carbon layer structure in the form of single-layer particles, uniformly coating the surface of carbon materials, thereby improving charge-discharge cycle performance and power characteristics.

[0083] Preferably, the acrylic hydrophobic monomer comprises one or more of ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, nonyl heptaacrylate, octyl methacrylate, nonyl methacrylate, and decyl methacrylate.

[0084] The acrylic hydrophobic monomers can diffuse into the micelles of the emulsion to form stable latex particles, which is beneficial for preparing polymer microspheres. This imparts excellent spatial structure effects, superior impact resistance, elasticity, and toughness to the polymer microspheres, giving them good lithium-ion conduction properties. At the same time, it can enhance the bonding force between the negative electrode active particles and the current collector.

[0085] Preferably, the initiator is a peroxide;

[0086] Preferably, the water is pure water or deionized water;

[0087] The amount of water added relative to 100 parts of the total dry weight of the composition can be, for example, 60-1000 parts, preferably 100-500 parts, and is not particularly limited as long as the desired emulsion copolymerization effect can be obtained.

[0088] Preferably, the carbon material is one or more of the following: natural graphite, artificial graphite, porous carbon, carbon fiber, mesophase carbon microspheres, hard carbon, soft carbon, graphite fiber, petroleum coke, needle coke, organic polymer pyrolysis carbon, resin carbon, carbon black, and amorphous carbon.

[0089] The particle size D50 of the carbon material is 5-45 μm, preferably 8-25 μm, more preferably 10-20 μm, and even more preferably 10-15 μm. There are no particular limitations as long as the expected negative electrode material performance can be obtained.

[0090] More preferably, in the above-mentioned method for preparing modified carbon materials,

[0091] The emulsion is a polymer microsphere emulsion, wherein the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, boron-containing compounds and initiators using an emulsion polymerization method.

[0092] Of which, based on 100 parts by dry weight of the composition, styrene monomers comprise 10-75 parts, preferably 10-73 parts; acrylic hydrophobic monomers comprise 24-89 parts, preferably 24.5-89.78 parts; boron-containing compounds comprise 0.01-5.0 parts, preferably 0.1-5.0 parts, more preferably 0.2-2.0 parts; and initiator comprises 0.001-2.0 parts, preferably 0.02-0.5 parts.

[0093] The boron-containing compound is any one or more of boric acid, metaboric acid, tetraphenylboric acid, sodium borate, sodium metaborate, sodium tetraphenylborate, calcium borate, and boron oxide.

[0094] By fully dissolving and dispersing boron-containing compounds in an emulsion system containing styrene-based monomers and hydrophobic acrylic monomers in an emulsion reactor, and then uniformly distributing them in the polymer microsphere emulsion, boron atoms are doped into the carbonized coating layer in the form of boron-oxygen or boron-carbon after drying and high-temperature sintering. This helps improve the overall conductivity of the carbon material, reduce internal resistance, and improve cycle performance. Even a small portion of boron atoms can penetrate into the pores or interlayers of the carbon material, increasing the interlayer spacing and facilitating lithium-ion insertion and extraction.

[0095] By doping boron into the carbon coating layer, the high conductivity of boron allows it to react with lithium, improving the affinity of the carbon material for lithium. Furthermore, the relatively large boron atom size alters the carbon layer structure, providing more lithium insertion sites. This improves the low-temperature performance of the modified carbon material, enhances lithium-ion conductivity, reduces internal resistance, and further improves rate performance and charge-discharge cycle performance. Additionally, during the three-stage sintering process, boron doping promotes graphitization, improving capacity and first-time efficiency. Moreover, by replacing carbon in the graphite crystals with boron, the conductivity and ion-conductivity of the carbon material are enhanced, reducing internal resistance.

[0096] More preferably, in the above-mentioned method for preparing modified carbon materials, the emulsion is a polymer microsphere emulsion, wherein the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, water-soluble polymers, boron-containing compounds and initiators using an emulsion polymerization method;

[0097] Of which, based on 100 parts of the total dry weight of the composition, styrene monomers comprise 10-48 parts, acrylic hydrophobic monomers comprise 24-89 parts, preferably 24.5-89.28 parts, water-soluble polymers comprise 0.5-25.0 parts, boron-containing compounds comprise 0.01-5.0 parts, preferably 0.1-5.0 parts, more preferably 0.2-2.0 parts, and initiator comprises 0.001-2.0 parts, preferably 0.02-0.5 parts;

[0098] Preferably, the water-soluble polymer comprises one or more of chitosan, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylamide, and polyacrylic acid, and more preferably one or more of polyvinyl alcohol, polyacrylamide, and polyacrylic acid. The molecular weight of the water-soluble polymer is 1,000 to 1,000,000.

[0099] The addition of the water-soluble polymer helps improve the dispersibility of polymer microspheres in the system, enhances the stability of the polymer microspheres during preparation, prevents gelation, leverages the spatial effect of uniform coating of emulsion microspheres, and improves the coating effect of organic matter. However, if the amount of water-soluble polymer is too large, it may lead to a decrease in the particle size and carbon content of the polymer microspheres, thereby affecting conductivity and power characteristics.

[0100] Preferably, the initiator is a peroxide; the initiator can generate free radicals with initiation activity to initiate polymerization in aqueous solution, emulsion or micelles, thereby achieving chain growth.

[0101] The initiator is not particularly limited as long as it can achieve the desired initiation effect. The peroxide can be an inorganic oxide, such as ammonium persulfate, potassium persulfate, sodium persulfate, etc. Further, the peroxide can be a hydroperoxide, acyl peroxide, dialkyl peroxide, ester peroxide, ketone peroxide, dicarbonate peroxide, etc., specifically tert-butyl hydroperoxide, cumene hydroperoxide, benzoyl peroxide (BPO), dodecyl peroxide (LPO), lauroyl peroxide, dicumyl peroxide, tert-butyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxyvalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxide, dicyclohexyl peroxide, etc., and the first initiator can also be azobisisobutyronitrile, azobisisoheptanenitrile, etc.

[0102] Furthermore, the initiator is preferably ammonium persulfate, benzoyl peroxide, etc., and the amount added is not particularly limited as long as the expected effect can be achieved.

[0103] The polymer microspheres used in this invention are formed by polymerization of a monomer combination containing multiple functional monomers in specific proportions. They possess excellent bonding properties and structural effects, and can uniformly coat the surface of carbon materials in the form of monolayer microspheres. After high-temperature treatment, a uniformly thick hard carbon coating layer or graphite coating layer with excellent adhesion is formed on the carbon material surface. This uniform coating structure can improve the formation of the SEI film on the carbon material surface, improve the lithium intercalation characteristics of the negative electrode material, reduce the internal resistance of the lithium-ion battery, and enhance rate discharge performance and charge-discharge cycle performance.

[0104] Preferably, the particle size of the polymer microspheres is 0.05–5.0 μm, more preferably 0.1–1.0 μm, and even more preferably 0.2–0.6 μm. This is to ensure the stability of the microsphere emulsion and to prevent gelation of the emulsion. If the particle size is too large, the coating layer may be too thick, which is not conducive to lithium intercalation and affects charge-discharge cycle performance. If the particle size is too small, the carbon coating layer may be too thin, which may lead to reduced conductivity and charge-discharge power.

[0105] Thermogravimetric analysis (TGA) can be used to analyze the residual mass of polymer microspheres. For example, after drying the polymer microspheres, they are sintered at 1100-1400°C under a nitrogen atmosphere for 1-10 hours, and the residual mass rate is calculated. There is no particular limitation on the residual mass rate, as long as the desired effect is achieved; for example, it can be 20-50%, preferably 25-35%, and more preferably 30-35%. By pre-measuring the residual mass rate of the polymer microspheres, the mass percentage of the carbon coating layer in the modified carbon material can be indirectly derived based on the input mass of the polymer microspheres and carbon material. The mass percentage of the carbon coating layer in the modified carbon material can be, for example, 1-10%, preferably 1-7%.

[0106] Preferably, in step (2) of the above preparation method, the drying is carried out by spray drying, the inlet temperature of the spray drying is 150-400℃, preferably 200-300℃, and the outlet temperature is 70-150℃, preferably 90-130℃.

[0107] If the inlet temperature of the spray dryer is too high, the material is prone to agglomeration, which can damage the equipment. If the inlet temperature is too low, the material cannot be completely dried, resulting in excessive moisture content. The particle size of the polymer microspheres after drying may decrease slightly, but this has no impact on performance.

[0108] Preferably, in step (3) of the above preparation method, the polymer-coated carbon material is heated to 300-500°C, preferably 350-450°C, at a heating rate of 60-120°C / h under an inert atmosphere, and then held at that temperature for 2-5 hours; then, the temperature is raised to 800-2000°C, preferably 800-1300°C, more preferably 1000-1200°C, at a heating rate of 60-120°C / h, and held at that temperature for 3-10 hours, and then cooled naturally. After discharge, the material is broken up and sieved to obtain the modified carbon material.

[0109] In the heating and carbonization step of the polymer-coated carbon material of the present invention, a stepped heating method is preferred. This is beneficial for the organic matter such as polymers to decompose slowly in stages, slowly losing elements such as hydrogen and oxygen. It avoids the formation of porous and non-dense conditions in the coating layer due to rapid decomposition, which is conducive to uniform carbonization, ensuring the consistency and density of the carbonized coating layer, and obtaining an excellent and uniform coating structure.

[0110] In the two-stage heating and holding method, in the first heating stage, the temperature is raised to 300-500℃ and held, causing the polymer to begin to decompose and slowly lose its hydrogen, oxygen, and other elements, thus avoiding the formation of porous structures due to rapid decomposition and volatilization at high temperatures. In the second heating stage, the temperature is raised to 800-2000℃, preferably 800-1300℃, and held, further decomposition and carbonization are carried out based on the decomposition in the first stage, avoiding the destruction of the carbon layer structure and improving the uniformity of carbonization.

[0111] In the heating and carbonization step of this invention, considering that there is an exothermic process during the carbonization of organic polymers, this invention uniquely employs a rotary kiln for heating and carbonization. The rotary kiln can rotate the material while performing heat treatment, and its relatively large processing space facilitates heat dissipation and uniform carbonization, resulting in more uniform internal and surface temperatures of the polymer-coated carbon material, thus improving the uniformity of the carbonization process. A roller kiln can also be used in the heating and carbonization step of this invention.

[0112] Preferably, in step (3), the polymer-coated carbon material is heated to 300-500°C, preferably 350-450°C, at a heating rate of 60-120°C / h under an inert atmosphere, and then held at that temperature for 2-5 hours; then, the temperature is raised to 800-2000°C, preferably 800-1300°C, more preferably 1000-1200°C, at a heating rate of 60-120°C / h, and held at that temperature for 3-10 hours; then, the temperature is raised to 2500-3500°C, preferably 2800-3200°C, at a heating rate of 60-120°C / h, and held at that temperature for 1-5 hours, preferably 2-4 hours; then, the temperature is allowed to cool naturally, and after discharge, the material is broken up and sieved to obtain the modified carbon material.

[0113] Preferably, the present invention employs a three-stage heating and holding process. After the two-stage heating and holding processes described above, the temperature is further increased to 2500-3500℃ and held for 1-5 hours to further graphitize the carbonized coating carbon material. This further improves the specific capacity and initial coulombic efficiency of the modified carbon material, reduces internal resistance, and enhances charge-discharge cycle performance and high-temperature storage capacity. Preferably, the three-stage heating process during boron doping fully utilizes the doping effect of boron and promotes graphitization, leveraging the synergistic effect of each component and step.

[0114] For the discharged material, it is preferable to use ball mill dispersers, turbine dispersers, mechanical dispersers, VC mixers, etc., to disperse it and eliminate any potential agglomeration. Large particles can be prevented by sieving, with screen meshes ranging from 200 to 500 mesh. After sieving, further classification can remove extremely fine powders. After sieving, demagnetization can also be performed, for example, using electromagnetic demagnetization, employing a demagnetizer or electromagnetic separator.

[0115] In a second aspect, the present invention provides a modified carbon material having a core-shell structure, comprising a core and a coating layer, wherein the core contains carbon material and the coating layer contains organic polymer pyrolytic carbon.

[0116] The organic polymer pyrolysis carbon is obtained by carbonization treatment of organic polymer;

[0117] Preferably, the organic polymer is prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, and an initiator using an emulsion polymerization method.

[0118] Of which, based on 100 parts of the total dry weight of the composition, styrene monomers comprise 10-75 parts, acrylic hydrophobic monomers comprise 24-89 parts, and initiator comprises 0.001-2.0 parts.

[0119] More preferably, the organic polymer is prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, boron-containing compounds, and an initiator using an emulsion polymerization method.

[0120] Of which, based on 100 parts by dry weight of the total composition, styrene monomers comprise 10-75 parts, acrylic hydrophobic monomers comprise 24-89 parts, boron-containing compounds comprise 0.01-5.0 parts, and initiator comprises 0.001-2.0 parts.

[0121] Preferably, the boron-containing compound is any one or more of boric acid, metaboric acid, tetraphenylboric acid, sodium borate, sodium metaborate, sodium tetraphenylborate, calcium borate, and boron oxide, and more preferably any one or more of boric acid, metaboric acid, tetraphenylboric acid, and sodium borate. Metaboric acid also has a dehydrating effect, reacting with moisture in the environment to generate boric acid, which helps maintain battery performance.

[0122] The modified carbon material can be prepared by the above-described preparation method.

[0123] The particle size D50 of the modified carbon material was determined using a laser particle size analyzer to be 8–25 μm, preferably 10–20 μm, and more preferably 10.5–17.5 μm.

[0124] The specific surface area of ​​the modified carbon material was measured using a TriStar II 3020 BET surface area analyzer, and the measured specific surface area was 2.0–4.0 m². 2 / g, preferably 2.5–3.5m 2 / g, more preferably 2.6–3.3m 2 / g, and the tap density measured using conventional methods is 1.0-1.2 g / cm³. 3 Specific capacity ≥350.0mAh / g.

[0125] The percentage of the coating layer mass to the total mass of the modified carbon material is 0.1-10.0%, preferably 0.5-10.0%, more preferably 2-8%, and even more preferably 4-6%.

[0126] Thirdly, the present invention provides a negative electrode material composition that uses the aforementioned modified carbon material.

[0127] The composition comprises, by dry weight, 100% of the total mass of the negative electrode material composition, 95.0-98.0% of the modified carbon material, 0.5-2.0% of the conductive agent, and 1.0-3.0% of the binder.

[0128] The conductive agent comprises one or more of the following: conductive carbon black, conductive graphite, modified conductive graphite, metal particles, Ketjen black, acetylene black, carbon nanotubes, carbon fibers, graphene, and conductive polymers.

[0129] The adhesive comprises one or more of the following: polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-propylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-ethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer.

[0130] Fourthly, the present invention provides a lithium-ion battery negative electrode that uses the above-mentioned negative electrode material composition.

[0131] Fifthly, the present invention provides a lithium-ion battery that uses the above-mentioned negative electrode material composition.

[0132] All raw materials and reagents used in this invention were purchased from mainstream manufacturers. Those without specified manufacturers or concentrations are all analytically pure raw materials or reagents that are readily available. There are no particular restrictions as long as they achieve the intended effect. The reaction vessels, mixers, rotary kilns, roller kilns, spray dryers, specific surface area analyzers, and other instruments and equipment used in this embodiment were all purchased from major manufacturers. There are no particular limitations as long as they achieve the intended effect. Where specific techniques or conditions are not specified in this embodiment, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions.

[0133] The raw materials and equipment used in the following examples and comparative examples are as follows. Styrene, acrylate, boric acid, etc., were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., and natural graphite, artificial graphite, etc., were purchased from BTR Corporation.

[0134] The present invention will now be described in more detail with reference to examples and comparative examples, but the scope of the present invention is not limited to these examples. It should be noted that, unless otherwise specified, all percentages, parts, and ratios used in the present invention are based on mass.

[0135] Example 1

[0136] (1) Preparation of slurry

[0137] (1.1) Preparation of polymer microsphere emulsion

[0138] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 70°C. 0.1 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.02 parts of ammonium persulfate by dry weight) were added. Then, 10.0 parts of styrene and 89.98 parts of ethyl acrylate were added to the reactor, and the mixture was stirred at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for 4 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 30% using deionized water.

[0139] The particle size D50 of the polymer microspheres was determined to be 0.32 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 30.1%.

[0140] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0141] First, add 300 parts water and 0.05 parts carboxymethyl cellulose, and stir and beat at 200 rpm for 60 min. Then, add 16.7 g of the above emulsion with a solid content of 30% (equivalent to 5 parts on dry weight) and 100 parts natural graphite (particle size D50 of 10 μm), and stir and disperse at 200 rpm for 60 min to obtain a slurry with a solid content of 25.2%.

[0142] (2) Preparation of polymer-coated carbon materials

[0143] The above slurry was dried using a spray dryer with an inlet temperature of 200°C and an outlet temperature of 90°C to obtain a polymer-coated carbon material powder with a polymer coating on the surface of the carbon material.

[0144] (3) Preparation of modified carbon materials

[0145] The polymer-coated carbon material was heated to 350°C at a heating rate of 60°C / h under a nitrogen atmosphere and then held at that temperature for 5 hours. Next, the temperature was increased to 800°C at a heating rate of 60°C / h and held for 10 hours. Then, the material was allowed to cool naturally. After discharge, the material was dispersed using a ball mill, passed through a 300-mesh sieve, and demagnetized using a demagnetizer to obtain the modified carbon material.

[0146] The modified carbon material was determined to have a particle size of 10.5 μm and a specific surface area of ​​3.3 m². 2 / g.

[0147] Example 2

[0148] (1) Preparation of slurry

[0149] (1.1) Preparation of polymer microsphere emulsion

[0150] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 80°C. 2.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.5 parts of ammonium persulfate by dry weight) were added. Then, 75.0 parts of styrene and 24.5 parts of ethyl acrylate were added to the reactor, and the mixture was stirred at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for another 2 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 40% using deionized water.

[0151] The particle size D50 of the polymer microspheres was determined to be 0.58 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 34.5%.

[0152] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0153] First, add 300 parts water and 0.2 parts carboxymethyl cellulose, and stir and beat at 600 rpm for 20 minutes. Then, add 50g of the above emulsion with a solid content of 40% (equivalent to 20 parts on dry weight) and 100 parts natural graphite (particle size D50 of 15μm), and stir and disperse at 600 rpm for 20 minutes to obtain a slurry with a solid content of 26.7%.

[0154] (2) Preparation of polymer-coated carbon materials

[0155] The above slurry was dried using a spray dryer with an inlet temperature of 300°C and an outlet temperature of 130°C to obtain a polymer-coated carbon material powder with a polymer coating on the surface of the carbon material.

[0156] (3) Preparation of modified carbon materials

[0157] The polymer-coated carbon material was heated to 450°C at a heating rate of 120°C / h under a nitrogen atmosphere and then held at that temperature for 2 hours. Next, the temperature was increased to 1300°C at a heating rate of 120°C / h and held at that temperature for 3 hours. Then, the material was allowed to cool naturally. After discharge, the material was dispersed using a ball mill, passed through a 300-mesh sieve, and demagnetized using a demagnetizer to obtain the modified carbon material.

[0158] The modified carbon material has a particle size of 17.3 μm and a specific surface area of ​​2.7 m². 2 / g.

[0159] Example 3

[0160] (1) Preparation of slurry

[0161] (1.1) Preparation of polymer microsphere emulsion

[0162] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 40.0 parts of styrene and 59.90 parts of ethyl acrylate were added to the reactor, and the mixture was stirred at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for 3 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0163] The particle size D50 of the polymer microspheres was determined to be 0.52 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 32.9%.

[0164] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0165] First, add 300 parts water and 0.1 parts carboxymethyl cellulose, and stir and beat at 400 rpm for 30 minutes. Then, add 30g of the above emulsion with a solid content of 35% (equivalent to 10.5 parts on dry weight) and 100 parts natural graphite (particle size D50 of 12μm), and stir and disperse at 400 rpm for 30 minutes to obtain a slurry with a solid content of 25.7%.

[0166] (2) Preparation of polymer-coated carbon materials

[0167] The above slurry was dried using a spray dryer with an inlet temperature of 260°C and an outlet temperature of 120°C to obtain a polymer-coated carbon material powder with a polymer coating layer on the surface of the carbon material.

[0168] (3) Preparation of modified carbon materials

[0169] The polymer-coated carbon material was heated to 400°C at a heating rate of 80°C / h under a nitrogen atmosphere and then held at that temperature for 3 hours. Next, the temperature was increased to 1100°C at a heating rate of 80°C / h and held at that temperature for 6 hours. Then, the material was allowed to cool naturally. After discharge, the material was dispersed using a ball mill, passed through a 300-mesh sieve, and demagnetized using a demagnetizer to obtain the modified carbon material.

[0170] The modified carbon material has a particle size of 13.2 μm and a specific surface area of ​​3.0 m². 2 / g.

[0171] Example 4

[0172] (1) Preparation of slurry

[0173] (1.1) Preparation of polymer microsphere emulsion

[0174] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 70°C. Then, 0.1 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.02 parts of ammonium persulfate by dry weight) were added. Next, 10.0 parts of styrene, 89.78 parts of ethyl acrylate, and 0.2 parts of metaboric acid were added to the reactor. The mixture was stirred at 600 rpm and added uniformly over 2 hours. After the addition was complete, the reaction continued for 4 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 30% using deionized water.

[0175] The particle size D50 of the polymer microspheres was determined to be 0.37 μm using a laser particle size analyzer. After drying the polymer microspheres, they were sintered at 1200 °C under a nitrogen atmosphere for 2 hours, and the residual mass was 30.3%.

[0176] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0177] First, add 300 parts water and 0.05 parts carboxymethyl cellulose, and stir and beat at 200 rpm for 60 min. Then, add 16.7 g of the above emulsion with a solid content of 30% (equivalent to 5 parts on dry weight) and 100 parts natural graphite (particle size D50 of 10 μm), and stir and disperse at 200 rpm for 60 min to obtain a slurry with a solid content of 25.2%.

[0178] (2) Preparation of polymer-coated carbon materials

[0179] The above slurry was dried using a spray dryer with an inlet temperature of 200°C and an outlet temperature of 90°C to obtain a polymer-coated carbon material powder with a polymer coating on the surface of the carbon material.

[0180] (3) Preparation of modified carbon materials

[0181] The polymer-coated carbon material was heated to 350°C at a heating rate of 60°C / h under a nitrogen atmosphere and held at that temperature for 5 hours. Then, it was heated to 800°C at a heating rate of 60°C / h and held for 10 hours. Next, it was heated to 2800°C at a heating rate of 60°C / h and held for 4 hours. Then, it was cooled naturally, discharged, and dispersed using a ball mill. The material was then passed through a 300-mesh sieve and demagnetized using a demagnetizer to obtain the modified carbon material.

[0182] The modified carbon material has a particle size of 10.8 μm and a specific surface area of ​​3.2 m². 2 / g.

[0183] Example 5

[0184] (1) Preparation of slurry

[0185] (1.1) Preparation of polymer microsphere emulsion

[0186] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 80°C. 2.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.5 parts of ammonium persulfate by dry weight) were added. Then, 73.0 parts of styrene, 24.5 parts of ethyl acrylate, and 2.0 parts of boric acid were added to the reactor. The mixture was stirred at 600 rpm and added uniformly over 2 hours. After the addition was complete, the reaction continued for another 2 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 40% using deionized water.

[0187] The particle size D50 of the polymer microspheres was determined to be 0.51 μm using a laser particle size analyzer. After drying the polymer microspheres, they were sintered at 1200 °C under a nitrogen atmosphere for 2 hours, and the residual mass was 35.3%.

[0188] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0189] First, add 300 parts water and 0.2 parts carboxymethyl cellulose, and stir and beat at 600 rpm for 20 minutes. Then, add 50g of the above emulsion with a solid content of 40% (equivalent to 20 parts on dry weight) and 100 parts natural graphite (particle size D50 of 15μm), and stir and disperse at 600 rpm for 20 minutes to obtain a slurry with a solid content of 26.7%.

[0190] (2) Preparation of polymer-coated carbon materials

[0191] The above slurry was dried using a spray dryer with an inlet temperature of 300°C and an outlet temperature of 130°C to obtain a polymer-coated carbon material powder with a polymer coating on the surface of the carbon material.

[0192] (3) Preparation of modified carbon materials

[0193] The polymer-coated carbon material was heated to 450°C at a heating rate of 120°C / h under a nitrogen atmosphere and held at that temperature for 2 hours. Then, it was heated to 1300°C at a heating rate of 120°C / h and held for 3 hours. Next, it was heated to 3000°C at a heating rate of 120°C / h and held for 2 hours. Then, it was cooled naturally, discharged, and dispersed using a ball mill. The material was then passed through a 300-mesh sieve and demagnetized using a demagnetizer to obtain the modified carbon material.

[0194] The modified carbon material has a particle size of 17.5 μm and a specific surface area of ​​2.6 m². 2 / g.

[0195] Example 6

[0196] (1) Preparation of slurry

[0197] (1.1) Preparation of polymer microsphere emulsion

[0198] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 40.0 parts of styrene, 58.90 parts of ethyl acrylate, and 1.0 part of boric acid were added to the reactor. The mixture was stirred at 600 rpm and added uniformly over 2 hours. After the addition was complete, the reaction continued for 3 hours. The reaction was stopped by evacuating under a vacuum of -75 kPa for 1 hour and cooling to below 45°C. The emulsion was then passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0199] The particle size D50 of the polymer microspheres was determined to be 0.48 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 33.0%.

[0200] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0201] First, add 300 parts water and 0.1 parts carboxymethyl cellulose, and stir and beat at 400 rpm for 30 minutes. Then, add 30g of the above emulsion with a solid content of 35% (equivalent to 10.5 parts on dry weight) and 100 parts natural graphite (particle size D50 of 12μm), and stir and disperse at 400 rpm for 30 minutes to obtain a slurry with a solid content of 25.7%.

[0202] (2) Preparation of polymer-coated carbon materials

[0203] The above slurry was dried using a spray dryer with an inlet temperature of 260°C and an outlet temperature of 120°C to obtain a polymer-coated carbon material powder with a polymer coating layer on the surface of the carbon material.

[0204] (3) Preparation of modified carbon materials

[0205] The polymer-coated carbon material was heated to 400°C at a heating rate of 80°C / h under a nitrogen atmosphere and held at that temperature for 3 hours. Then, it was heated to 1100°C at a heating rate of 80°C / h and held for 6 hours. Next, it was heated to 2900°C at a heating rate of 80°C / h and held for 3 hours. Then, it was cooled naturally, discharged, and dispersed using a ball mill. The material was then passed through a 300-mesh sieve and demagnetized using a demagnetizer to obtain the modified carbon material.

[0206] The modified carbon material has a particle size of 13.4 μm and a specific surface area of ​​2.8 m². 2 / g.

[0207] Example 7

[0208] In step (1), in the preparation of the polymer microsphere emulsion (1.1), boron-containing compounds and water-soluble polymers are added as follows. Apart from this, the preparation steps and condition parameters of the remaining steps (1.2), (2), and (3) are basically the same as those in Example 4.

[0209] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 70°C. Then, 0.1 parts by weight of a 20% ammonium persulfate deionized water solution (equivalent to 0.02 parts of ammonium persulfate by dry weight) were added. Next, 10.0 parts of 2-methylstyrene, 89.28 parts of butyl acrylate, 0.2 parts of metaboric acid, and 0.5 parts of polyvinyl alcohol were added to the reactor. The mixture was stirred and mixed at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for 4 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 30% using deionized water.

[0210] The particle size D50 of the polymer microspheres was determined to be 0.21 μm using a laser particle size analyzer. After drying the polymer microspheres, they were sintered at 1200 °C under a nitrogen atmosphere for 2 hours, and the residual mass was 30.0%.

[0211] Example 8

[0212] As shown below, in the preparation of the polymer microsphere emulsion in step (1) (1.1), boron-containing compounds and water-soluble polymers are added. Apart from this, the preparation steps and condition parameters of the remaining steps (1.2), (2) and (3) are basically the same as those in Example 5.

[0213] (1.1) Preparation of polymer microsphere emulsion

[0214] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 80°C. 2.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.5 parts of ammonium persulfate by dry weight) were added. Then, 48.0 parts of 2-fluorostyrene, 24.5 parts of hexyl acrylate, 2.0 parts of boric acid, and 25.0 parts of polyacrylamide were added to the reactor. The mixture was stirred and mixed at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for another 2 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 40% using deionized water.

[0215] The particle size D50 of the polymer microspheres was determined to be 0.39 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 34.8%.

[0216] Example 9

[0217] As shown below, in the preparation of the polymer microsphere emulsion in step (1) (1.1), boron-containing compounds and water-soluble polymers are added. Apart from this, the preparation steps and condition parameters of the remaining steps (1.2), (2) and (3) are basically the same as those in Example 6.

[0218] (1.1) Preparation of polymer microsphere emulsion

[0219] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 35.0 parts of styrene, 53.90 parts of ethyl acrylate, 1.0 part of boric acid, and 10.0 parts of polyvinyl alcohol were added to the reactor. The mixture was stirred and mixed at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for 3 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0220] The particle size D50 of the polymer microspheres was determined to be 0.28 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 33.2%.

[0221] Comparative Example 1

[0222] In step (1), in the preparation of the polymer microsphere emulsion (1.1), the amount of acrylic hydrophobic monomer is lower than the preferred range of the present invention, and correspondingly the amount of styrene monomer is higher than the preferred range of the present invention. Apart from this, the preparation steps and condition parameters of the remaining steps (1.2), (2), and (3) are basically the same as those in Example 6.

[0223] (1.1) Preparation of polymer microsphere emulsion

[0224] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 90.0 parts of styrene, 8.90 parts of ethyl acrylate, and 1.0 part of boric acid were added to the reactor. The mixture was stirred at 600 rpm and added uniformly over 2 hours. After the addition was complete, the reaction continued for 3 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0225] The particle size D50 of the polymer microspheres was determined to be 0.60 μm using a laser particle size analyzer. After drying the polymer microspheres, they were sintered at 1200 °C under a nitrogen atmosphere for 2 hours, and the residual mass was 33.4%.

[0226] Comparative Example 2

[0227] In step (1), during the mixing and dispersion of carbon materials and emulsion in step (1), carboxymethyl cellulose is not added for stirring and gelling. Apart from this, the preparation steps and condition parameters of the remaining steps (1.1), (2), and (3) are basically the same as those in Example 6.

[0228] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0229] First, add 300 parts of water, then add 30g of the above emulsion with a solid content of 35% (equivalent to 10.5 parts on dry weight) and 100 parts of natural graphite (particle size D50 of 12μm), and stir and disperse at 400rpm for 30min to obtain a slurry with a solid content of 25.7%.

[0230] Comparative Example 3

[0231] In an argon atmosphere, 100 parts of natural graphite (particle size D50 of 12 μm) were added to 300 parts of a polystyrene dimethyl carbonate solution with a solid content of 3.5%. The mixture was stirred at 500 r / min for 30 min at 40 °C to obtain a slurry. The slurry was then spray-dried using a spray drying tower with an inlet temperature of 180 °C and an outlet temperature of 110 °C. The solvent was removed and the mixture was granulated to obtain polystyrene-coated carbon material powder with a polystyrene coating on the surface of the carbon material.

[0232] The polystyrene-coated carbon material was heated to 400°C at a heating rate of 80°C / h under a nitrogen atmosphere and then held at that temperature for 3 hours. Next, the temperature was increased to 1100°C at a heating rate of 80°C / h and held at that temperature for 6 hours. Then, the material was allowed to cool naturally. After discharge, the material was dispersed using a ball mill, passed through a 300-mesh sieve, and demagnetized using a demagnetizer to obtain the modified carbon material.

[0233] Comparative Example 4

[0234] In step (1), during the mixing and dispersion of carbon material and emulsion in step (1), 120g of the above emulsion with a solid content of 35% is added as follows. Apart from this, the preparation steps and condition parameters of the remaining steps (1.1), (2), and (3) are basically the same as those in Example 6.

[0235] (1.2) Mixing, stirring and dispersing of carbon materials and emulsion

[0236] First, add 300 parts water and 0.1 parts carboxymethyl cellulose, and stir and beat at 400 rpm for 30 minutes. Then, add 120 g of the above emulsion with a solid content of 35% (equivalent to 42 parts on dry weight) and 100 parts natural graphite (particle size D50 of 12 μm), and stir and disperse at 400 rpm for 30 minutes to obtain a slurry with a solid content of 32.1%.

[0237] Comparative Example 5

[0238] In the preparation of the modified carbon material in step (3), a one-step sintering is carried out as follows. Apart from this, the preparation steps and condition parameters of the remaining steps (1.1), (1.2) and (2) are basically the same as those in Example 6.

[0239] (3) Preparation of modified carbon materials

[0240] The polymer-coated carbon material was heated to 3000°C at a heating rate of 80°C / h under a nitrogen atmosphere, held at that temperature for 3 hours, and then allowed to cool naturally. After discharge, the material was dispersed using a ball mill, passed through a 300-mesh sieve, and demagnetized using a demagnetizer to obtain the modified carbon material.

[0241] Comparative Example 6

[0242] In step (1), in the preparation of the polymer microsphere emulsion (1.1), an excess of boron-containing compound is added as follows. Apart from this, the preparation steps and conditions of the remaining steps (1.2), (2), and (3) are basically the same as those in Example 6.

[0243] (1.1) Preparation of polymer microsphere emulsion

[0244] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 40.0 parts of styrene, 52.90 parts of ethyl acrylate, and 7.0 parts of boric acid were added to the reactor. The mixture was stirred at 600 rpm and added uniformly over 2 hours. After the addition was complete, the reaction continued for 3 hours. The reaction was stopped by evacuating under a vacuum of -75 kPa for 1 hour and cooling to below 45°C. The emulsion was then passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0245] The particle size D50 of the polymer microspheres was determined to be 0.51 μm using a laser particle size analyzer. After drying the polymer microspheres and sintering them at 1200 °C under a nitrogen atmosphere for 2 hours, the residual mass was 33.6%.

[0246] Comparative Example 7

[0247] In step (1), in the preparation of the polymer microsphere emulsion (1.1), an excess of water-soluble polymer is added as follows. Apart from this, the preparation steps and conditions of the remaining steps (1.2), (2), and (3) are basically the same as those in Example 6.

[0248] (1.1) Preparation of polymer microsphere emulsion

[0249] Based on a total dry weight of 100 parts, 100 parts of deionized water were added to the emulsion reactor, and the temperature was raised to 75°C. 0.5 parts by weight of a 20% ammonium persulfate deionized aqueous solution (equivalent to 0.1 parts of ammonium persulfate by dry weight) were added. Then, 20.0 parts of styrene, 38.90 parts of ethyl acrylate, 1.0 part of boric acid, and 40.0 parts of polyvinyl alcohol were added to the reactor. The mixture was stirred and mixed at 600 rpm over 2 hours at a uniform rate. After the addition was complete, the reaction continued for 3 hours. The mixture was then evacuated under a vacuum of -75 kPa for 1 hour, cooled to below 45°C, and the reaction was stopped. The emulsion was passed through a 100-mesh sieve to obtain a polymer microsphere emulsion. The solid content of the emulsion was adjusted to 35% using deionized water.

[0250] The particle size D50 of the polymer microspheres was determined to be 0.18 μm using a laser particle size analyzer. After drying the polymer microspheres, they were sintered at 1200 °C under a nitrogen atmosphere for 2 hours, and the residual mass was 32.5%.

[0251] The following section introduces the battery manufacturing and testing process.

[0252] <Preparation of Liquid Lithium-ion Batteries>

[0253] (1) Preparation of positive electrode sheet

[0254] A positive electrode slurry (70% solid content) is prepared by mixing lithium nickel cobalt manganese oxide (NCM811), conductive agent SuperP, carbon nanotubes, and binder polyvinylidene fluoride (PVDF) in a mass ratio of 97:1:0.5:1.5 with N-methylpyrrolidone (NMP). The slurry is coated on both sides of the current collector aluminum foil, dried at 100°C, and then cold-pressed at room temperature. After that, the edges are cut, the sheets are cut, and the sheets are slit. The tabs are then welded to form the positive electrode sheet.

[0255] (2) Preparation of negative electrode sheet

[0256] Under a nitrogen protective atmosphere, the solvent N-methylpyrrolidone (NMP) and the binder PVDF were stirred and mixed thoroughly. Then, the conductive agent SuperP was added and stirred and mixed thoroughly. Next, the modified carbon material prepared in the above examples or the corresponding material in the comparative examples were added and stirred thoroughly to prepare a negative electrode slurry (solid content of 50%). According to the dosage range of the negative electrode material composition of the present invention, the mass ratio of the modified carbon material prepared in the above examples or the corresponding material in the comparative examples, the conductive agent SuperP, and the binder PVDF is 97.5:1.0:1.5. The above negative electrode slurry was coated on both sides of the current collector copper foil, dried at 100°C, cold-pressed at room temperature, and then trimmed, cut, and slit, and the tabs were welded to form the negative electrode sheet.

[0257] (3) Assembly of lithium-ion batteries

[0258] Using a porous PE polymer film as a separator, the prepared positive electrode sheet, separator, negative electrode sheet, and separator are stacked sequentially, with the separator positioned between the positive and negative electrode sheets, and then wound to obtain a bare battery cell. The bare battery cell is placed in an aluminum-plastic shell package and subjected to a relative vacuum pressure of -0.95 × 10⁻⁶. 5 At Pa, the cells are dried at 100°C until the moisture content is below 100 ppm. The electrolyte, which consists of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (EC:EMC:DEC volume ratio = 1:1:1) and LiPF6 (concentration 1.0M), is then vacuum-sealed and left to stand to produce a soft-pack liquid lithium-ion battery.

[0259] <Testing Liquid Lithium-ion Batteries>

[0260] (1) First Coulomb efficiency test

[0261] The batteries prepared above were formed and capacity tested using a battery testing cabinet. The formation step consisted of charging at a constant current of 0.05C for 2.0 hours, followed by charging at a constant current of 0.15C for 2.5 hours. The capacity testing step consisted of charging at a constant current of 0.33C to 4.2V, then charging at a constant voltage of 4.2V to the cutoff current of 0.02C, and discharging at 0.33C to 2.5V. The sum of the above charging and discharging capacities were recorded as the first charging capacity and the first discharging capacity, and the first charging specific capacity, the first discharging specific capacity, and the first coulombic efficiency were calculated.

[0262] (2) Rate discharge performance test

[0263] At 25°C, the liquid battery, after being formed and tested for capacity, was charged to 4.2V at a constant current and voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 0.33C at 25°C, and the 0.33C discharge capacity was recorded. The battery was then allowed to rest for 5 minutes. The same process was repeated: charging to 4.2V at a constant current and voltage of 0.33C, with a cutoff current of 0.02C, and allowing to rest for 5 minutes. Finally, discharging to 2.5V at 3C, the 3C discharge capacity was recorded.

[0264] 3C discharge capacity retention rate (%) = 3C discharge capacity / 0.33C discharge capacity × 100%

[0265] (3) Room temperature cycling performance test

[0266] At 25°C, the liquid battery, after being formed and tested, was charged to 4.2V at a constant current and constant voltage of 0.5C, with a cutoff current of 0.02C, and allowed to rest for 5 minutes. Then, it was discharged to 2.5V at a constant current of 1C and allowed to rest for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was calculated using the following formula:

[0267] Capacity retention rate (%) after 500 cycles at room temperature = (Discharge capacity after 500 cycles / Discharge capacity after 1 cycle) × 100%.

[0268] (4) High-temperature cycling performance test

[0269] First, at 25℃, the liquid battery, after being formed and tested, was charged to 4.2V at a constant current and constant voltage of 0.33C, with a cutoff current of 0.02C. After resting for 5 minutes, it was discharged to 2.5V at 0.33C, and the initial discharge capacity was recorded. The battery was then placed in a 45℃ high-temperature chamber and charged to 4.2V at a constant current and constant voltage of 0.33C, rested for 5 minutes, discharged to 2.5V at 0.33C, and rested for 5 minutes. This cycle was repeated 500 times. The capacity retention rate after the 500th cycle was calculated using the following formula:

[0270] High-temperature capacity retention rate after 500 cycles (%) = (500th cycle discharge capacity / 1st cycle discharge capacity) × 100%.

[0271] Table 1. Performance data of electrode materials obtained from the examples and comparative examples.

[0272]

[0273]

[0274] As shown in Table 1, in Examples 1-3, the initial coulombic efficiency was above 93%, the 3C discharge capacity retention rate was above 92.9%, the capacity retention rate after 500 cycles at room temperature was above 92.0%, and the capacity retention rate after 500 cycles at high temperature was above 85.0%, achieving excellent initial efficiency, rate performance, and cycle performance. In Examples 4-6, the initial coulombic efficiency was above 95.3%, the 3C discharge capacity retention rate was above 95.2%, the capacity retention rate after 500 cycles at room temperature was above 94.0%, and the capacity retention rate after 500 cycles at high temperature was above 87.8%, achieving even better initial efficiency, rate performance, and cycle performance. In Examples 7-9, the initial coulombic efficiency was above 95.8%, the 3C discharge capacity retention rate was above 95.7%, the capacity retention rate after 500 cycles at room temperature was above 94.3%, and the capacity retention rate after 500 cycles at high temperature was above 88.3%, thus achieving superior initial efficiency, rate performance, and cycle performance.

[0275] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 1 shows that the rate performance and cycle performance deteriorated. The possible reason is that the contained acrylic hydrophobic monomers are too few, which is not conducive to the formation of microsphere structure. The excellent coating effect and microstructure effect of microspheres cannot be brought into play, resulting in poor coating effect and not conducive to significantly improving battery performance.

[0276] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 2 shows that the rate performance and cycle performance deteriorated. The possible reason is that carboxymethyl cellulose was not added for stirring and gelling during the mixing and dispersion of carbon materials and emulsion, which may have led to poor dispersibility and stability of the slurry, which is not conducive to the uniform coating of carbon materials by polymer microspheres, thus affecting the rate performance and cycle performance.

[0277] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 3 shows that the technical route of the existing pitch-coated graphite material is completely different from that of the polymer microsphere emulsion-coated graphite material of the present invention. It cannot obtain the excellent coating effect and spatial effect of the emulsion microspheres of the present invention, nor does it have the boron doping effect and graphitization promotion effect. Therefore, it does not have the excellent modification effect of the present invention.

[0278] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 4 shows that the rate performance and cycle performance deteriorated. The possible reason is that during the mixing and dispersion of carbon materials and emulsion, the amount of emulsion added was too large, and the dry weight of the emulsion microspheres relative to the mass of carbon materials was too large, resulting in an excessively thick coating layer on the carbon materials. This may easily generate fine carbon powder, leading to a large overall specific surface area of ​​the material, which makes it prone to side reactions and rapid capacity decay.

[0279] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 5 shows that the rate performance and cycle performance deteriorated significantly. The possible reason is that directly sintering at 3000 degrees Celsius for 12 hours in one step can easily lead to rapid decomposition of organic matter, which can easily generate gas and form a porous structure. This may result in uneven carbonization and a non-dense carbon layer, which is not conducive to the formation of the SEI film and the performance of the cycle performance.

[0280] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 6 shows that the rate performance and cycle performance deteriorated significantly. The possible reason is that excessive boron doping can easily cause instability in the slurry and result in a non-dense and uneven carbon coating structure, which may be detrimental to the formation and stability of the SEI film, easily causing side reactions and leading to a significant reduction in cycle performance.

[0281] As shown in Table 1, the analysis of the test results of Examples 1-9 and Comparative Example 7 shows that the rate performance and cycle performance are low. The possible reasons are that the amount of water-soluble polymer added is too large, which is not conducive to the formation of emulsion microspheres, or the microspheres are too small, which cannot give full play to the excellent coating effect and spatial structure effect of emulsion microspheres.

[0282] As can be seen from the above, the emulsion copolymerization composition with the unique formulation of this invention, followed by coating and carbonizing or graphitizing of carbon materials, can leverage the excellent coating performance and spatial encapsulation effect of emulsion microspheres, significantly improving the initial coulombic efficiency, rate cycle performance, and high and low temperature cycle performance of lithium-ion batteries. Furthermore, by adding a specific amount of boron-containing compound to the polymer microsphere emulsion preparation composition and leveraging the synergistic effect of the three-stage calcination process, graphitization is significantly promoted, thereby significantly improving capacity and initial efficiency, enhancing the lithium intercalation performance of carbon materials, and reducing internal resistance. Compared to existing technologies, this significantly improves rate performance and cycle performance, achieving unexpectedly significant results and demonstrating great application potential.

[0283] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. The specific examples used above to illustrate the present invention are only for the purpose of helping to understand the present invention and are not intended to limit the present invention. Those skilled in the art to which this invention pertains can make several simple deductions, modifications, substitutions, or combinations based on the concept of the present invention. These deductions, modifications, substitutions, or combinations also fall within the scope of the claims of the present invention.

Claims

1. A modified carbon material, characterized in that, The modified carbon material has a core-shell structure, with the core containing carbon material and the coating layer containing organic polymer pyrolytic carbon; wherein, the organic polymer pyrolytic carbon is obtained by carbonization treatment of polymer microspheres; The method for preparing the modified carbon material includes the following steps: (1) First add water and carboxymethyl cellulose, stir and gel, then add emulsion and carbon material, stir and disperse to obtain slurry; (2) The slurry is dried to obtain a polymer-coated carbon material with a polymer coating layer on the surface of the carbon material; (3) The polymer-coated carbon material is heated in an inert atmosphere to carbonize it, and then sieved to obtain the modified carbon material, wherein the heating method adopts a step heating method; In step (3), the polymer-coated carbon material is heated to 300-500°C at a heating rate of 60-120°C / h under an inert atmosphere, and then held at that temperature for 2-5 hours; then, it is heated to 800-2000°C at a heating rate of 60-120°C / h and held at that temperature for 3-10 hours; then, it is heated to 2500-3500°C at a heating rate of 60-120°C / h and held at that temperature for 1-5 hours; then, it is cooled naturally, and after discharge, it is broken up and sieved to obtain the modified carbon material. The emulsion is a polymer microsphere emulsion; the polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, boron-containing compounds, and an initiator using an emulsion polymerization method; the acrylic hydrophobic monomers comprise one or more of ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, and decyl (meth)acrylate; the boron-containing compound comprises one or more of boric acid, metaboric acid, tetraphenylboric acid, sodium borate, sodium metaborate, sodium tetraphenylborate, calcium borate, and boron oxide. Of which, based on 100 parts of the total dry weight of the composition, styrene monomers comprise 10-75 parts, acrylic hydrophobic monomers comprise 24-89 parts, boron-containing compounds comprise 0.1-5.0 parts, and initiators comprise 0.001-2.0 parts.

2. The modified carbon material according to claim 1, characterized in that, The polymer microspheres are prepared by copolymerization of a composition comprising styrene monomers, acrylic hydrophobic monomers, water-soluble polymers, boron-containing compounds, and initiators using an emulsion polymerization method. Of which, based on 100 parts of the total dry weight of the composition, styrene monomers comprise 10-48 parts, acrylic hydrophobic monomers comprise 24-89 parts, water-soluble polymers comprise 0.5-25.0 parts, boron-containing compounds comprise 0.1-5.0 parts, and initiators comprise 0.001-2.0 parts.

3. The modified carbon material according to claim 2, characterized in that, Based on 100 parts of the total dry weight of the composition, the amount of the acrylic hydrophobic monomer is 24.5-89.28 parts; And / or, the initiator is 0.02-0.5 parts.

4. The modified carbon material according to claim 2, characterized in that, Based on 100 parts of the total dry weight of the composition, the boron-containing compound comprises 0.2-2.0 parts.

5. The modified carbon material according to claim 2, characterized in that, The water-soluble polymer comprises one or more of chitosan, polyvinylpyrrolidone, polyvinyl alcohol, polyacrylamide, and polyacrylic acid.

6. The modified carbon material according to claim 1 or 2, characterized in that, The styrene monomers include one or more of styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2-fluorostyrene, 3-fluorostyrene, and 4-fluorostyrene. And / or, the initiator is a peroxide; And / or, the water mentioned in step (1) is pure water or deionized water; And / or, the carbon material mentioned in step (1) is one or more of natural graphite, artificial graphite, porous carbon, carbon fiber, hard carbon and soft carbon.

7. The modified carbon material according to claim 1 or 2, characterized in that, In step (1), the carbon material is one or more of graphite fiber, mesophase carbon microspheres, petroleum coke, organic polymer pyrolysis carbon, and carbon black.

8. The modified carbon material according to claim 1 or 2, characterized in that, In step (1), the carbon material is one or both of needle coke and resin carbon.

9. The modified carbon material according to any one of claims 1-5, characterized in that, The modified carbon material has a particle size D50 of 8~25μm and a specific surface area of ​​2.0~4.0m². 2 / g.

10. The modified carbon material according to claim 9, characterized in that, The modified carbon material has a particle size D50 of 10~20μm and / or a specific surface area of ​​2.5~3.5m². 2 / g.

11. The modified carbon material according to any one of claims 1-5, characterized in that, The percentage of the coating layer mass to the total mass of the modified carbon material is 0.1-10%.

12. A method for preparing a modified carbon material according to any one of claims 1-11, characterized in that, It includes the following steps: (1) First add water and carboxymethyl cellulose, stir and gel, then add emulsion and carbon material, stir and disperse to obtain slurry; (2) The slurry is dried to obtain a polymer-coated carbon material with a polymer coating layer on the surface of the carbon material; (3) The polymer-coated carbon material is heated in an inert atmosphere to carbonize it, and then sieved to obtain the modified carbon material, wherein the heating method adopts a step heating method.

13. The method for preparing the modified carbon material according to claim 12, characterized in that, In step (1), the stirring speed of the mixing and glue application is 200~600 rpm, and the mixing and glue application time is 20~60 min; And / or, the stirring speed for the stirring and dispersion is 200~600 rpm, and the stirring and dispersion time is 20~60 min; And / or, the solid content of the emulsion is 25-50%; And / or, the solid content of the slurry is 10-60%.

14. The method for preparing the modified carbon material according to claim 13, characterized in that, The solid content of the emulsion is 30-40%; And / or, the solid content of the slurry is 20-40%.

15. The method for preparing the modified carbon material according to claim 12, characterized in that, In step (1), the mass ratio of the carbon material to the carboxymethyl cellulose is 1:0.0005~0.002, or The mass ratio of the carbon material to the dry weight of the emulsion is 1:0.05~0.

30.

16. The method for preparing the modified carbon material according to claim 15, characterized in that, In step (1), the ratio of the mass of the carbon material to the dry weight of the emulsion is 1:0.05~0.

20.

17. The method for preparing the modified carbon material according to any one of claims 12-16, characterized in that, In step (2), the drying is carried out by spray drying, and the inlet temperature of the spray dryer is 150~400℃ and the outlet temperature is 70~150℃.

18. The method for preparing the modified carbon material according to claim 17, characterized in that, In step (2), the inlet temperature of the spray dryer is 200~300℃.

19. The method for preparing the modified carbon material according to claim 17, characterized in that, In step (2), the outlet temperature of the spray dryer is 90~130℃.

20. The method for preparing the modified carbon material according to any one of claims 12-16, characterized in that, In step (3), the polymer-coated carbon material is heated to 350-450°C at a heating rate of 60-120°C / h under an inert atmosphere, and then kept at that temperature for 2-5 hours. Next, the temperature is increased to 800-2000℃ at a heating rate of 60-120℃ / h, and held for 3-10 hours; Next, the temperature is increased to 2500-3500℃ at a heating rate of 60-120℃ / h and held for 1-5 hours; then it is cooled naturally, and after discharge, it is broken up and sieved to obtain modified carbon material.

21. The method for preparing the modified carbon material according to any one of claims 12-16, characterized in that, In step (3), the polymer-coated carbon material is heated to 300-500°C at a heating rate of 60-120°C / h under an inert atmosphere, and then kept at that temperature for 2-5 hours. Next, the temperature is increased to 800-1300℃ at a heating rate of 60-120℃ / h, and held for 3-10 hours. Next, the temperature is increased to 2500-3500℃ at a heating rate of 60-120℃ / h and held for 1-5 hours; then it is cooled naturally, and after discharge, it is broken up and sieved to obtain modified carbon material.

22. The method for preparing the modified carbon material according to any one of claims 12-16, characterized in that, In step (3), the polymer-coated carbon material is heated to 300-500°C at a heating rate of 60-120°C / h under an inert atmosphere, and then kept at that temperature for 2-5 hours. Next, the temperature is increased to 1000-1200℃ at a heating rate of 60-120℃ / h, and held for 3-10 hours; Next, the temperature is increased to 2500-3500℃ at a heating rate of 60-120℃ / h and held for 1-5 hours; then it is cooled naturally, and after discharge, it is broken up and sieved to obtain modified carbon material.

23. A negative electrode material composition, characterized in that, It contains the modified carbon material according to any one of claims 1-11 or the modified carbon material prepared by the method of preparing the modified carbon material according to any one of claims 12-22; The composition comprises, by dry weight, 100% of the total mass of the negative electrode material composition, 95.0-98.0% of the modified carbon material, 0.5-2.0% of the conductive agent, and 1.0-3.0% of the binder.

24. A lithium-ion battery, characterized in that, It contains the negative electrode material composition as described in claim 23.

Citation Information

Patent Citations

  • Lithium ion battery cathode composite material and preparation method thereof

    CN101916846B

  • Negative electrode material and preparation method thereof, battery negative electrode and lithium ion battery

    CN113422030A

  • Modified natural graphite material used in lithium ion battery negative electrodes, and preparation method thereof

    CN102231434A

  • High-molecular polymer composite coating material as well as preparation method and application thereof

    CN114874576A