Preparation method and application of material for multifunctional interlayer and high-catalytic sulfur positive electrode of lithium-sulfur battery
By leveraging the synergistic effect of the lightweight, multifunctional intermediate layer material CBC@SnS-SnO and the highly efficient catalytic sulfur cathode material CBC@SnS-SnO/S, the volume expansion, polysulfide shuttle effect, and lithium dendrite problems of lithium-sulfur batteries are solved, achieving high capacity density and long-term stability, thus improving the performance of lithium-sulfur batteries.
Patent Information
- Application Number
- CN202310748283.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-25
AI Technical Summary
In practical applications, lithium-sulfur batteries suffer from problems such as severe volume expansion of the sulfur cathode, insulation and shuttle effect of polysulfides, and corrosion of the lithium anode, resulting in poor battery performance and safety hazards. Existing modification strategies cannot simultaneously solve the defects of the positive and negative electrodes, hindering their stable operation under high current density and high-capacity charge and discharge.
By leveraging the synergistic effect of lightweight, multifunctional intermediate layer material CBC@SnS-SnO and highly efficient catalytic sulfur cathode material CBC@SnS-SnO/S, polysulfides are adsorbed through a 3D interconnected porous network structure, providing active sites for catalytic conversion, inhibiting lithium dendrite formation, achieving uniform lithium deposition, and improving redox reaction kinetics.
At a high current density of 4C, the lithium-sulfur battery exhibits a high discharge specific capacity of 705.5 mAh g⁻¹, good long-term cycle stability, significantly improved battery capacity density and safety, and solved many defects of lithium-sulfur batteries.
Smart Images

Figure CN116995201B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-sulfur battery technology. It relates to a strategy for using a multifunctional interlayer material and a modified cathode material in lithium-sulfur batteries, and to methods for preparing and applying the lithium-sulfur battery interlayer material and sulfur cathode material. Specifically, it relates to methods for preparing and applying materials that can be used simultaneously as a multifunctional interlayer and a highly catalytic sulfur cathode in lithium-sulfur batteries. Background Technology
[0002] As market demands for portable electronic devices and electric vehicles increase, the relatively low energy density of lithium-ion batteries can no longer meet energy storage requirements, necessitating the development of energy storage devices with higher energy density. These devices possess a high theoretical specific capacity (~1675 mAh g⁻¹). -1 ) and high energy density (~2600Wh kg) -1 Lithium-sulfur batteries (LSBs) are considered one of the viable alternatives to LIBs [1,2]. However, LSBs have failed to be widely adopted in practical applications mainly due to several significant drawbacks: severe volume expansion of the sulfur cathode during cycling, the insulating properties of sulfur and polysulfides, the shuttle effect of soluble long-chain lithium polysulfides (LiPoS), and severe corrosion of the lithium anode. These drawbacks result in poor rate performance, rapid capacity decay, and serious safety issues [3,4].
[0003] To address these issues, extensive research has focused on modifying cathode materials. Among these, carbon composite metal oxides or metal sulfides have demonstrated excellent performance as sulfur cathode materials. The carbon component exhibits good conductivity and mechanical flexibility [5,6], while metal oxides play a significant role in adsorbing polysulfides and suppressing the shuttle effect [7]. Metal sulfides, on the other hand, play an important role in catalyzing sulfur conversion, accelerating redox kinetics, and improving cathode sulfur utilization [8]. Studies have found that improving the rapid electrocatalytic ability of polysulfides after adsorption is a necessary condition for achieving high-performance sulfur cathodes. Therefore, designing carbon composite metal oxide and metal sulfide cathode materials that can provide a large number of active sites and improving the redox kinetics of the sulfur cathode substrate under high sulfur loading conditions is crucial.
[0004] In addition to cathode materials that enable efficient catalytic sulfur conversion, introducing interlayer materials into LSBs can effectively block and convert polysulfides dissolved in the electrolyte, thus mitigating the shuttle effect of polysulfides [9]. On the other hand, the interlayer can play a role in uniform lithium ion migration, thereby mitigating anodic corrosion and inhibiting the formation of lithium dendrites by reducing uneven lithium deposition
[10] . To achieve the above outstanding functions, the interlayer needs to have excellent electrolyte wettability, excellent polysulfide adsorption capacity, and high catalytic activity to accelerate the conversion of lithium polysulfides.
[0005] In summary, while modifying the cathode material or introducing an intermediate layer can alleviate some performance defects in lithium-sulfur batteries, it cannot solve all the problems existing at both ends of the positive and negative electrodes. This seriously hinders the practical application and industrialization of lithium-sulfur batteries. Numerous research results on modified cathode materials or intermediate layers have been reported, but few systematic designs can simultaneously alleviate all defects in both the positive and negative electrodes of lithium-sulfur batteries, resulting in the inability of lithium-sulfur batteries to operate stably at high current densities and provide large charge-discharge capacities [5-10]. Therefore, designing an efficient strategy that can simultaneously cover all performance optimizations of lithium-sulfur batteries remains an urgent problem to be solved.
[0006] References:
[0007] [1]ZWSeh,Y.Sun,Q.Zhang,Y.Cui,Designing high-energy lithium-sulfurbatteries.Chem.Soc.Rev.45(2016)5605-5634.
[0008] [2]A.Manthiram,Y.Fu,SHChung,C.Zu,YSSu,Rechargeable lithium-sulfurbatteries.Chem.Rev.114(2014)11751-87.
[0009] [3]M.Zhao,BQLi,HJPeng,H.Yuan,JYWei,JQHuang,Lithium-sulfurbatteries under lean electrolyte conditions:Challenges and opportunities.Angew.Chem.Int.Ed.Engl.59(2020)12636-12652.
[0010] [4]G.Li,S.Wang,Y.Zhang,M.Li,Z.Chen,J.Lu,Revisiting the role ofpolysulfides in lithium-sulfur batteries.Adv.Mater.30(2018)e1705590.
[0011] [5]J.E.Knoop,S.Ahn,Recent advances in nanomaterials for high-performance lithium-sulfur batteries.J.Energy Chem.47(2020)86-106.
[0012] [6]W.Chen,H.Yu,S.Y.Lee,T.Wei,J.Li,Z.Fan,Nanocellulose:A promisingnanomaterial for advanced electrochemical energy storage.Chem.Soc.Rev.47(2018)2837-2872.
[0013] [7]X.Liu,J.Q.Huang,Q.Zhang,L.Mai,Nanostructured metal oxides andsulfides for lithium-sulfur batteries.Adv.Mater.29(2017)1601759.
[0014] [8]S.Cheng,X.Xia,H.Liu,Y.Chen,Core-shell structured MoS2@S sphericalcathode with improved electrochemical performance for lithium-sulfur batteries.J.Mater.Sci.Technol.34(2018)1912-1918.
[0015] [9]L.Fan,M.Li,X.Li,W.Xiao,Z.Chen,J.Lu,Interlayer material selectionfor lithium-sulfur batteries.Joule 3(2019)361-386.
[0016]
[10] D. Zhu, T. Long, B. Xu, Y. Zhao, H. Hong, R. Liu, F. Meng, J. Liu, Recent advances in interlayer and separator engineering for lithium-sulfurbatteries. J. Energy Chem. 57 (2021) 41-60. Summary of the Invention
[0017] To address the current obstacles hindering the practical application and industrialization of lithium-sulfur batteries, this invention provides a simple and low-cost modification method for preparing an intermediate layer material and a sulfur cathode material for lithium-sulfur batteries. Their combined application in lithium-sulfur batteries can simultaneously resolve the aforementioned defects in both the positive and negative electrodes. Specifically, through the synergistic effect of the lightweight, multifunctional intermediate layer and the highly efficient catalytic sulfur cathode material, the low sulfur utilization rate of both electrodes and the surface corrosion of the lithium cathode can be alleviated simultaneously, increasing the battery's capacity density, significantly reducing the shuttle effect of polysulfides, and resolving the safety hazards caused by sulfur expansion and lithium dendrite formation during long-term operation. Lithium-sulfur batteries equipped with the intermediate layer and cathode material provided by this invention still exhibit a current density of 705.5 mA hg under long-term cycling at a high current density of 4C. -1 Its discharge specific capacity exceeds that of most research inventions reported to date.
[0018] The technical solution of the present invention is as follows:
[0019] A method for preparing a material that can be used as both a multifunctional intermediate layer and a highly catalytic sulfur cathode in lithium-sulfur batteries includes the following steps:
[0020] Step 1: Synthesis of bacterial cellulose (BC) aerogel: Anhydrous glucose, yeast extract, lactopeptone and sodium dihydrogen phosphate were dissolved and stirred in ultrapure water, and BC hydrogel was cultured using Acetobacter xylinum strain; the BC hydrogel was purified with sodium hydroxide solution and then repeatedly washed with ultrapure water until the washing solution was neutral, and then the washed BC was placed in a freezer to freeze, and then dried in a freeze dryer to generate BC aerogel.
[0021] Step 2: Preparation of carbonized bacterial cellulose (CBC): BC aerogel is carbonized in a quartz tube furnace to obtain CBC;
[0022] Step 3: Preparation of tin ion solution: Dissolve tin tetrachloride pentahydrate and thiourea in isopropanol;
[0023] Step 4: Synthesis of CBC@SnS-SnO interlayer material: The tin ion solution prepared in Step 3 and the CBC prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave and placed in an oven for reaction. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution was transparent. Then, the product was frozen in a freezer and dried in a freeze dryer to obtain the CBC@SnS-SnO interlayer material.
[0024] Step 5: Preparation of CBC@SnS-SnO powder material: Grind the CBC@SnS-SnO intermediate layer material obtained in Step 4 into powder and sieve it;
[0025] Step 6: Synthesis of CBC@SnS-SnO / S cathode material: The CBC@SnS-SnO powder material obtained in step 5 is mixed with sulfur, and sulfur is loaded in a quartz tube furnace to obtain CBC@SnS-SnO / S cathode material;
[0026] In step one, the ratio of anhydrous glucose: yeast extract: lactopeptone: sodium dihydrogen phosphate: ultrapure water is 10:3:4:4:200 (mass ratio). The culture time of Acetobacter xylinum strain in BC hydrogel is 12-36h, preferably 24h; the concentration of sodium hydroxide solution is 1-3wt%, preferably 2wt%; and the passivation time is 3-9h, preferably 6h.
[0027] In step two, the diameter of the BC aerogel ranges from 1.5 to 2.5 cm, preferably 2 cm; the thickness is 0.2 to 0.6 mm, preferably 0.4 mm. The carbonization temperature in the quartz tube furnace is in the range of 500 to 900 °C, preferably 700 °C; the holding time is in the range of 1 to 3 hours, preferably 2 hours.
[0028] In step three, the mass concentration of added tin tetrachloride pentahydrate is 0.02-0.2 mol / L. -1 Within the range, 0.12 mol L is preferred. -1 The molar ratio of tin tetrachloride pentahydrate to thiourea is selected to be in the range of 1-16:2, preferably 2:1.
[0029] In step four, the mass ratio of CBC to tin tetrachloride pentahydrate in step three is 1:5-50, preferably 1:30; the oven heating temperature is in the range of 120-200℃, preferably 160℃; and the heat preservation time is in the range of 6-18h, preferably 12h.
[0030] In step six, the molar ratio of CBC@SnS-SnO powder material to sulfur is 1:3-4, preferably 1:3.5; the sulfur loading time in the tube furnace is 12-36h, preferably 24h.
[0031] The prepared lightweight multifunctional intermediate layer material and highly efficient catalytic sulfur cathode material are applied to battery assembly. The obtained sulfur cathode material is coated with Super P and PVDF on aluminum foil, cut into circular cathode electrode sheets, and used to assemble button batteries with the prepared intermediate layer material, separator and lithium sheet.
[0032] Compared with the prior art, the beneficial effects of the present invention are:
[0033] CBCs with a 3D interconnected porous network structure can adapt to the huge volume changes during the conversion of elemental sulfur, provide physical adsorption to suppress the shuttle effect, and accelerate lithium-ion diffusion during cycling.
[0034] In terms of cathode materials, a large number of SnS-SnO heterostructures are densely loaded within the CBC network to form the sulfur-containing cathode host material CBC@SnS-SnO, providing abundant active sites for catalyzing the conversion of sulfur and polysulfides. It can also be used for Li... + Electrons provide shorter diffusion paths, significantly enhancing redox reaction kinetics.
[0035] In the intermediate layer, CBC@SnS-SnO can rapidly capture soluble lithium polysulfides and accelerate their catalytic conversion through strong adsorption, achieving rapid regulation of the lithium polysulfide capture and conversion process. Furthermore, CBC@SnS-SnO can promote uniform lithium deposition, inhibit lithium dendrite formation, and improve the stability of SEI formation.
[0036] This invention leverages the advantages of the aforementioned CBC@SnS-SnO / S cathode material and CBC@SnS-SnO interlayer material to form a hierarchical functionalization strategy for the stepwise catalysis-adsorption-conversion of sulfur compounds. This effectively improves the reversible specific capacity, high sulfur mass loading, and excellent long-term cycling stability and ultra-low capacity decay of LSBs. A lithium-sulfur battery equipped with the CBC@SnS-SnO interlayer and CBC@SnS-SnO / S cathode material still exhibits a capacity of 705.5 mAh g / L after 250 cycles at a high current density of 4C. -1 Its high discharge specific capacity surpasses most previously reported research findings. This novel strategy also provides inspiration for the rational design of other emerging energy storage applications.
[0037] A literature search revealed that the preparation method of the multifunctional intermediate layer and highly efficient catalytic sulfur cathode material proposed in this invention, which can be applied to lithium-sulfur batteries, has not been publicly reported. Attached Figure Description
[0038] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0039] Figure 1 These are XRD patterns of the lithium-sulfur battery cathode material and intermediate layer material prepared in Example 1 of this invention;
[0040] Figure 2 These are SEM images of the lithium-sulfur battery cathode material and intermediate layer material prepared in Example 1 of this invention;
[0041] Figure 3 These are TEM images of the lithium-sulfur battery cathode material and intermediate layer material prepared in Example 1 of this invention;
[0042] Figure 4 This is a comparison of the rate performance test data of a lithium-sulfur battery assembled from the positive electrode material and intermediate layer material prepared in Example 1 of this invention.
[0043] Figure 5 This is a comparison of the cycle performance test data of a lithium-sulfur battery assembled from the positive electrode body material and intermediate layer material prepared in Example 1 of this invention.
[0044] Figure 6 This is a SEM image of the sulfur positive electrode and lithium negative electrode after testing of a lithium-sulfur battery assembled from the positive electrode body material and intermediate layer material prepared in Example 1 of this invention.
[0045] Figure 7 These are SEM images of the CBC@SnS-SnO / S cathode material and lithium anode electrode sheet after cycle testing. Detailed Implementation
[0046] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The embodiments given are only for explaining the present invention and are not intended to limit the scope of the invention. Unless otherwise defined, all technical and scientific terms used herein have the meaning commonly understood by one of ordinary skill in the art.
[0047] This invention proposes a strategy of jointly applying a multifunctional interlayer material and a modified cathode material in lithium-sulfur batteries, and provides a highly efficient catalytic sulfur cathode material and a lightweight multifunctional interlayer material, the preparation method of which includes the following steps:
[0048] Step 1: Synthesis of bacterial cellulose (BC) aerogel: Anhydrous glucose, yeast extract, lactopeptone, and sodium dihydrogen phosphate were dissolved and stirred in ultrapure water, and BC hydrogel was cultured using Acetobacter xylinum strain; the BC hydrogel was purified with sodium hydroxide solution and then repeatedly washed with ultrapure water until the washing solution was neutral, and then the washed BC was placed in a freezer to freeze, and then dried in a freeze dryer to generate BC aerogel;
[0049] Step 2: Preparation of carbonized bacterial cellulose (CBC): BC aerogel is carbonized in a quartz tube furnace to obtain CBC;
[0050] Step 3: Preparation of tin ion solution: Dissolve tin tetrachloride pentahydrate and thiourea in isopropanol;
[0051] Step 4: Synthesis of CBC@SnS-SnO interlayer material: The tin ion solution prepared in Step 3 and the CBC prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave and placed in an oven for reaction. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution was transparent. Then, the product was frozen in a freezer and dried in a freeze dryer to obtain the CBC@SnS-SnO interlayer material.
[0052] Step 5: Preparation of CBC@SnS-SnO powder material: Grind the CBC@SnS-SnO intermediate layer material obtained in Step 4 into powder and sieve it;
[0053] Step 6: Synthesis of CBC@SnS-SnO / S cathode material: The CBC@SnS-SnO powder material obtained in step 5 is mixed with sulfur, and sulfur is loaded in a quartz tube furnace to obtain CBC@SnS-SnO / S cathode material.
[0054] The preparation methods for the intermediate layer material CBC@SnS-SnO and the sulfur cathode material CBC@SnS-SnO / S described in this embodiment employ a static culture method, a solvothermal method, and a one-step carbonization annealing method. The process is simple, the reaction conditions are mild, the raw material costs are low, and it is environmentally friendly and pollution-free. Using CBC@SnS-SnO / S and CBC@SnS-SnO materials in lithium-sulfur batteries establishes a hierarchical functionalization strategy for the stepwise catalysis-adsorption-conversion of sulfur substances. This can increase the loading of the sulfur cathode, promote uniform lithium deposition, inhibit lithium dendrite formation, and improve the stability of SEI formation. It effectively improves the reversible specific capacity of LSBs, exhibiting long-term cycle stability and ultra-low capacity decay.
[0055] Specifically, in step one above, the ratio of anhydrous glucose: yeast extract: milk peptone: sodium dihydrogen phosphate: ultrapure water is 10:3:4:4:200 (mass ratio); the culture time of Acetobacter xylinum strain in BC hydrogel is 12-36h, preferably 24h; the concentration of sodium hydroxide solution is 1-3wt%, preferably 2wt%; and the passivation time is 3-9h, preferably 6h.
[0056] Specifically, in step two above, the diameter of the BC aerogel is 1.5-2.5cm, preferably 2cm; the thickness is 0.2-0.6mm, preferably 0.4mm; the carbonization temperature in the quartz tube furnace is in the range of 500-900℃, preferably 700℃; and the heat preservation time is in the range of 1-3h, preferably 2h.
[0057] Specifically, in step three above, the mass concentration of the added tin tetrachloride pentahydrate is between 0.02 and 0.2 mol / L. -1 Within the range, 0.12 mol L is preferred. -1 The molar ratio of tin tetrachloride pentahydrate to thiourea is selected to be in the range of 1-16:2, preferably 2:1.
[0058] Specifically, in step four above, the mass ratio of CBC to tin tetrachloride pentahydrate in step three is 1:5-50, preferably 1:30; the oven heating temperature is in the range of 120-200℃, preferably 160℃; and the heat preservation time is in the range of 6-18h, preferably 12h.
[0059] Specifically, in step six above, the ratio of the CBC@SnS-SnO powder material to sulfur is in the range of 1:3-4, preferably 1:3.5. The sulfur loading time in the tube furnace is in the range of 12-36 hours, preferably 24 hours.
[0060] Based on the above embodiments, the present invention provides specific examples of the CBC@SnS-SnO interlayer material and the CBC@SnS-SnO / S sulfur cathode material and their preparation methods.
[0061] Example 1:
[0062] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain. Incubate the solution at 30℃ for 24h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 2wt% sodium hydroxide solution for 6h, then repeatedly wash the BC hydrogel with ultrapure water until the pH of the washing solution reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0063] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0064] Step 3: Preparation of tin ion solution. 21.02 g of tin tetrachloride pentahydrate and 2.29 g of thiourea were dissolved in 500 mL of isopropanol at a molar ratio of 2:1 and stirred for 20 min to obtain 0.12 mol / L tin ion solution. -1 A clear solution of tin ions.
[0065] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated in an oven at 160℃ for 12h. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24h to obtain the CBC@SnS-SnO interlayer material.
[0066] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0067] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. 100 mg of CBC@SnS-SnO powder obtained in Step Five was mixed with 350 mg of elemental sulfur at a molar ratio of 1:3.5. The mixture was then placed in a quartz tube furnace and kept at 155 °C for 24 h to obtain the CBC@SnS-SnO / S cathode material.
[0068] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 hours. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60°C for 16 hours, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a 25°C incubator for 12 hours before electrochemical testing.
[0069] Taking the CBC@SnS-SnO interlayer material and sulfur cathode host material prepared in Example 1 as examples, X-ray diffraction analysis was performed, as follows: Figure 1As shown, the X-ray diffraction (XRD) pattern of CBC@SnS-SnO exhibits distinct SnS diffraction peaks (JCPDS: 75-0325) and SnO diffraction peaks (JCPDS: 72-1012), indicating that the material has a stable crystal structure and high product purity. The absence of carbon peaks suggests that CBC exists in the form of amorphous carbon.
[0070] like Figure 2 As shown, scanning electron microscopy (SEM) imaging of CBC@SnS-SnO clearly reveals that nanoscale particles are uniformly loaded onto the microfiber network of CBC. Combined with... Figure 3 Transmission electron microscopy (TEM) imaging confirmed that the nanoparticles were SnS-SnO heterojunction nanoparticles, and also verified the amorphous state of CBC and the uniform distribution of SnS-SnO nanoparticles on the fiber network.
[0071] like Figure 4 The image shows the galvanostatic charge-discharge (GCD) test data of a lithium-sulfur battery equipped with a CBC@SnS-SnO interlayer and a CBC@SnS-SnO / S cathode material at different currents (0.5C, 1C, 2C, 3C, 4C, 5C), exhibiting a charge-discharge rate of 1580.4 mA hg. -1 1297.8mA hg -1 1194.3mA hg -1 991.3mA hg -1 795.5mA hg -1 596.9mA hg -1 Its high discharge specific capacity reflects its excellent rate capability.
[0072] like Figure 5 The figure shows the cycle test data of a lithium-sulfur battery equipped with a CBC@SnS-SnO interlayer and a CBC@SnS-SnO / S cathode material at a 2C current density. Even after 300 cycles at a high current density of 2C, it still exhibits a current rating of 815.5 mA hg. -1 The discharge specific capacity was higher than that of the standard battery, while the comparison battery without the CBC@SnS-SnO interlayer and CBC@SnS-SnO / S cathode material only showed 681.9 mA hg. -1 and 400.8mA hg -1 The specific discharge capacity. For example... Figure 6 As shown, after 250 cycles at a high current density of 4C, the lithium-sulfur battery equipped with a CBC@SnS-SnO interlayer and a CBC@SnS-SnO / S cathode material still exhibits a current density of 705.5 mA hg. -1Its discharge specific capacity exceeds that of most currently reported lithium-sulfur battery studies, indicating that the battery can maintain excellent charge-discharge performance even under high current.
[0073] Combination Figure 7 SEM results of the CBC@SnS-SnO / S cathode material and lithium anode sheet after cycle testing revealed that the three-dimensional network structure of CBC@SnS-SnO still exists, and sulfur particles are uniformly distributed on the fiber surface, indicating the high stability and excellent catalytic ability of CBC@SnS-SnO. The almost absence of lithium dendrites on the lithium electrode sheet indicates that the CBC@SnS-SnO interlayer plays a role in inducing uniform lithium ion deposition and avoiding the formation of lithium dendrites. At the same time, the absence of obvious polysulfides indicates that the presence of the interlayer enables the capture and conversion of polysulfides, effectively mitigating the effects of the shuttle effect. This provides high charge and discharge specific capacity while extending the service life of the lithium-sulfur battery.
[0074] Example 2:
[0075] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain. Incubate the solution at 30℃ for 24h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 2wt% sodium hydroxide solution for 6h, then repeatedly wash the BC hydrogel with ultrapure water until the pH of the washing solution reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0076] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0077] Step 3: Preparation of tin ion solution. Dissolve 3.506 g of tin tetrachloride pentahydrate and 0.76 g of thiourea in 500 mL of isopropanol at a molar ratio of 2:1 and stir for 20 min to obtain 0.02 mol / L tin ion solution. -1 A clear solution of tin ions.
[0078] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated in an oven at 200°C for 24 hours. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24 hours to obtain the CBC@SnS-SnO interlayer material.
[0079] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0080] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. The CBC@SnS-SnO powder material obtained in Step Five was mixed with elemental sulfur at a molar ratio of 1:4. The mixture was then placed in a quartz tube furnace and kept at 155°C for 36 hours to obtain the CBC@SnS-SnO / S cathode material.
[0081] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 h. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60 °C for 16 h, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm for later use. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a constant temperature oven at 25 °C for 36 h before electrochemical testing. It exhibits 628.3 mA hg after 250 cycles at a high current density of 4C. -1 The specific discharge capacity.
[0082] Example 3:
[0083] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain. Incubate the solution at 30℃ for 12h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 1wt% sodium hydroxide solution for 3h, then repeatedly wash the BC hydrogel with ultrapure water until the washing solution pH reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0084] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0085] Step 3: Preparation of tin ion solution. Dissolve 10.52 g of tin tetrachloride pentahydrate and 0.57 g of thiourea in 500 mL of isopropanol at a molar ratio of 4:1, and stir for 20 min to obtain 0.06 mol / L tin ion solution. -1 A clear solution of tin ions.
[0086] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated at 180°C for 18 hours in an oven. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24 hours to obtain the CBC@SnS-SnO interlayer material.
[0087] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0088] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. The CBC@SnS-SnO powder material obtained in Step Five is mixed with elemental sulfur at a molar ratio of 1:3. The mixture is then placed in a quartz tube furnace and kept at 155°C for 12 hours to obtain the CBC@SnS-SnO / S cathode material.
[0089] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 hours. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60°C for 16 hours, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a 25°C incubator for 12 hours before electrochemical testing. It exhibits 496.1 mA hg after 250 cycles at a high current density of 4C. -1 The specific discharge capacity.
[0090] Example 4:
[0091] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain. Incubate the solution at 30℃ for 12h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 1wt% sodium hydroxide solution for 3h, then repeatedly wash the BC hydrogel with ultrapure water until the pH of the washing solution reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0092] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0093] Step 3: Preparation of tin ion solution. Dissolve 17.53 g of tin tetrachloride pentahydrate and 0.63 g of thiourea in 500 mL of isopropanol at a molar ratio of 6:1 and stir for 20 min to obtain 0.1 mol / L tin ion solution. -1 A clear solution of tin ions.
[0094] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated in an oven at 200°C for 18 hours. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24 hours to obtain the CBC@SnS-SnO interlayer material.
[0095] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0096] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. The CBC@SnS-SnO powder material obtained in Step Five is mixed with elemental sulfur at a molar ratio of 1:3. The mixture is then placed in a quartz tube furnace and kept at 155°C for 24 hours to obtain the CBC@SnS-SnO / S cathode material.
[0097] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 hours. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60°C for 16 hours, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a 25°C incubator for 12 hours before electrochemical testing. It exhibits 320.6 mA hg after 250 cycles at a high current density of 4C. -1 The specific discharge capacity.
[0098] Example 5:
[0099] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain solution. Incubate the solution at 30℃ for 36h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 3wt% sodium hydroxide solution for 9h, then repeatedly wash the BC hydrogel with ultrapure water until the pH of the washing solution reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0100] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0101] Step 3: Preparation of tin ion solution. 28.05 g of tin tetrachloride pentahydrate and 0.76 g of thiourea were dissolved in 500 mL of isopropanol at a molar ratio of 8:1 and stirred for 20 min to obtain 0.16 mol / L tin ion solution. -1 A clear solution of tin ions.
[0102] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated in an oven at 200°C for 24 hours. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24 hours to obtain the CBC@SnS-SnO interlayer material.
[0103] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0104] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. The CBC@SnS-SnO powder material obtained in Step Five was mixed with elemental sulfur at a molar ratio of 1:4. The mixture was then placed in a quartz tube furnace and kept at 155°C for 24 hours to obtain the CBC@SnS-SnO / S cathode material.
[0105] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 hours. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60°C for 16 hours, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a 25°C incubator for 12 hours before electrochemical testing. It exhibits 422.8 mA hg after 250 cycles at a high current density of 4C. -1 The specific discharge capacity.
[0106] Example 6:
[0107] Step 1: Synthesis of BC aerogel. Dissolve 5g anhydrous glucose, 1.5g yeast extract, 2g peptone, and 2g sodium dihydrogen phosphate in 100mL of ultrapure water. Adjust the pH of the culture medium to 5 using 30% acetic acid, and sterilize at 115℃ for 30min. Then add 0.1mL of concentrated Acetobacter xylinum strain. Incubate the solution at 30℃ for 36h to obtain BC hydrogel. Purify the BC hydrogel by soaking in 2wt% sodium hydroxide solution for 6h, then repeatedly wash the BC hydrogel with ultrapure water until the pH of the washing solution reaches 7. Freeze the washed BC hydrogel in a freezer, and then freeze-dry it to generate BC aerogel.
[0108] Step 2: Preparation of carbonized bacterial cellulose (CBC). 200 mg of three-dimensional BC aerogel with a diameter of 2 cm and a thickness of 0.4 mm was carbonized in a quartz tube furnace at 700 °C to obtain CBC tablets.
[0109] Step 3: Preparation of tin ion solution. 35.06 g of tin tetrachloride pentahydrate and 15.22 g of thiourea were dissolved in 500 mL of isopropanol at a molar ratio of 1:2 and stirred for 20 min to obtain 0.2 mol / L tin ion solution. -1 A clear solution of tin ions.
[0110] Step 4: Synthesis of CBC@SnS-SnO composite material. The solution prepared in Step 3 and 0.7g of the CBC sheet prepared in Step 2 were transferred to a polytetrafluoroethylene-lined autoclave, and then heated in an oven at 140°C for 12 hours. After the autoclave cooled naturally to room temperature, the product was washed with deionized water and ethanol until the washing solution became transparent, and then freeze-dried for 24 hours to obtain the CBC@SnS-SnO interlayer material.
[0111] Step 5: Preparation of CBC@SnS-SnO powder material. Grind the above CBC@SnS-SnO intermediate layer material into powder, and refine the powder to pass through a 300-mesh sieve.
[0112] Step Six: Synthesis of CBC@SnS-SnO / S cathode material. The CBC@SnS-SnO powder material obtained in Step Five was mixed with elemental sulfur at a molar ratio of 1:3.5. The mixture was then placed in a quartz tube furnace and kept at 155°C for 12 hours to obtain the CBC@SnS-SnO / S cathode material.
[0113] The prepared lightweight multifunctional interlayer material and highly efficient catalytic sulfur cathode material were applied to battery assembly. 80 mg of the prepared CBC@SnS-SnO / S material was thoroughly ground with 10 mg of Super P and 10 mg of PVDF at a mass ratio of 8:1:1. NMP solution was then added and the mixture was continuously magnetically stirred for 8 hours. The uniformly dispersed, viscous slurry was coated onto aluminum foil, dried at 60°C for 16 hours, and cut into circular cathode electrode sheets with a diameter of approximately 12 mm. The prepared CBC@SnS-SnO interlayer, CBC@SnS-SnO / S cathode electrode sheets, Celgard 2400 separator, and lithium anode were then used to assemble a 2025 model button lithium-sulfur battery in a glove box. 15 μL of electrolyte was added to the positive electrode side and 10 μL to the negative electrode side. The assembled battery was then allowed to stand in a 25°C incubator for 12 hours before electrochemical testing. It exhibits 456.9 mA hg after 250 cycles at a high current density of 4C. -1 The specific discharge capacity.
[0114] The technical solutions disclosed and proposed in this invention can be implemented by those skilled in the art by appropriately modifying the conditions and routes, etc. Although the methods and preparation techniques of this invention have been described through preferred embodiments, those skilled in the art can obviously modify or recombine the methods and technical routes described herein without departing from the content, spirit, and scope of this invention to achieve the final preparation technique. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included within the spirit, scope, and content of this invention.
Claims
1. A method for preparing a material that can be used simultaneously as a multifunctional intermediate layer and a highly catalytic sulfur cathode in lithium-sulfur batteries, characterized in that, Includes the following steps: Step 1: Synthesis of bacterial cellulose aerogel: Anhydrous glucose, yeast extract, lactopeptone and sodium dihydrogen phosphate were dissolved and stirred in ultrapure water, and BC hydrogel was cultured using Acetobacter xylinum strain; the BC hydrogel was purified with sodium hydroxide solution and then repeatedly washed with ultrapure water until the washing solution was neutral, and then the washed BC was placed in a freezer to freeze, and then dried in a freeze dryer to generate BC aerogel; Step 2: Preparation of carbonized bacterial cellulose: BC aerogel is carbonized in a quartz tube furnace to obtain bacterial cellulose CBC; Step 3: Preparation of tin ion solution: Dissolve tin tetrachloride pentahydrate and thiourea in isopropanol to prepare a tin ion solution; Step 4: Synthesis of CBC@SnS-SnO interlayer material: The tin ion solution prepared in Step 3 and the CBC prepared in Step 2 are transferred to a polytetrafluoroethylene-lined autoclave and placed in an oven for reaction; after the autoclave cools naturally to room temperature, the product is washed with deionized water and ethanol until the washing solution is transparent, and then the product is frozen in a freezer and dried in a freeze dryer to obtain the CBC@SnS-SnO interlayer material; Step 5: Preparation of CBC@SnS-SnO powder material: Grind the CBC@SnS-SnO intermediate layer material obtained in Step 4 into powder and sieve it; Step 6: Synthesis of CBC@SnS-SnO / S cathode material: The CBC@SnS-SnO powder material obtained in step 5 is mixed with sulfur, and sulfur is loaded in a quartz tube furnace to obtain CBC@SnS-SnO / S cathode material.
2. The preparation method according to claim 1, characterized in that, In step one, the mass ratio of anhydrous glucose: yeast extract: peptone: sodium dihydrogen phosphate: ultrapure water is 10:3:4:4:
200. The culture time of Acetobacter xylinum strain in BC hydrogel is 12-36h, the concentration of sodium hydroxide solution is 1-3wt%, and the purification time is 3-9h.
3. The preparation method according to claim 1, characterized in that, In step two, the diameter of the BC aerogel ranges from 1.5 to 2.5 cm, and the thickness is 0.2 to 0.6 mm; the carbonization temperature is 500 to 900 ℃, and the holding time is 1 to 3 hours.
4. The preparation method according to claim 1, characterized in that, In step three, tin tetrachloride pentahydrate is added at a mass concentration of 0.02-0.2 mol / L. -1 The molar ratio of tin tetrachloride pentahydrate and thiourea was selected as 1-16:
2.
5. The preparation method according to claim 1, characterized in that, In step four, the mass ratio of CBC to tin tetrachloride pentahydrate in step three is 1:5-50, the oven heating temperature is in the range of 120-200℃, and the reaction time is in the range of 6-24h.
6. The preparation method according to claim 1, characterized in that, In step six, the molar ratio of CBC@SnS-SnO powder material to sulfur is 1:3-4; the sulfur loading time in the tube furnace is 12-36 hours.
7. The lightweight, multifunctional interlayer material and the highly efficient catalytic sulfur cathode material prepared by the method of claim 1 are applied to battery assembly, characterized in that, The obtained sulfur cathode material was coated with Super P and PVDF on aluminum foil, cut into circular cathode electrode sheets, and used to assemble button batteries with the prepared intermediate layer material, separator and lithium sheet.
Citation Information
Patent Citations
Tin sulfide / nitrogen-doped carbonized bacterial cellulose negative electrode material for lithium-ion batteries and preparation method thereof
CN107317001A
Preparation method of tin dioxide@oxidized bacterial cellulose / reduced graphene oxide electrode material
CN112768655A