氯化钾的生产方法

By using crushing and desliming methods and system mother liquor washing, the problems of low utilization rate and high water consumption of carnallite ore were solved, the yield and grade of potassium chloride were improved, and the product quality was enhanced.

CN117003259BActive Publication Date: 2026-11-24郭柏春
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211209585.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2026-11-24
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

Existing technologies suffer from low utilization rates of carnallite ore, high water consumption, and low potassium chloride grade. In particular, the crushing and dissolution of natural carnallite is difficult, resulting in low potassium chloride production efficiency.

Method used

The crushing and desliming process is adopted, and a saturated solution of magnesium chloride is used to deslim the carnallite ore. Combined with the system mother liquor for washing and crystallization, the mud particles are reduced from entering the crystallization and flotation process. The water consumption is reduced and the yield of potassium chloride is increased by supplementing the mother liquor.

Benefits of technology

It improved the utilization rate of carnallite, reduced water consumption, increased the grade and yield of potassium chloride, and improved the whiteness of potassium chloride products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117003259B_ABST
    Figure CN117003259B_ABST
Patent Text Reader

Abstract

The application discloses a production method of potassium chloride, which comprises the following steps: crushing and desliming, crushing carnallite ore and desliming the ore with a saturated magnesium chloride solution; and crystallization, mixing the deslimed ore, water and system mother liquor, and then feeding the mixture into a crystallizer to perform dissolution and crystallization. According to the application, the ore is cleaned before the crystallization step to remove the soil, so that the soil of the ore entering the crystallization and flotation process can be removed in time, the accumulation of soil particles in the crystallization and flotation process is avoided, the adverse effects of the soil particles on the crystallization and flotation process are avoided, and the whiteness of the potassium chloride product is improved. Meanwhile, the ore is deslimed with the system mother liquor, so that the washing water consumption is reduced, the tail liquid treatment amount is reduced, the ore decomposition in the desliming stage is prevented, and the dissolution in the crystallizer is completed at one time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of potassium chloride extraction, specifically relating to a method for producing potassium chloride using carnallite ore. Background Technology

[0002] Potassium chloride is an indispensable fertilizer in agricultural production and also an important ore in the chemical, metallurgical, pharmaceutical, and food industries. The main ores used to produce potassium chloride include sylvite and carnallite. Carnallite resources are relatively abundant, but its potassium content is usually lower than that of sylvite, resulting in higher processing energy consumption and a smaller proportion in potassium chloride production. Based on its formation process, carnallite is mainly divided into natural carnallite and salt lake carnallite. Salt lake carnallite is produced through a year of sun-drying and is easily broken and dissolved. Natural carnallite, especially Lao carnallite, has been underground for over 68 million years, making it about 10 times more difficult to break and dissolve than salt lake carnallite. Currently, most of the carnallite ore used in potassium chloride production is salt lake carnallite.

[0003] The existing process for producing potassium chloride from carnallite ore generally involves crushing, crystallization, flotation, and then a brine washing process to remove mud and insoluble impurities, thereby obtaining potassium chloride.

[0004] Existing methods generally suffer from drawbacks such as low utilization of carnallite, high water consumption, and low grade of potassium chloride produced. Summary of the Invention

[0005] The improved potassium chloride production method of this invention can increase the utilization rate of carnallite, reduce water consumption, and improve the grade of potassium chloride.

[0006] This invention provides a method for producing potassium chloride, comprising: crushing and desliming, crushing carnallite ore and desliming the ore with a saturated solution of magnesium chloride; and crystallization, mixing the deslimed ore, water and system mother liquor and then entering a crystallizer for dissolution and crystallization.

[0007] According to one embodiment of the present invention, in the crushing and desliming step, the carnallite ore is crushed into particles with a diameter of less than or equal to 20 mm, then deslimed, and then the deslimed ore is formed into particles with a diameter of less than or equal to 1 mm by a rod mill.

[0008] According to another embodiment of the present invention, the saturated solution of magnesium chloride is the system stock solution.

[0009] According to another embodiment of the present invention, the solids content in the desliming step is 50%-60%.

[0010] According to another embodiment of the present invention, in the crystallization step, the overflow of the crystallizer enters the solid-liquid separation device for solid-liquid separation, the separated solid enters the recrystallizer for further crystallization, and both the underflow of the crystallizer and the underflow of the recrystallizer enter the flotation step for flotation.

[0011] According to another embodiment of the present invention, in the crystallization step, the mass ratio of the deslimed ore, water and system mother liquor in the crystallizer is 1:0.2-0.35:4-6.5; preferably 1:0.25-0.35:4-6.

[0012] According to another embodiment of the present invention, the saturated solution of magnesium chloride is the system stock solution.

[0013] According to another embodiment of the invention, the recrystallizer is replenished with liquid via the system mother liquor.

[0014] According to another embodiment of the present invention, more than 70% of the potassium chloride crystals with a diameter greater than 0.15 mm are in the underflow of the crystallizer and the recrystallizer.

[0015] This invention removes mud from the ore before the crystallization step, thus promptly removing mud from the ore entering the crystallization and flotation processes. This prevents the accumulation of mud particles during crystallization and flotation and avoids their adverse effects on the crystallization and flotation processes, thereby improving the whiteness of the potassium chloride product. Simultaneously, this invention uses system mother liquor to deslim the ore, reducing washing water consumption and tailings treatment volume, preventing ore decomposition during the desliming stage, and ensuring that dissolution is completed in the crystallizer in a single step. Attached Figure Description

[0016] Figure 1 This is a flowchart illustrating one embodiment of the present invention.

[0017] Figure 2 This is a flowchart illustrating another embodiment of the present invention. Detailed Implementation

[0018] The present invention will now be described in detail with reference to specific embodiments.

[0019] The inventors discovered that carnallite ore inevitably contains clay, and these clay particles, once introduced into the crystallization process, act as crystal nuclei. An excessive number of these nuclei negatively impacts the production of potassium chloride crystals, thus affecting the particle size of the potassium chloride. Subsequently, in the flotation process, clay sludge inhibitors are added to mitigate the adverse effects of clay particles on positive flotation. Even then, some clay particles inevitably mix into the potassium chloride, affecting the whiteness of the product. Furthermore, the subsequent washing of crude potassium chloride requires a large amount of water to remove the inhibitors. This water-intensive washing process not only consumes a lot of water but also leads to the dissolution and loss of potassium chloride, resulting in a low yield. The inventors improved upon existing technology by using a system mother liquor to deslim the crushed ore, thus preventing clay particles from entering the crystallization and flotation processes. This avoids the adverse effects of clay particles on these two processes, improving whiteness, reducing water consumption, and increasing the yield of potassium chloride.

[0020] like Figure 1 As shown, the method for producing potassium chloride provided by the present invention includes: crushing and desliming, crushing carnallite ore and desliming the ore with a saturated solution of magnesium chloride; and crystallization, mixing the deslimed ore, water and system mother liquor and then entering a crystallizer for crystallization.

[0021] In this patent, "system mother liquor" refers to the liquid discharged from the system, such as the liquid separated from the crude potassium filtration process, the liquid separated from the tail salt filtration process, and the liquid discharged from the system that has been retained historically. The "system mother liquor" is a saturated solution of magnesium chloride.

[0022] Specifically, in the crushing and desliming step, the ore is first crushed and screened. The undersize material (which can be of an appropriate crushing particle size, such as, but not limited to, ≤20mm, ≤15mm, ≤10mm, ≤5mm, etc.) is washed, while the oversize material is returned to the crushing process for further crushing. During the washing process, the crushed ore is washed with system mother liquor.

[0023] Using the system's mother liquor to deslim the crushed ore can reduce the amount of washing water and tailings treatment, while also preventing the ore from decomposing during the desliming stage, allowing the dissolution to be completed in the crystallizer in one go.

[0024] After washing, the ore is screened, and the oversize material (greater than or equal to 1 mm) is further crushed. Rod milling is preferred for crushing, as it breaks the ore into particles smaller than 1 mm to facilitate dissolution within the crystallizer. The undersize material (less than or equal to 1 mm) flows into a solid-liquid separation unit; the solids enter the crystallization unit, while the liquid flows into a filtration unit for desliming. The liquid after removing the mud cake is then returned to the washing process for reuse. Since the underflow from each step carries away some mother liquor, it can be used to replenish the washing process. The solid content during washing is 50%-60%, maximizing the thorough washing of the ore.

[0025] In an optional implementation, the crystallization step may include the reuse of fine grains in the crystallizer overflow. Figure 2 This implementation method will be explained in detail. For example... Figure 2 As shown, in the crushing and desliming steps and Figure 1 The implementation methods shown are the same and will not be described again.

[0026] The undersize material (≤1mm) after rod milling enters the crystallizer, where the washed ore decomposes, and potassium chloride precipitates under the action of a saturated magnesium chloride solution. The precipitated potassium chloride gradually grows and flows into the flotation unit from the underflow. The overflow from the crystallizer contains small, ungrown crystals; after solid-liquid separation, the fine crystals enter the recrystallizer through the underflow. In the recrystallizer, the fine crystals grow again, and after reaching the predetermined size, they enter the flotation unit for flotation from the underflow. Since the underflow contains a certain amount of mother liquor, the liquid content in the crystallizer and recrystallizer decreases after the underflow from the crystallizer and recrystallizer. The liquid in the crystallizer and recrystallizer can be replenished by the system mother liquor.

[0027] In the crushing and desliming process, the underflow from the washed screened material, after filtration and thickening, can enter either the crystallizer or the recrystallizer, or a portion can enter the crystallizer and the other portion can enter the recrystallizer, depending on the actual operating conditions. In the recrystallizer, the fine crystals are reused, which can improve the yield of potassium chloride.

[0028] This invention utilizes the system's mother liquor to wash the ore and replenish the crystallizer and recrystallizer. This fully leverages the mother liquor while avoiding the "crystal bursting" that can occur during crystallization due to the addition of fresh water, which would otherwise hinder crystal growth and reduce potassium chloride production efficiency. "Crystal bursting" refers to the phenomenon where the addition of fresh water causes crystals to separate into smaller particles, leading to a rapid increase in the number of crystal nuclei and hindering further growth.

[0029] The liquid separated by the solid-liquid separation device contains finer potassium chloride crystals. After entering the fine crystal tank, the liquid is dissolved in fresh water to form an unsaturated potassium chloride solution. This solution enters the crystallizer to dissolve the crushed ore that has entered it. The mass ratio of the crushed ore, water, and saturated magnesium chloride solution in the crystallizer is 1:0.2–0.35:4–6.5. Preferably, it is 1:0.25–0.35:4–6.

[0030] In an optional implementation, the saturated solution of magnesium chloride can be the system stock solution.

[0031] In an optional implementation, more than 70% of the potassium chloride crystals with a diameter greater than 0.15 mm are found in the underflow of the crystallizer and recrystallizer.

[0032] In an optional implementation, the carnallite ore may be an ore such as Lao carnallite ore.

[0033] The present invention will be further described below through specific examples. However, these examples are merely exemplary and do not constitute any limitation on the scope of protection of the present invention.

[0034] Unless otherwise specified, all reagents, materials and instruments used in the following examples and comparative examples are commercially available.

[0035] Example 1

[0036] In the crushing unit, 10 kg of Lao carnallite is crushed into particles with a diameter of 5–20 mm. The crushed ore is then deslimed using the system's mother liquor, with a solids content of 60% during the desliming process. The deslimed ore is further rod-milled to form particles ≤1 mm, which are then fed into the crystallizer for crystallization. The crystallization process involves dissolution within the central cylinder of the crystallizer, with fine crystals entering the crystallization zone through a guide tube. Some potassium chloride crystal nuclei grow and fall to the bottom of the crystallizer due to gravity, then are sent to the slurry preparation tank via the underflow. Other potassium chloride crystal nuclei are discharged through the overflow outlet to the solid-liquid separation equipment for solid-liquid separation under the action of the fluid. The fine potassium chloride crystals enter the recrystallizer and, after recrystallization, enter the slurry preparation tank via the underflow outlet. The crystallizer underflow then enters the flotation unit. 70% of the potassium chloride crystals in the crystallizer underflow have a diameter greater than 0.15 mm.

[0037] In the flotation unit, octadecylamine is used as the flotation agent for flotation. Finally, the crude potassium chloride obtained is washed, dried, weighed, and its purity is tested.

[0038] Calculations showed that the yield of potassium chloride in this example was 82.0%, and the water consumption was 2.8 kg. The purity of the obtained potassium chloride was 98.2%.

[0039] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for producing potassium chloride, characterized in that, include: Crushing and desliming: The carnallite ore is crushed and deslimed with a saturated magnesium chloride solution. and Crystallization involves mixing the deslimed ore, water, and system mother liquor before introducing them into a crystallizer for dissolution and crystallization. In the crushing and desliming step, the carnallite ore is crushed into particles with a diameter of less than or equal to 20 mm, then deslimed, and then screened. The ore that has been deslimed after screening is ground into particles of less than or equal to 1 mm by a rod mill and then enters the crystallizer. The undersize material is fed into a solid-liquid separation device. The solid enters the crystallizer, and the liquid flows into a filtration device for filtration and desliming. The liquid after removing the mud cake is then returned to the crushing and desliming step for reuse. In the crystallization step, the overflow of the crystallizer enters the solid-liquid separation device for solid-liquid separation. The separated solid enters the recrystallizer for further crystallization, and the separated liquid contains finer potassium chloride crystals. After the liquid enters the fine crystal tank, fresh water is added to dissolve the potassium chloride crystals in the liquid to form an unsaturated potassium chloride solution. The unsaturated solution enters the crystallizer to dissolve the crushed ore that has entered it. The recrystallizer is replenished with liquid through the system mother liquor; both the underflow from the crystallizer and the underflow from the recrystallizer enter the flotation step for flotation, and more than 70% of the potassium chloride crystals with a diameter greater than 0.15 mm are present in the underflow from the crystallizer and the recrystallizer. In the crystallization step, the mass ratio of the deslimed ore, water, and system mother liquor in the crystallizer is 1:0.2~0.35:4~6.5; The saturated solution of magnesium chloride is the system's mother liquor; The solid content in the crushing and desliming step is 50%-60%.

2. The method for producing potassium chloride according to claim 1, characterized in that, In the crystallization step, the mass ratio of the deslimed ore, water, and system mother liquor in the crystallizer is 1: 0.25~0.35: 4~6.

Citation Information

Patent Citations

  • Novel system and method for producing potassium chloride by utilizing carnallite

    CN104058428A

  • Method for producing KCl from ground surface carnallite

    CN104163440A