Epoxy cyclohexane water reducing agent, its preparation method and application
By preparing an epoxy cyclohexane water-reducing agent and utilizing the polymerization of epoxy cyclohexane block polyether monomers and acrylic monomers, the problems of water bleeding and poor cohesiveness of polycarboxylate water-reducing agents in concrete were solved, thereby improving the fluidity and retention properties of concrete.
Patent Information
- Application Number
- CN202210470967.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-04-28
AI Technical Summary
Existing polycarboxylate superplasticizers have problems such as bleeding, slurry seepage, and poor cohesion in concrete, making it difficult to meet the requirements of construction pumping, especially when the quality of sand and gravel raw materials declines.
A novel epoxycyclohexane water-reducing agent was prepared by polymerizing polyether monomers containing different epoxycyclohexane blocks with acrylic monomers. By adjusting the polymerization reaction conditions and raw material ratios, the flowability, encapsulation, and cohesiveness were optimized.
It improves the fluidity, coating properties, and cohesiveness of concrete, enhances the concrete's retention performance, and addresses the shortcomings of existing water-reducing agents in the use of high mud content and manufactured sand.
Smart Images

Figure CN117003954B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of concrete water-reducing agent technology, and specifically relates to an epoxy cyclohexane water-reducing agent, its preparation method, and its application. Background Technology
[0002] Polycarboxylate superplasticizers, as an important component of modern concrete, have been widely used in the field of concrete engineering technology due to their excellent advantages such as low dosage, high water reduction, high slump retention, and high degree of freedom in molecular design. Currently, the widely used polycarboxylate superplasticizers on the market are polymerized from ether monomers, ester monomers, and acrylic monomers. Among them, ether monomers dominate the polycarboxylate superplasticizer market due to their higher cost-effectiveness, while the market share of mother liquor synthesized from ester monomers is relatively low.
[0003] As market demand changes, ether monomers are also constantly evolving. From APEG to HPEG, the focus is mainly on water reduction performance. From HPEG to TPEG, the focus is on slump retention. And in recent years, vinyl ether monomers have emerged, moving towards a combination of water reduction and slump retention. With the shortage of raw materials such as sand and gravel in the market, the widespread use of manufactured sand, and the continuous decline in material quality, concrete is prone to bleeding, slurry bleeding, rapid loss, and poor encapsulation and cohesion, making it difficult to pump. Therefore, concrete has placed higher demands on the comprehensive performance of polycarboxylate superplasticizers in terms of water reduction, slump retention, encapsulation, and cohesion. Summary of the Invention
[0004] To meet the technical requirements for some or all of the above-mentioned performance characteristics, the present invention provides a water-reducing agent having a structure as shown in formula (1) or formula (2):
[0005]
[0006] Where 0 < n ≤ 10, and n is an integer or a non-integer, with a further preference for 0 < n ≤ 5. For example, n can be 1, 2, 3, 4, or 5. a and b are integers or non-integers, the same or different, and are independently selected from any of the following continuous ranges: 0 < a ≤ 200, 0 ≤ b ≤ 10; for example, 5 ≤ a ≤ 150, 1 ≤ b ≤ 8; or 10 ≤ a ≤ 130, 2 ≤ b ≤ 6. For example, a can be 18, 19, 47, 48, 57, 58, 61, 62, 81, 82, 127, or 128; and b can be 0 or 3.
[0007] R1 is ethylene glycol *-OCH2CH2O-* or diethylene glycol *-OCH2CH2OCH2CH2O-*, where * indicates the linkage site;
[0008] R3 is selected from C 1-9Alkyl or H, such as C 1-6 Alkyl groups, such as C 1-4 Alkyl group, exemplarily, R3 is selected from H;
[0009] R2 is selected from H; R4 is selected from H or C. 1-9 Alkyl or C 2-4 Hydroxyl-substituted alkyl group; R5 is selected from H or methyl; preferably, R2, R4, and R5 are independently selected from H;
[0010] c and d are integers or non-integers, the same or different, and are independently selected from any consecutive numbers within the following range: 0 < c ≤ 100; 0 < d ≤ 100; for example, 20 ≤ c ≤ 180; 14 ≤ d ≤ 148; and 10 ≤ c ≤ 90, 7 ≤ d ≤ 74.
[0011] The arrangement of ethylene oxide segments and propylene oxide segments is as shown in formula (1) or formula (2).
[0012] According to an embodiment of the present invention, the repeating unit The terminator is determined according to the termination method of the free radical polymerization reaction in this application, such as coupling termination and disproportionation termination. Specifically, the initiator and chain transfer agent used in this application provide the terminating group, such as terminating groups -H, -OH, -SCH2COOH or -SCH2CH2COOH, etc.
[0013] According to an exemplary embodiment of the present invention, the water-reducing agent has a structure as shown in any one of formulas (9)-(12):
[0014]
[0015]
[0016] The present invention also provides a method for preparing the water-reducing agent as described above, which is obtained by polymerization of raw materials including polyether monomers and acrylic monomers represented by formula (3) or (4):
[0017]
[0018] Among them, R1, R2, and R3 have the meanings described above; n, a, and b have the value ranges shown above;
[0019] The arrangement of ethylene oxide segments and propylene oxide segments is as shown in formula (3) or formula (4);
[0020] The acrylic monomer is at least one of acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, dimethyl maleate, diethyl maleate, di-n-propyl maleate, and dibutyl maleate.
[0021] According to an embodiment of the present invention, the acrylic monomer is preferably acrylic acid.
[0022] According to an embodiment of the present invention, the amount of polyether monomer in the raw material is 20-60 parts by weight. For example, the amount of polyether monomer is 30-50 parts, exemplarily 30 parts, 43 parts, 45 parts, 46 parts, 49 parts, and 50 parts.
[0023] According to an embodiment of the present invention, the amount of acrylic monomer in the raw material is 0.5-25 parts by weight, for example 1-20 parts, and exemplary amounts are 2.3 parts, 2.7 parts, 3.6 parts, 3.7 parts, 4.7 parts, 4.8 parts, 5 parts, 5.6 parts, 13 parts, and 14.8 parts.
[0024] According to an embodiment of the present invention, the polymerization reaction is carried out in the presence of an initiator. The initiator content is 0.1-2 parts by weight, for example 0.1-1 parts; exemplaryly, the initiator content is 0.1 parts, 0.3 parts, 0.5 parts, 0.6 parts, 0.8 parts, or 1 part.
[0025] According to an embodiment of the present invention, the initiator is at least one selected from hydrogen peroxide, ammonium persulfate, potassium persulfate, sodium persulfate, azobisisobutyronitrile, and azobisisoheptanenitrile.
[0026] According to an embodiment of the present invention, the polymerization reaction is carried out in the presence of a chain transfer agent. The amount of the chain transfer agent, by weight, is 0.05-3 parts, for example 0.1-2 parts, exemplarily 0.1 parts, 0.12 parts, 0.15 parts, 0.16 parts, 0.2 parts, 0.27 parts, 0.35 parts, 0.42 parts, 0.68 parts, 0.78 parts, 0.88 parts, 1.6 parts, and 2 parts.
[0027] According to an embodiment of the present invention, the chain transfer agent is at least one selected from mercaptopropionic acid, mercaptoacetic acid, isopropanol, sodium formate, isooctyl 3-mercaptopropionate, dodecyl mercaptosulfonate or sodium hypophosphite, and mercaptoethanol; preferably mercaptoacetic acid or mercaptopropionic acid.
[0028] According to an embodiment of the present invention, the polymerization reaction is carried out in the presence of a reducing agent. The amount of the reducing agent is 0.05-1.5 parts by weight, for example 0.1-0.8 parts, exemplarily 0.1 parts, 0.12 parts, 0.15 parts, 0.2 parts, 0.3 parts, 0.35 parts, 0.42 parts, 0.68 parts, and 0.8 parts.
[0029] According to an embodiment of the present invention, the reducing agent is at least one selected from L-ascorbic acid, sodium formaldehyde sulfoxylate, bisulfite, sulfite, thiosulfate, metabisulfite and ferrous salt, preferably L-ascorbic acid.
[0030] According to an embodiment of the present invention, the polymerization reaction is carried out in the presence of water. The amount of water used is 20-70 parts by weight, for example 25-35 parts, such as 25 parts, 28 parts, 30 parts, 32.5 parts, 33 parts, and 35 parts.
[0031] According to an embodiment of the present invention, the water-reducing agent is prepared by polymerization of raw material polyether monomer and acrylic monomer in the presence of an additive;
[0032] By weight, the raw materials and additives include: 30-50 parts of polyether monomer, 1-20 parts of acrylic monomer, 0.1-1 part of initiator, 0.1-2 parts of chain transfer agent, 0.1-0.8 parts of reducing agent, and 30-70 parts of water.
[0033] According to an embodiment of the present invention, the method for preparing the water-reducing agent includes the following steps:
[0034] (1) Mix the polyether monomer, initiator and water evenly to obtain material one;
[0035] (2) Mix the acrylic monomer, chain transfer agent, reducing agent and water evenly to obtain material two;
[0036] (3) Mix the second material and the first material, keep warm and mature to obtain the water-reducing agent;
[0037] The amounts of the polyether monomer, initiator, acrylic monomer, chain transfer agent, and reducing agent have the meanings and ranges described above.
[0038] According to an embodiment of the present invention, in step (1), the polyether monomer and water can be mixed first, and after the polyether monomer is dissolved, an initiator can be added to it.
[0039] According to an embodiment of the present invention, in step (1), the amount of water added is sufficient to dissolve the polyether monomer.
[0040] The total amount of water used in steps (1) and (2) is 30-70 parts.
[0041] According to an embodiment of the present invention, in step (1), the dissolution temperature of the polyether monomer is 0-60°C, for example 10-60°C, or 20-50°C, or 30-40°C.
[0042] According to an embodiment of the present invention, in step (3), the mixing can be stirring or dripping, preferably dripping.
[0043] According to an embodiment of the present invention, in step (3), when material one and material two are mixed by stirring, the stirring time can be 20-40 minutes, for example 30 minutes.
[0044] According to an embodiment of the present invention, in step (3), when material two is added dropwise to material one to mix the two, the dropping time can be 25-180 min, for example 30-150 min. For example, the dropping can be added continuously or in batches.
[0045] According to an embodiment of the present invention, in step (3), the temperature of mixing and heat preservation is controlled at 0-60°C, for example 10-50°C, or 20-50°C, or 30-40°C.
[0046] According to an embodiment of the present invention, in step (3), the heat preservation and curing time is 0.5-3h, for example 1-2.5h, exemplarily 1h, 1.5h, 2h or 2.5h.
[0047] The present invention also provides polyether monomers represented by formula (3) or formula (4):
[0048]
[0049] Among them, R1, R2, and R3 have the meanings described above; n, a, and b have the value ranges shown above.
[0050] According to an embodiment of the present invention, the polyether monomer has any one of the structures of formulas (5)-(8):
[0051]
[0052] Where n is 1, a is 19, and b is 0;
[0053] Alternatively, n is 2, a is 48, and b is 0;
[0054] Alternatively, n is 2, a is 62, and b is 0;
[0055] Alternatively, n is 3, a is 82, and b is 0;
[0056] Alternatively, n is 3, a is 128, and b is 0;
[0057] Alternatively, n can be 2, a can be 58, and b can be 3;
[0058]
[0059]
[0060] Where n is 1, a is 18, and b is 0;
[0061] Alternatively, n is 2, a is 47, and b is 0;
[0062] Or n is 2, a is 61, and b is 0;
[0063] Or n is 3, a is 81, and b is 0;
[0064] Or n is 3, a is 127, and b is 0;
[0065] Or n is 2, a is 57, and b is 3;
[0066]
[0067] According to an embodiment of the present invention, the weight-average molecular weight of the polyether monomer is 1000-10000, for example 2000-6000.
[0068] The present invention also provides a method for preparing the polyether monomer as described above, comprising the following steps: reacting vinyl glycol ether or diethylene glycol monovinyl ether with cyclohexane oxide, then introducing ethylene oxide or propylene oxide for polymerization, and optionally adding propylene oxide or ethylene oxide to undergo a polymerization reaction to obtain the polyether monomer.
[0069] According to embodiments of the present invention, the molar ratio of vinyl glycol ether or diethylene glycol monovinyl ether, cyclohexane oxide, ethylene oxide, and propylene oxide is (0.9-1.2):(0.9-5):a:b, for example, 1:(1-3):a:b. Wherein, a and b have the value ranges shown above. Exemplarily, the molar ratio is 1:1:19:0, 1:2:48:0, 1:2:62:0, 1:3:82:0, 1:3:128:0, 1:1:18:0, 1:2:61:0, 1:3:81:0, 1:3:127:0, 1:2:58:3, or 1:2:57:3.
[0070] According to an embodiment of the present invention, the order in which ethylene oxide and propylene oxide are added in the above method is not limited. For example, ethylene oxide can be added first to react with the intermediate, and then propylene oxide can be added; or propylene oxide can be added first to react with the intermediate, and then ethylene oxide can be added.
[0071] According to an embodiment of the present invention, the polymerization reaction is carried out in the presence of a catalyst. The catalyst is a basic catalyst, for example, selected from one, two, or more of alkali metals, alkaline earth metals, hydrides, oxides, hydroxides, alkoxides, and strong base-weak acid salts of alkali metals or alkaline earth metals; for example, the basic catalyst can be one, two, or more of KOH, NaOH, CH3ONa, and CH3OK. Further, the mass of the catalyst is 0.01–3.0% of the total mass, where the total mass is the total mass of vinyl ethylene glycol ether or diethylene glycol monovinyl ether with cyclohexane oxide, ethylene oxide, and optionally propylene oxide, for example, 0.05–2.5%, or 0.1–2%.
[0072] According to one embodiment of the present invention, the method for preparing the polyether monomer includes: first adding a catalyst to vinyl ethylene glycol ether or diethylene glycol monovinyl ether; after the temperature rises to 100-120°C, introducing cyclohexane oxide to carry out a polymerization reaction, maintaining the reactor pressure in the range of 0.2-0.4 MPa; after all the cyclohexane oxide has been added, maintaining the temperature, and when the reactor pressure no longer decreases, introducing ethylene oxide into the reactor to carry out a polymerization reaction; after the reaction is completed, degassing under vacuum, and cooling to obtain the polyether monomer. The system temperature when ethylene oxide is added is maintained at 110-130°C, for example, 120°C. After all the ethylene oxide is added, the reaction time is 1-3 hours, for example, 1 hour; the reaction temperature is 120-140°C, for example, 130°C.
[0073] According to an embodiment of the present invention, the temperature is reduced to 70-90°C, for example, 80°C.
[0074] According to an embodiment of the invention, the polymerization reaction is carried out under an inert atmosphere, such as nitrogen.
[0075] The present invention also provides the use of polyether monomers as shown in formula (3) or formula (4) as described above in the preparation of water-reducing agents with structures as shown in formula (1) or formula (2).
[0076] The present invention also provides the application of the above-mentioned water-reducing agent in improving the workability of concrete. Preferably, the application is in improving the encapsulation, cohesiveness, and flow retention properties of concrete.
[0077] According to an embodiment of the present invention, the water-reducing agent has a solid content of 0.1-0.3% of the cement mass in the concrete, for example, 0.2%.
[0078] The present invention also provides concrete comprising the above-described water-reducing agent. Preferably, the water-reducing agent is used in the amount shown above.
[0079] Beneficial effects of the present invention
[0080] (1) The water-reducing agent provided by the present invention is polymerized with polyether monomers containing different epoxy cyclohexane blocks containing oxides and acrylic monomers to obtain samples with better flowability, encapsulation, cohesiveness and retention. Compared with ordinary water-reducing agents sold on the market, it has better performance in terms of concrete encapsulation, cohesiveness and retention.
[0081] (2) The water-reducing agent preparation method of this invention has a wider temperature range (0-60℃) during the synthesis process, and is not limited to the low temperature (0-20℃) of the prior art. Large-scale production can be carried out normally without the need for equipment improvement or addition, and the raw materials used are all common mother liquor synthesis raw materials that are readily available on the market. Therefore, the water-reducing agent of this invention has certain application prospects. Attached Figure Description
[0082] Figure 1 The NMR spectrum of the polyether monomer prepared in Example 1 (the deuteration reagent is deuterated chloroform).
[0083] Figure 2 The NMR spectrum of the water-reducing agent prepared in Example 1 (the deuterated reagent is deuterated chloroform).
[0084] Figure 3 This is a gel chromatogram of the polyether monomer prepared in Example 1.
[0085] Terminology Explanation and Definition
[0086] Unless otherwise defined, all technical terms in this document have the same meaning as commonly understood by one of ordinary skill in the art to which the subject matter of the claims pertains. Unless otherwise stated, all patents, patent applications, and publications cited in this document are incorporated herein by reference in their entirety. If multiple definitions exist for terms in this document, the definitions provided in this section shall prevail.
[0087] The numerical ranges described in this application specification and claims, when the range can only be "integers," should be understood to include the two endpoints of the range and every integer within the range. For example, "0 < n ≤ 10, and n is an integer" should be understood to include every integer of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. When the numerical range is described as "non-integer," it should be understood to include every decimal, where the decimal includes the sum of each integer 0, 1, 2, 3, 4, 5, 6, 7, 8, and 9 with 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, respectively. For example, "0 < n ≤ 10, and n is a non-integer" should be understood as recording the sum of each integer 0, 1, 2, 3, 4, 5, 6, 7, 8, 9 with 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9; "0 < a ≤ 200", "0 ≤ b ≤ 10", "0 < c ≤ 100", and "0 < d ≤ 100" have the same definition of n as above.
[0088] Term "C" 1-9 "Alkyl" should be understood as a straight-chain or branched saturated monovalent hydrocarbon group having 1, 2, 3, 4, 5, 6, 7, 8, or 9 carbon atoms. The alkyl group is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl, or 1,2-dimethylbutyl, etc., or isomers thereof. In particular, the group has 1, 2, 3, 4, 5, or 6 carbon atoms ("C"). 1-6 Alkyl groups, such as methyl, ethyl, propyl, butyl, isopropyl, isobutyl, sec-butyl, tert-butyl, and more particularly, said groups have 1, 2, 3, or 4 carbon atoms (“C”). 1-4 Alkyl), such as methyl, ethyl, n-propyl, isopropyl, or butyl.
[0089] Term "C" 2-4 "Hydroxy-substituted alkyl" indicates a group containing 2, 3, or 4 carbon atoms -ROH, where R is C. 2-4 Alkyl, the C 2-4 Alkyl groups have the above definition. As an example, the C... 2-4 The hydroxyl-substituted alkyl group is selected from -C2H4OH or -C3H6OH.
[0090] All polymer molecular weights mentioned in this application refer to weight-average molecular weights. Detailed Implementation
[0091] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0092] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0093] In the following examples, "**" refers to parts by weight.
[0094] In the following examples, the molecular weight of the polyether monomer was obtained by theoretical calculation of the feed amount and GPC testing. That is, the polyether monomer was first synthesized by theoretical calculation of the feed reaction, and then verified by GPC testing.
[0095] Example 1
[0096] 1. Add 43 parts of polyether monomer 1 and 28 parts of water to the reactor, stir and melt at 10-20℃, then add 0.5 parts of hydrogen peroxide initiator, stir for 5 minutes to obtain material one.
[0097] The structure of polyether monomer 1 is shown in formula (5).
[0098]
[0099] Where n is 1, a is approximately 19, and b is 0.
[0100] The preparation process of polyether monomer 1 is as follows: 200g of vinyl ethylene glycol ether is added to a stainless steel high-pressure reactor, along with 4.54g of potassium hydroxide solid. Nitrogen purging is performed, followed by stirring and heating to approximately 90°C. The reactor is then maintained at 90°C under vacuum for 1 hour for dehydration. After another nitrogen purging, the temperature is raised to 120°C, and 223g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added. The reactor is then kept at this temperature for approximately 1 hour until the pressure no longer decreases. Next, 1850g of ethylene oxide is slowly introduced into the reactor for polymerization, maintaining the temperature at 130°C and the pressure at approximately 0.3MPa until all the ethylene oxide is added. The reactor is then kept at this temperature for approximately 1 hour. The temperature is lowered to 80°C, and after vacuum degassing, the product is discharged to obtain polyether monomer 1 with a molecular weight of approximately 1000. Its NMR characterization results are as follows: Figure 1 As shown, the gel chromatogram is as follows: Figure 3 As shown.
[0101] 2. Preparation of dropwise addition: Mix 19 parts water, 13 parts acrylic acid, 0.78 parts chain transfer agent mercaptoacetic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0102] 3. Add the prepared feedstock to material 1 dropwise over a period of 60 minutes, maintaining the temperature inside the reactor at 38°C. After the addition is complete, keep the mixture at this temperature for 90 minutes to allow it to mature. Then, discharge the material to obtain water-reducing agent 1. Its NMR characterization results are as follows: Figure 2 As shown;
[0103] The water-reducing agent 1 has the structure shown in formula (9):
[0104]
[0105] Where c:d is approximately 4.2.
[0106] Example 2
[0107] 1. Add 43 parts of polyether monomer 2 and 28 parts of water to the reactor, stir and melt at 20-30℃, then add 0.5 parts of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0108] The structure of polyether monomer 2 is shown in formula (5).
[0109]
[0110] Where n is approximately 2, a is approximately 48, and b is 0.
[0111] The preparation process of polyether monomer 2 is as follows: 105g of vinyl ethylene glycol ether is added to a stainless steel high-pressure reactor, along with 5.72g of potassium hydroxide solid. Nitrogen gas is used for purging. Then, under stirring, heating is started and the temperature is raised to about 90℃. Vacuum dehydration is maintained at 90℃ for 1 hour. After nitrogen purging again, the temperature is raised to 120℃, and 233g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130℃, and the pressure is relatively constant at about 0.3MPa until all the cyclohexane oxide is added to the reactor. The temperature is maintained for about 1 hour, and when the reactor pressure no longer decreases, 2524g of ethylene oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130℃, and the pressure is relatively constant at about 0.3MPa until all the ethylene oxide is added to the reactor. The temperature is maintained for about 1 hour, and the temperature is lowered to 80℃. After vacuum degassing, the product is discharged to obtain polyether monomer 2 with a molecular weight of about 2400.
[0112] 2. Preparation of dropwise addition: Mix 19 parts water, 5 parts acrylic acid, 0.1 parts chain transfer agent mercaptoacetic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0113] 3. Add the prepared dropper to material 1 over a period of 55 minutes. Control the temperature inside the reactor at 42°C. After the dropper is finished, keep it warm and mature for 90 minutes. Then discharge the material to obtain water-reducing agent 2.
[0114] The water-reducing agent 2 has the structure shown in formula (9).
[0115]
[0116] Where c:d is approximately 3.9.
[0117] Example 3
[0118] 1. Add 30 parts of polyether monomer 3 and 25 parts of water to the reactor, stir and melt at 30-40℃, then add 0.5 parts of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0119] The structure of polyether monomer 3 is shown in formula (5).
[0120]
[0121] Where n is approximately 2, a is approximately 62, and b is 0.
[0122] Vinylon glycol ether (85g) was added to a stainless steel high-pressure reactor, along with 5.79g of solid potassium hydroxide (or another alkaline catalyst). Nitrogen purging was performed, and then, with stirring, heating was initiated to approximately 90°C. This temperature was maintained at 90°C under vacuum for 1 hour for dehydration. After another nitrogen purging, the temperature was raised to 120°C, and 189g of cyclohexane oxide was slowly introduced into the reactor to initiate the polymerization reaction. The temperature was maintained at 130°C, and the pressure remained relatively constant at approximately 0.3MPa until all the cyclohexane oxide was added to the reactor. The reactor was then kept at this temperature for approximately 1 hour. When the reactor pressure no longer decreases, the temperature is lowered to 80°C, and after vacuum degassing, intermediate 3 is discharged. Intermediate 3 is then completely added to a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After the temperature rises to 120°C, 2623g of ethylene oxide is slowly introduced into the reactor to carry out the polymerization reaction. The temperature is maintained at 130°C, and the pressure is kept relatively constant at about 0.3MPa until all the ethylene oxide is added to the reactor. The reactor is then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product is discharged to obtain polyether monomer 3 with a molecular weight of about 3000.
[0123] 2. Preparation of dropwise addition: Mix 19 parts water, 2.7 parts acrylic acid, 0.16 parts chain transfer agent mercaptoacetic acid, and 0.1 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0124] 3. Add the prepared additive to material 1 over a period of 75 minutes. Control the temperature inside the reactor to 38°C. After the addition is complete, keep the mixture warm for 90 minutes before discharging to obtain water-reducing agent 3.
[0125] The water-reducing agent 3 has the structure shown in formula (9).
[0126]
[0127] Where c:d is approximately 3.75
[0128] Example 4
[0129] 1. Add 49 parts of polyether monomer 4 and 32.5 parts of water to the reactor, stir and melt at 30-40℃, then add 1.0 part of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0130] The structure of polyether monomer 4 is shown in formula (5).
[0131]
[0132] Where n is approximately 3, a is approximately 82, and b is 0.
[0133] The preparation process of polyether monomer 4 is as follows: 65g of vinyl ethylene glycol ether is added to a stainless steel high-pressure reactor, along with 5.91g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration is maintained at 90°C for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 217g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature. After about 1 hour, when the reactor pressure no longer decreased, the temperature was lowered to 80°C, and after vacuum degassing, intermediate 4 was discharged. Intermediate 4 was then completely added to a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After the temperature was raised to 120°C, 2672g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C, and the pressure was kept relatively constant at about 0.3MPa until all the ethylene oxide was added to the reactor. The reactor was then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 4 with a molecular weight of about 4000.
[0134] 2. Preparation of dropwise addition: Mix 21 parts water, 3.6 parts acrylic acid, 0.26 parts chain transfer agent mercaptopropionic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0135] 3. Add the prepared additive to material 1 over a period of 75 minutes. Control the temperature inside the reactor at 42°C. After the addition is complete, keep the mixture warm for 90 minutes before discharging to obtain water-reducing agent 4.
[0136] The water-reducing agent 4 has the structure shown in formula (9):
[0137]
[0138] Where c:d is approximately 4.1.
[0139] Example 5
[0140] 1. Add 45 parts of polyether monomer and 35 parts of water to the reactor, stir and melt at 30-40℃, then add 1.0 part of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0141] The structure of polyether monomer 5 is shown in formula (5).
[0142]
[0143] Where n is approximately 3, a is approximately 128, and b is 0.
[0144] The preparation process of polyether monomer 5 is as follows: 45g of vinyl ethylene glycol ether is added to a stainless steel high-pressure reactor, along with 6.13g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen purging is performed, followed by heating under stirring to approximately 90°C. The reactor is then maintained at 90°C under vacuum for 1 hour for dehydration. After another nitrogen purging, the temperature is raised to 120°C, and 150g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide has been added to the reactor. The reactor is then kept at this temperature. After about 1 hour, when the reactor pressure no longer decreased, the temperature was lowered to 80°C, and after vacuum degassing, intermediate 5 was discharged. Intermediate 5 was then completely added to a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After the temperature was raised to 120°C, 2872g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C, and the pressure was kept relatively constant at about 0.3MPa until all the ethylene oxide was added into the reactor. The reactor was then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 5 with a molecular weight of about 6000.
[0145] 2. Preparation of dropwise addition: Mix 19 parts water, 2.3 parts acrylic acid, 0.2 parts chain transfer agent mercaptopropionic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0146] 3. Add the prepared dropper to material 1 over a period of 75 minutes. Control the temperature inside the reactor at 40°C. After the dropper is finished, keep it warm for 90 minutes before discharging to obtain water-reducing agent 5.
[0147] The water-reducing agent 5 has the structure shown in formula (9):
[0148]
[0149] Where c:d is approximately 4.3.
[0150] Example 6
[0151] 1. Add 49 parts of polyether monomer 6 and 33 parts of water to the reactor, stir and melt at 10-20℃, then add 0.8 parts of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0152] The preparation process of polyether monomer 6 is as follows: 250g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 3.79g of potassium hydroxide solid (or other alkaline catalyst). Nitrogen is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration at 90°C is maintained for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 186g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. When the reactor pressure no longer decreases, 1894g of ethylene oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the ethylene oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. The temperature is lowered to 80°C, and after vacuum degassing, the product is discharged to obtain polyether monomer 6 with a molecular weight of approximately 1000.
[0153] The structure of polyether monomer 6 is shown in formula (7).
[0154]
[0155] Where n is approximately 1, a is approximately 18, and b is 0.
[0156] 2. Preparation of dropwise addition: Mix 21 parts water, 14.8 parts acrylic acid, 0.88 parts chain transfer agent mercaptoacetic acid, and 0.13 parts reducing agent L-ascorbic acid and stir until the materials are dissolved evenly and set aside.
[0157] 3. Add the prepared feedstock to material 1 over a period of 60 minutes. Control the temperature inside the reactor to 35°C. After the feedstock is added, keep it warm for 90 minutes before discharging to obtain water-reducing agent 6.
[0158] The water-reducing agent 6 has the structure shown in formula (11).
[0159]
[0160] Where c:d is approximately 4.2.
[0161] Example 7
[0162] 1. Add 45 parts of polyether monomer and 30 parts of water to the reactor, stir and melt at 30-40℃, then add 0.8 parts of hydrogen peroxide as initiator and stir for 5 minutes to obtain material one.
[0163] Polyether monomer 7 has the structure shown in formula (7).
[0164]
[0165] Where n is approximately 2, a is approximately 47, and b is 0.
[0166] The preparation process of polyether monomer 7 is as follows: 120g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 4.36g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration at 90°C is maintained for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 178g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. When the reactor pressure no longer decreases, 1883g of ethylene oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the ethylene oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. The temperature is lowered to 80°C, and after vacuum degassing, the product is discharged to obtain polyether monomer 7 with a molecular weight of approximately 2400.
[0167] 2. Preparation of dropwise addition: Mix 21 parts water, 5.6 parts acrylic acid, 0.15 parts chain transfer agent mercaptopropionic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are dissolved and uniform before use.
[0168] 3. Add the prepared dropper to material 1 over a period of 55 minutes. Control the temperature inside the reactor to 38°C. After the dropper is finished, keep it warm for 90 minutes before discharging to obtain water-reducing agent 7.
[0169] The water-reducing agent 7 has the structure shown in formula (11).
[0170]
[0171] Where c:d is approximately 4.1.
[0172] Example 8
[0173] 1. Add 49 parts of polyether monomer and 33 parts of water to the reactor, stir and melt at 30-40℃, then add 0.8 parts of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0174] Polyether monomer 8 has the structure shown in formula (7).
[0175]
[0176] Where n is approximately 2, a is approximately 61, and b is 0.
[0177] The preparation method of polyether monomer 8 is as follows: 95g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 4.31g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen purging is performed, followed by heating under stirring to approximately 90°C. The mixture is then kept at 90°C for vacuum dehydration for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 141g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide has been added to the reactor. After heating for about 1 hour, when the reactor pressure no longer decreased, the temperature was lowered to 80°C. After vacuum degassing, intermediate 8 was discharged. All intermediate 8 was put into a stainless steel high-pressure reactor, purged with nitrogen, and then heated with stirring. After heating to 120°C, 1923g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C and the pressure was relatively constant at about 0.3MPa until all the ethylene oxide was added into the reactor. The reactor was then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 8 with a molecular weight of about 3000.
[0178] 2. Preparation of dropwise addition: Mix 19 parts water, 4.8 parts acrylic acid, 0.16 parts chain transfer agent mercaptoacetic acid, and 0.1 parts reducing agent L-ascorbic acid and stir until the materials are dissolved evenly and set aside.
[0179] 3. Add the prepared feedstock to material 1 over a period of 75 minutes. Control the temperature inside the reactor to 35°C. After the feedstock is added, keep it warm for 90 minutes before discharging to obtain water-reducing agent 8.
[0180] The water-reducing agent 8 has the structure shown in formula (11).
[0181]
[0182] Where c:d is approximately 4.1.
[0183] Example 9
[0184] 1. Add 49 parts of polyether monomer and 32.5 parts of water to the reactor, stir and melt at 30-40℃, then add 1.0 part of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0185] The structural formula of polyether monomer 9 is shown in formula (7):
[0186]
[0187] Where n is approximately 3, a is approximately 81, and b is 0.
[0188] The preparation process of polyether monomer 9 is as follows: 80g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 4.84g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen purging is performed, followed by heating under stirring to approximately 90°C. Vacuum dehydration at 90°C is maintained for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 141g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. After heating for about 1 hour, when the reactor pressure no longer decreased, the temperature was lowered to 80°C. After vacuum degassing, intermediate 9 was discharged. All intermediate 9 was put into a stainless steel high-pressure reactor, purged with nitrogen, and then heated with stirring. After heating to 120°C, 2166g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C and the pressure was relatively constant at about 0.3MPa until all the ethylene oxide was added into the reactor. The reactor was then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 9 with a molecular weight of about 4000.
[0189] 2. Preparation of dropwise addition: Mix 21 parts water, 3.7 parts acrylic acid, 0.27 parts chain transfer agent mercaptoacetic acid, and 0.12 parts reducing agent L-ascorbic acid and stir until the materials are evenly dissolved and ready for use.
[0190] 3. Add the prepared dropper to material 1 over a period of 75 minutes, keeping the temperature inside the reactor below 38°C. After the dropper is finished, keep it warm for 70 minutes before discharging to obtain water-reducing agent 9.
[0191] The water-reducing agent 9 has the structure shown in formula (11):
[0192]
[0193] Where c:d is approximately 4.2.
[0194] Example 10
[0195] The only difference between Example 10 and Example 5 is the polyether monomer used. Example 10 uses polyether monomer 10, the structural formula of which is shown in formula (7):
[0196]
[0197] Where n is approximately 3, a is approximately 127, and b is 0.
[0198] The preparation process of polyether monomer 10 is as follows: 60g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 5.45g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen gas is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration is maintained at 90°C for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 133g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature. After about 1 hour, when the reactor pressure no longer decreased, the temperature was lowered to 80°C, and after vacuum degassing, intermediate 10 was discharged. Intermediate 10 was then completely added to a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After the temperature was raised to 120°C, 2533g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C, and the pressure was kept relatively constant at about 0.3MPa until all the ethylene oxide was added to the reactor. The reactor was then kept at this temperature for about 1 hour, cooled to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 10 with a molecular weight of about 6000.
[0199] The structural formula of the prepared water-reducing agent 10 is shown in formula (11):
[0200]
[0201] Where c:d is approximately 4.3.
[0202] Example 11
[0203] 1. Add 49 parts of polyether monomer 11 and 32.5 parts of water to the reactor, stir and melt at 30-40℃, then add 0.8 parts of hydrogen peroxide initiator and stir for 5 minutes to obtain material one.
[0204] The structural formula of polyether monomer 11 is shown in formula (5).
[0205]
[0206] Where n is approximately 2, a is approximately 58, and b is 3.
[0207] The preparation process of polyether monomer 11 is as follows: 80g of vinyl ethylene glycol ether is added to a stainless steel high-pressure reactor, along with 5.45g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration at 90°C is maintained for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 178g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. When the reactor pressure no longer decreases, the temperature is lowered to 80°C, and after vacuum degassing, intermediate 11 is obtained. Intermediate 11 is then fully processed... The ethylene oxide was placed in a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After reaching 120°C, 2310g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C, and the pressure was kept relatively constant at around 0.3MPa until all the ethylene oxide was added to the reactor. The reactor was then kept at this temperature for about 1 hour. After cooling down to 120°C, 158g of propylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 120°C, and the pressure was kept relatively constant at around 0.3MPa until all the propylene oxide was added to the reactor. The reactor was then kept at this temperature for about 1 hour. When the reactor pressure no longer decreased, the temperature was lowered to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 11 with a molecular weight of approximately 3000.
[0208] 2. Preparation of dropwise addition: Mix 21 parts water, 4.7 parts acrylic acid, 0.26 parts chain transfer agent mercaptoacetic acid, and 0.15 parts reducing agent L-ascorbic acid and stir until the materials are dissolved evenly and set aside.
[0209] 3. Add the prepared additive to material 1 over a period of 50 minutes, keeping the temperature inside the reactor below 35°C. After the addition is complete, keep the mixture warm for 90 minutes before discharging to obtain water-reducing agent 11.
[0210] The water-reducing agent 11 has the structure shown in formula (9).
[0211]
[0212] Where c:d is approximately 4.0.
[0213] Example 12
[0214] The only difference between Example 12 and Example 11 is the polyether monomer used. The structural formula of polyether monomer 12 in Example 12 is shown in formula (7).
[0215]
[0216] Where n is approximately 2, a is approximately 57, and b is 3.
[0217] The preparation process of polyether monomer 12 is as follows: 90g of diethylene glycol monovinyl ether is added to a stainless steel high-pressure reactor, along with 4.09g of solid potassium hydroxide (or other alkaline catalyst). Nitrogen is used for purging. Then, under stirring, heating is initiated and the temperature is raised to approximately 90°C. Vacuum dehydration at 90°C is maintained for 1 hour. After another nitrogen purging, the temperature is raised to 120°C, and 133g of cyclohexane oxide is slowly introduced into the reactor for polymerization. The temperature is maintained at 130°C, and the pressure is kept relatively constant at approximately 0.3MPa until all the cyclohexane oxide is added to the reactor. The reactor is then kept at this temperature for approximately 1 hour. When the reactor pressure no longer decreases, the temperature is lowered to 80°C, and after vacuum degassing, intermediate 12 is obtained. Intermediate 12 is then... All the ethylene oxide was placed in a stainless steel high-pressure reactor, purged with nitrogen, and then heated under stirring. After the temperature reached 120°C, 1703g of ethylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 130°C and the pressure was kept relatively constant at about 0.3MPa until all the ethylene oxide was added into the reactor. The reactor was then kept at this temperature for about 1 hour. After the temperature dropped to 120°C, 119g of propylene oxide was slowly introduced into the reactor to carry out the polymerization reaction. The temperature was maintained at 120°C and the pressure was kept relatively constant at about 0.3MPa until all the propylene oxide was added into the reactor. The reactor was then kept at this temperature for about 1 hour. When the reactor pressure stopped dropping, the temperature was lowered to 80°C, and after vacuum degassing, the product was discharged to obtain polyether monomer 12 with a molecular weight of about 3000.
[0218] The water-reducing agent 12 has the structure shown in formula (11).
[0219]
[0220] Where c:d is approximately 4.0.
[0221] Application examples
[0222] Measurement of implementation effect:
[0223] Concrete mix design (parts by weight)
[0224] cement river sand pebbles water 360 760 1050 170
[0225] The cement in the concrete formula is PO42.5 Southern Cement, the river sand has a fineness modulus of 2.0 and a mud content of 2.7% (by weight), and the aggregate size is 5-20mm.
[0226] A C7 type general-purpose polycarboxylate superplasticizer from Jiangsu Chaoli Building Materials Co., Ltd. was selected as a control example. Its addition amount was 0.2% (consolidated weight) of the cement mass. In the application examples, the same amount was added as the control example, and tests were conducted. The performance of concrete prepared using the control example and the superplasticizers from Examples 1-12 is shown in Table 1.
[0227] Table 1 Comparison of concrete performance in application
[0228] The relevant performance tests of concrete were conducted in accordance with the "Standard for Test Methods of Performance of Ordinary Concrete Mixtures" (GB / T50080-2016) and "Concrete Admixtures" (GB / T 8076-2016).
[0229]
[0230]
[0231] Application Example 1 uses the water-reducing agent prepared in Example 1, Application Example 2 uses the water-reducing agent prepared in Example 2, and so on.
[0232] As can be seen from Table 1, the water-reducing agent synthesized by the method of the present invention has improved concrete encapsulation, cohesiveness and retention performance, among which the water-reducing agent prepared in Example 12 has the best performance.
[0233] The embodiments of the present invention have been described above. However, the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A water-reducing agent, characterized in that, The water-reducing agent has a structure as shown in formula (1) or formula (2): Equation (1) ; Equation (2) Where 2≤n≤5, n is an integer or a non-integer; a and b are integers or non-integers, the same or different, and are independently selected from any of the following continuous ranges: 47≤a≤130, 0≤b≤5; R1 is an ethylene glycol group. or diethylene glycol group , where * indicates a connection site; R3 is selected from H; R2 is selected from H; R4 is selected from H; R5 is selected from H or methyl; c and d are integers or non-integers, the same or different, and are independently selected from any consecutive numbers within the following range: 0 < c ≤ 100; 0 < d ≤ 100; The arrangement of ethylene oxide segments and propylene oxide segments is as shown in formula (1) or formula (2).
2. The water-reducing agent according to claim 1, characterized in that, 47≤a≤128。 3. The water-reducing agent according to claim 1 or 2, characterized in that, n is 2, 3, 4, or 5; a is 47, 48, 57, 58, 61, 62, 81, 82, 127, 128; b is 0 or 3; R3 is selected from H; c and d are integers or non-integers, the same or different, and are independently selected from any consecutive numbers within the following range: 10≤c≤90, 7≤d≤74.
4. The water-reducing agent according to claim 1, characterized in that, The water-reducing agent has any one of the structures of formula (9)-(12): Equation (9) Equation (10) Equation (11) Equation (12) Wherein, a, b, c, d, and n have the meanings described in claim 1.
5. A method for preparing the water-reducing agent according to any one of claims 1-4, characterized in that, It is obtained by polymerization of raw materials including polyether monomers and acrylic monomers as shown in formula (3) or (4): Equation (3) ; Equation (4) Wherein, R1, R2, R3, n, a, and b have the meaning as described in any one of claims 1-4; The arrangement of ethylene oxide segments and propylene oxide segments is as shown in formula (3) or formula (4); The acrylic monomer is acrylic acid or methacrylic acid.
6. The preparation method according to claim 5, characterized in that, The amount of polyether monomer in the raw material is 20-60 parts by weight; The amount of acrylic monomers used in the raw materials is 0.5-25 parts.
7. The preparation method according to claim 5 or 6, characterized in that, The polymerization reaction is carried out in the presence of an initiator.
8. The preparation method according to claim 7, characterized in that, The initiator content is 0.1-2 parts by weight.
9. The preparation method according to claim 7, characterized in that, The initiator is at least one of hydrogen peroxide, ammonium persulfate, potassium persulfate, sodium persulfate, azobisisobutyronitrile, and azobisisoheptanenitrile.
10. The preparation method according to claim 5, characterized in that, The polymerization reaction is carried out in the presence of a chain transfer agent.
11. The preparation method according to claim 10, characterized in that, The amount of the chain transfer agent is 0.05-3 parts by weight.
12. The preparation method according to claim 10, characterized in that, The chain transfer agent is at least one of mercaptopropionic acid, mercaptoacetic acid, isopropanol, sodium formate, isooctyl 3-mercaptopropionate, dodecyl mercaptothiol or sodium hypophosphite, and mercaptoethanol.
13. The preparation method according to claim 10, characterized in that, The polymerization reaction is carried out in the presence of a reducing agent.
14. The preparation method according to claim 13, characterized in that, The amount of the reducing agent is 0.05-1.5 parts by weight.
15. The preparation method according to claim 13, characterized in that, The reducing agent is at least one of L-ascorbic acid, sodium formaldehyde sulfoxylate, bisulfite, sulfite, thiosulfate, metabisulfite, and ferrous salt.
16. The preparation method according to claim 5, characterized in that, The polymerization reaction is carried out in the presence of water.
17. The preparation method according to claim 16, characterized in that, The amount of water used is 20-70 parts by weight.
18. The use of the water-reducing agent according to any one of claims 1-4 in improving the workability of concrete.
19. The application of the water-reducing agent according to any one of claims 1-4 in improving the encapsulation, cohesiveness, and flow retention properties of concrete.
20. The application according to claim 18 or 19, characterized in that, The water-reducing agent has a solid content of 0.1-0.3% of the cement mass in the concrete.
21. A type of concrete, characterized in that, Includes the water-reducing agent according to any one of claims 1-4.
Citation Information
Patent Citations
Alkenyl-terminated unsaturated polyether, preparation method and application thereof
CN103897169A
Concrete conditioning agent and preparation method and application thereof
CN112538143A