Interface-modified recycled carbon fiber epoxy resin composite material and preparation method and application thereof

By using in-situ polymerization and the π-π conjugation effect of aromatic diamine monomers, the problems of complex formulation and weak interfacial bonding in the treatment of recycled carbon fibers were solved, and the uniform dispersion and high-efficiency microwave absorption performance of recycled carbon fibers in resin were achieved.

CN117004184BActive Publication Date: 2026-11-24BEIJING UNIV OF CHEM TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311039141.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-17
Publication Date
2026-11-24
Estimated Expiration
2043-08-17

AI Technical Summary

Technical Problem

Existing methods for processing recycled carbon fibers have complex formulations, require vacuum infiltration assistance, and the sizing methods suffer from insufficient mechanical properties and weak interfacial bonding.

Method used

An in-situ polymerization method is used to perform π-π conjugation between aromatic diamine monomers and recycled carbon fibers. The uniform coating of the recycled carbon fibers with polyimide improves their dispersibility in the resin, and the reaction between benzimidazole groups and epoxy resin groups enhances the interfacial bonding strength between the filler and the resin matrix.

Benefits of technology

This method achieves uniform coating of polyimide on the surface of recycled carbon fibers, improves its dispersion in the resin, reduces the material's electrical conductivity, and enhances its microwave absorption performance and interfacial bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117004184B_ABST
    Figure CN117004184B_ABST
Patent Text Reader

Abstract

This invention relates to an interface-modified recycled carbon fiber epoxy resin composite material, its preparation method, and its application. It solves the technical problems of existing methods for treating recycled carbon fibers, such as complex formulations, the need for vacuum infiltration to assist in sizing, insufficient mechanical properties, and weak interfacial bonding. The interface-modified recycled carbon fiber epoxy resin composite material provided by this invention includes carbon fibers and a coating layer; the coating layer is a polyimide obtained by polymerization and imidization of monomers containing benzimidazole diamine and dianhydride; this invention can be used in the field of microwave absorbing material preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a recycled carbon fiber material, its preparation method, and its application; more specifically, it relates to an interface-modified recycled carbon fiber epoxy resin composite material, its preparation method, and its application. Background Technology

[0002] The widespread adoption of communication technologies and advanced electronic devices has brought immense convenience to human life, but it has also led to electromagnetic interference and leakage problems. Simultaneously, the continuous development of high-end industrial equipment has placed higher demands on the performance of electromagnetic absorbing materials. Currently, domestic electromagnetic absorbing materials are mainly coating-type, containing ferrites or metals, and suffer from problems such as high density, poor thermal stability, and weak mechanical properties. The rapid development of high-end aerospace equipment has placed higher demands on the manufacturing of composite material components. Structural / functional integrated composite materials have the advantages of low density, good mechanical properties, and long lifespan, and are currently the main development direction for composite material research in the military and aerospace industries.

[0003] Carbon fiber possesses excellent electrical conductivity and microwave absorption properties, making it an important microwave absorber. However, the high degree of graphitization and chemical inertness of carbon fiber surfaces make dispersion very difficult, and the high production cost limits the application of carbon fiber resin matrix composites in structural / functional integration. Compared to virgin carbon fiber, recycled carbon fiber (also known as regenerated carbon fiber) obtained from composite materials has a higher retention rate of mechanical properties and lower cost, but a larger surface roughness, thus attracting widespread attention in the field of electromagnetic shielding / absorbing.

[0004] Currently, surface modification of carbon materials is divided into covalent modification and non-covalent modification. Covalent modification methods, such as chemical oxidation, electrochemical oxidation, plasma treatment, and chemical grafting, are relatively complex and can affect the properties of carbon fibers. Non-covalent modification methods, on the other hand, are simpler to operate and do not damage the fiber surface structure. Polyimide refers to a class of special engineering materials containing a five-membered ring structure of imide in its main chain, possessing excellent mechanical properties, high and low temperature resistance, and insulation properties. Aromatic polyimides contain a large number of benzene rings, offering structural advantages whether used as a carbon material matrix or for surface treatment.

[0005] Recycled carbon fiber is produced by chemical or heat treatment of carbon fiber composites. Its original long fiber morphology is destroyed, and it is mainly used in the form of short-cut fibers. At present, there is a lack of effective surface modification methods for recycled carbon fiber.

[0006] Chinese invention patent CN202210816244.1 discloses an aqueous sizing agent and sizing method for treating recycled carbon fibers. This patent uses a relatively complex formulation and requires vacuum infiltration to complete the sizing process. The sizing method suffers from insufficient mechanical properties and weak interfacial bonding, making it unsuitable for practical applications. Summary of the Invention

[0007] This invention aims to address the technical problems of existing methods for processing recycled carbon fibers, such as complex formulations, the need for vacuum infiltration to assist in sizing, insufficient mechanical properties, and weak interfacial bonding. It provides an interface-modified epoxy resin composite material for recycled carbon fibers, its preparation method, and its application.

[0008] Therefore, the present invention provides an interface-modified recycled carbon fiber epoxy resin composite material, which includes carbon fibers and a coating layer; the coating layer is a polyimide obtained by polymerization and imidization of monomers containing benzimidazole diamine and dianhydride; the mass fraction of carbon fibers and polyimide in the composite material is 0.1% to 2%.

[0009] This invention also provides a method for preparing an interface-modified carbon fiber epoxy resin composite material, which includes the following steps: (1) Grinding recycled carbon fibers using a ball mill and separating recycled carbon fiber powder of a certain length using a mesh screen; adding the recycled carbon fiber powder to a solvent containing diamine monomers and performing ultrasonication and stirring; then adding dianhydride monomers for in-situ polymerization to obtain polyamic acid-coated recycled carbon fibers; (2) Slowly pouring the mixture obtained in step (1) into ice water to wash away the solvent, filtering, and freeze-drying the filtered product to obtain recycled carbon fiber / polyamic acid powder; (3) High-temperature imidizing the powder prepared in step (2) in a carbonization furnace, and grinding the resulting product to obtain recycled carbon fiber / polyimide powder; (4) Adding the recycled carbon fiber / polyimide powder to epoxy resin, heating and stirring until uniform, adding a curing agent and mixing thoroughly; casting the resin using a mold to obtain an interface-modified recycled carbon fiber epoxy resin composite material.

[0010] Preferably, in step (1), the raw material carbon fiber for the recycled carbon fiber is polyacrylonitrile-based carbon fiber or pitch-based carbon fiber, including high-strength carbon fiber (T300, T700, T800, T1000, T1100, etc.) and high-modulus carbon fiber (M35J, M40J, M46J, M50J, M55J, M60J, etc.).

[0011] Preferably, in step (1), the length of the recovered carbon fiber is between 20 μm and 0.5 mm; the diamine monomer is one of 2-(4-aminophenyl)-5-aminobenzimidazole or 2-(3-aminophenyl)-5-aminobenzimidazole; the dianhydride monomer is at least one of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, and 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride; and the solvent is one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0012] Preferably, in step (1), the total mass of the monomers to the mass ratio of the recycled carbon fibers is 1:(2-20); the reaction time is 12h-24h.

[0013] Preferably, in step (4), the epoxy resin is at least one of difunctional epoxy resin, trifunctional epoxy resin, and tetrafunctional epoxy resin; the curing agent is an amine curing agent, including 4,4'-diaminodiphenyl sulfone or 4,4'-methylenediphenylamine.

[0014] This invention also provides an application of interface-modified carbon fiber epoxy resin composite material as a microwave absorbing material.

[0015] The present invention has the following beneficial effects:

[0016] This invention utilizes in-situ polymerization and the π-π conjugation between aromatic diamine monomers and recycled carbon fibers to achieve uniform coating of polyimide on the surface of recycled carbon fibers. This improves its dispersibility in the resin, reduces the material's electrical conductivity, and enhances its microwave absorption performance. Simultaneously, the introduced benzimidazole groups react with epoxy groups during epoxy resin curing, increasing the interfacial bonding strength between the filler and the resin matrix. Attached Figure Description

[0017] Figure 1 This is an electron microscope image of the recycled carbon fiber / polyimide powder prepared in Example 1 of the present invention, with a magnification of 500x;

[0018] Figure 2 This is the DSC curve of the reaction between the recycled carbon fiber / polyimide and AG-80 epoxy resin in Example 3 of the present invention. Detailed Implementation

[0019] The present invention will be further described below with reference to embodiments.

[0020] In this embodiment of the invention, the carbon fiber in the selected waste carbon fiber resin matrix composite material is Toray T700 carbon fiber, with a single filament tensile strength of 4.90 GPa. The recycled carbon fiber was obtained through pyrolysis. The reflection loss data characterizing the microwave absorption performance of the epoxy resin composite material was measured using the coaxial method.

[0021] Example 1

[0022] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0023] (1) The recycled carbon fibers were pre-milled using a ball mill and separated using a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 20 μm to 100 μm. 1.7 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 50 mL of N,N-dimethylformamide. 2 g of the recycled carbon fiber powder was added, and the mixture was ultrasonicated and stirred. 1.7 mmol of pyromellitic dianhydride was added for in-situ polymerization, and the reaction was carried out for 12 h to obtain polyamic acid-coated recycled carbon fibers. The mass ratio of the total monomer to the recycled carbon fibers was 1:2.

[0024] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0025] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0026] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 0.1%, is added to the epoxy resin. The mixture of resin and filler is heated to 120°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably E-51 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:31.5; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

[0027] The surface-modified recycled carbon fiber prepared in this embodiment has the following appearance: Figure 1 As shown, the carbon fiber surface is coated with a thick polyimide layer with spherical protrusions. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -8.5 dB and a flexural strength of 103.6 MPa.

[0028] Example 2

[0029] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0030] (1) The recycled carbon fibers were pre-milled using a ball mill and separated using a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 20 μm to 100 μm. 0.34 mmol of 2-(3-aminophenyl)-5-aminobenzimidazole was dissolved in 50 mL of N,N-dimethylformamide. 2 g of the recycled carbon fiber powder was added, and the mixture was sonicated and stirred. 0.34 mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added for in-situ polymerization, and the reaction was carried out for 18 h to obtain polyamic acid-coated recycled carbon fibers. The mass ratio of the total monomer to the recycled carbon fibers was 1:5.

[0031] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0032] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0033] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 0.5%, is added to the epoxy resin. The mixture of resin and filler is heated to 80°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably E-51 and 4,4'-methylenediphenylamine, respectively, and the mass ratio of epoxy resin to curing agent is 100:29; the curing process of the resin is 80°C for 1 hour, 120°C for 3 hours, and 150°C for 2 hours.

[0034] The surface-modified recycled carbon fiber prepared in this embodiment exhibits a relatively uniform polyimide coating on its surface without obvious protrusions. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -16.3 dB, a -10 dB bandwidth of 1.6 GHz, and a flexural strength of 110.9 MPa.

[0035] Example 3

[0036] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0037] (1) The recycled carbon fibers were pre-milled using a ball mill and separated by a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 100 μm to 0.5 mm. 0.34 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 50 mL of N,N-dimethylacetamide. 1 g of recycled carbon fiber powder was added, and the mixture was sonicated and stirred. 0.34 mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added for in-situ polymerization, and the reaction was carried out for 18 h to obtain polyamic acid-coated recycled carbon fibers. The mass ratio of the total monomer to the recycled carbon fibers was 1:5.

[0038] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0039] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0040] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 0.5%, is added to the epoxy resin. The mixture of resin and filler is heated to 120°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:40; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

[0041] The surface-modified recycled carbon fiber prepared in this embodiment exhibits a relatively uniform polyimide coating on its surface, with no obvious protrusions. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -19.7 dB, a -10 dB bandwidth of 2.5 GHz, and a flexural strength of 82.3 MPa.

[0042] refer to Figure 2 As can be seen from the DSC curve, the exothermic peak of the addition of recycled carbon fiber / polyimide is significantly enhanced, indicating that polyimide reacts with AG-80 under the condition of no curing agent.

[0043] Example 4

[0044] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0045] (1) The recycled carbon fibers were pre-milled using a ball mill and separated using a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 20 μm to 100 μm. 0.17 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 20 mL of N,N-dimethylacetamide. 1 g of the recycled carbon fiber powder was added, and the mixture was sonicated and stirred. 0.17 mmol of 3,3',4,4'-tetracarboxylic acid diphenyl ether dianhydride was added for in-situ polymerization, and the reaction was carried out for 18 h to obtain polyamic acid-coated recycled carbon fibers. The mass ratio of the total monomer to the recycled carbon fibers was 1:10.

[0046] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0047] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0048] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 0.5%, is added to the epoxy resin. The mixture of resin and filler is heated to 120°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:40; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

[0049] The surface-modified recycled carbon fiber prepared in this embodiment exhibits a relatively uniform polyimide coating on its surface. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -22.0 dB, a -10 dB bandwidth of 3.6 GHz, and a flexural strength of 79.5 MPa.

[0050] Example 5

[0051] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0052] (1) The recycled carbon fibers were pre-milled using a ball mill and separated using a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 20 μm to 100 μm. 0.17 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 20 mL of N-methylpyrrolidone. 1 g of the recycled carbon fiber powder was added, and the mixture was sonicated and stirred. 0.17 mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added for in-situ polymerization, and the reaction was carried out for 24 h to obtain polyamic acid-coated recycled carbon fibers. The mass ratio of the total monomer to the recycled carbon fibers was 1:10.

[0053] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0054] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0055] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 2%, is added to the epoxy resin. The mixture of resin and filler is heated to 120°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:40; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

[0056] The surface-modified recycled carbon fiber prepared in this embodiment exhibits a relatively uniform polyimide coating on its surface. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -26.6 dB, a -10 dB bandwidth of 3.9 GHz, and a flexural strength of 90.8 MPa.

[0057] Example 6

[0058] The method for preparing surface-modified recycled carbon fiber and its epoxy resin composite material provided in this embodiment includes the following:

[0059] (1) The recycled carbon fibers were pre-ground using a ball mill, and the shorter fibers were separated using a 300-mesh sieve. 0.085 mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 20 mL of N,N-dimethylacetamide. 1 g of recycled carbon fibers was added, and the mixture was sonicated and stirred. 0.085 mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added for in-situ polymerization, and the reaction was carried out for 24 h to obtain polyamic acid-coated recycled carbon fiber powder. The mass ratio of the total monomer to the recycled carbon fibers was 1:20.

[0060] (2) Slowly pour the mixture generated from the reaction into ice water to wash away the solvent. Freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder;

[0061] (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder.

[0062] (4) Recycled carbon fiber / polyimide powder, with a mass fraction of 1%, is added to the epoxy resin. The mixture of resin and filler is heated to 120°C, stirred evenly, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain a carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:40; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

[0063] The surface-modified recycled carbon fiber prepared in this embodiment exhibits a uniform polyimide layer coating on its surface. Testing revealed that the carbon fiber / polyimide / epoxy resin composite material prepared in this embodiment has a minimum reflectivity of -24.3 dB, a -10 dB bandwidth of 2.9 GHz, and a flexural strength of 97.2 MPa.

[0064] The interface-modified recycled carbon fiber epoxy resin composite materials prepared in Examples 1 to 6 above can be used directly as microwave absorbing materials.

[0065] Comparative Example

[0066] This embodiment describes surface modification of recycled carbon fibers using an acid oxidation method. The recycled carbon fibers were pre-milled using a ball mill and separated using a mesh sieve to obtain recycled carbon fiber powder with a length of approximately 20 μm to 100 μm. A mixed acid solution of 100 mL of concentrated sulfuric acid (98%) and concentrated nitric acid (64%) in equal volume ratio was prepared, added to a reflux reflux apparatus along with 5 g of the recycled carbon fiber powder, and refluxed at 60°C for 1 h. The product was removed, washed thoroughly with deionized water, and dried under vacuum at 100°C for 12 h. A 5% silane coupling agent / ethanol solution was prepared using γ-aminopropyltriethoxysilane, and the acid-treated recycled carbon fibers were added and mixed thoroughly, then stirred for 9 h. This yielded the surface-modified recycled carbon fibers.

[0067] Preparation of carbon fiber / epoxy resin composite material: Surface-modified recycled carbon fiber, with a mass fraction of 1%, is added to epoxy resin. The mixture of resin and filler is heated to 120°C, stirred until homogeneous, and then a curing agent is added and stirred for 1 hour. After vacuum degassing, the resulting mixture is cast using a mold to obtain the carbon fiber / polyimide / epoxy resin composite material. In this embodiment, the epoxy resin and curing agent are preferably TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, with a mass ratio of epoxy resin to curing agent of 100:40; the resin curing process is 150°C for 1 hour and 180°C for 3 hours.

[0068] The carbon fiber / epoxy resin composite material prepared in this comparative example has a minimum reflectivity of -18.7dB, a -10dB bandwidth of 2.4GHz, and a flexural strength of 77.5MPa.

[0069] However, the above description is merely a specific embodiment of the present invention and should not be construed as limiting the scope of the present invention. Therefore, any substitution of equivalent components or equivalent changes and modifications made in accordance with the scope of protection of the present invention should still fall within the scope of the claims of the present invention.

Claims

1. The application of an interface-modified recycled carbon fiber epoxy resin composite material as a microwave absorbing material, characterized in that, The composite material is prepared using a method comprising the following steps: (1) The recycled carbon fiber was pre-ground by a ball mill and separated by a mesh screen to obtain recycled carbon fiber powder with a length of 20μm to 100μm; 0.17mmol of 2-(4-aminophenyl)-5-aminobenzimidazole was dissolved in 20mL of N-methylpyrrolidone; 1g of recycled carbon fiber powder was added, and the mixture was sonicated and stirred; 0.17mmol of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added for in-situ polymerization, and the reaction was carried out for 24 h to obtain polyamic acid-coated recycled carbon fiber, with the total mass of monomers to the mass ratio of recycled carbon fiber being 1:10; (2) Slowly pour the mixture generated by the reaction into ice water to wash away the solvent, and freeze-dry the filtered product to obtain recycled carbon fiber / polyamic acid powder; (3) The powder prepared in step (2) is imidized in a carbonization furnace at 350°C for 1 hour, and the resulting product is ground to obtain recycled carbon fiber / polyimide powder. (4) Add recycled carbon fiber / polyimide powder to epoxy resin, with a mass fraction of 2%; heat the mixture of resin and filler to 120°C, stir evenly, add curing agent and stir for 1 hour; after vacuum degassing the mixture, cast it with a mold to obtain carbon fiber / polyimide / epoxy resin composite material; the epoxy resin and curing agent are TDE-85 and 4,4'-diaminodiphenyl sulfone, respectively, and the mass ratio of epoxy resin to curing agent is 100:40; the curing process of the resin is 150°C for 1 hour and 180°C for 3 hours.

Citation Information

Patent Citations

  • Aqueous sizing agent and sizing method suitable for recycling carbon fiber