A gas diffusion electrode, its preparation method and use
By designing a porous current collector and catalytic diffusion layer, and combining it with coating treatment of catalytically active materials and polymers, a gas diffusion electrode with high dispersibility and good stability was constructed, which solved the problems of poor mechanical strength and stability in the existing technology and realized the CO₂ reduction reaction under high current density.
Patent Information
- Application Number
- CN202210476206.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-04-29
AI Technical Summary
Existing gas diffusion electrodes suffer from problems such as low mechanical strength, high cost, uneven catalyst dispersion, and poor electrode stability in CO₂ reduction reactions, making it difficult to achieve industrial applications at high current densities.
A gas diffusion electrode was designed, comprising a current collector, a catalytic diffusion layer, and a catalytic layer. The current collector has a porous structure, and the catalytic diffusion layer and the catalytic layer are composed of first and second catalytically active substances and a polymer, respectively. The electrode structure with high dispersibility and good stability is formed by coating, cold pressing, and annealing.
A gas diffusion electrode with high dispersibility, high mechanical strength, and good stability was achieved. It can carry out CO₂ reduction reaction at high current density, exhibits high selectivity and low overpotential, and demonstrates good electrochemical performance.
Smart Images

Figure HDA0003625676910000011 
Figure HDA0003625676910000012 
Figure HDA0003625676910000021
Abstract
Description
Technical Field
[0001] This invention relates to the field of gas diffusion electrode technology, and in particular to a gas diffusion electrode, its preparation method, and its application. Background Technology
[0002] CO2 is one of the main greenhouse gases, and its concentration in the atmosphere has increased approximately 100 times faster than the previous natural increase over the past two decades. Due to the urgency of reducing greenhouse gas emissions, the electrochemical conversion of CO2 into valuable fuels and industrial feedstocks has attracted widespread attention. However, large-scale application of this technology requires the ability to maintain a current density of 200 mA / cm² over extended periods. 2 Only in this way can economic benefits be achieved. Currently, over 95% of research and testing are conducted in traditional H-type electrolytic cells, using CO2 dissolved in the electrolyte as the reaction raw material. Due to the limited solubility of CO2 in solution, its limiting current density is approximately 35 mA / cm². 2 This is far less than the requirements for industrialization.
[0003] Some work has drawn inspiration from the gas diffusion electrode structure in fuel cells, overcoming the limitations of gas solubility and utilizing the gas-liquid-solid three-phase interface to directly carry out the CO2 reduction reaction, achieving testing at higher current densities. However, firstly, using carbon paper as the substrate for supporting the catalyst results in low mechanical strength and high cost, leading to excessively high costs for industrial applications. Secondly, the dispersion of the catalyst on the carbon paper is not high; a high loading amount leads to an increase in the thickness of the catalyst layer, preventing some catalyst from contacting the reactants and causing a decrease in catalytic efficiency, while a low loading amount results in insufficient catalytic activity. Furthermore, the background reaction between CO2 and the alkaline electrolyte generates a large amount of salt in situ inside the gas diffusion electrode, clogging the gas transport channels, reducing electrode stability, and making long-term stable operation difficult. Therefore, these problems urgently need to be solved. Summary of the Invention
[0004] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a gas diffusion electrode, its preparation method and application, wherein the gas diffusion electrode has high dispersibility, good stability and high mechanical strength.
[0005] To achieve the above and other related objectives, the first aspect of the present invention provides a gas diffusion electrode, comprising a current collector, a catalytic diffusion layer, and a catalytic layer;
[0006] The current collector has a porous structure;
[0007] The catalytic diffusion layer fills the porous structure, and the catalytic diffusion layer includes a first catalytically active substance and a first polymer;
[0008] The catalyst layer is loaded on the catalytic diffusion layer, and the catalyst layer includes a second catalytically active material and a second polymer.
[0009] Preferably, it further includes at least one of the following technical features:
[0010] a1) The mass ratio of the catalytic diffusion layer to the current collector is 1:2 to 1:10, such as 1:2 to 3:8, 3:8 to 1:3, 1:3 to 1:4 or 1:4 to 1:10;
[0011] a2) The mass ratio of the catalyst layer to the current collector is 1:10 to 1:100, such as 1:10 to 1:12, 1:12 to 1:17, 1:17 to 1:25, 1:25 to 1:35, 1:35 to 1:48 or 1:48 to 1:100;
[0012] a3) The current collector is selected from at least one of nickel foam, copper foam, stainless steel mesh, copper mesh, nickel mesh, metal-based nano-polypropylene film, and metal-based nano-polytetrafluoroethylene film.
[0013] More preferably, in feature a3), the metal base is Ag or Cu nanoparticles.
[0014] Preferably, it further includes at least one of the following technical features:
[0015] b1) The first catalytically active material is selected from at least one of the following: carbon-based supported metal with CO2 catalytic activity, carbon-based supported metal oxide with CO2 catalytic activity, carbon-based supported single-atom catalyst with CO2 catalytic activity, and carbon-based supported molecular catalyst.
[0016] b2) The first polymer is selected from at least one of polytetrafluoroethylene and polyvinylidene fluoride;
[0017] b3) The mass ratio of the first catalytic active substance to the first polymer is 2:3 to 15:1, such as 2:3 to 1:1, 1:1 to 2:1, 2:1 to 8:3, 8:3 to 8:1 or 8:1 to 15:1;
[0018] b4) The second catalytically active material is selected from at least one of the following: carbon-based supported metal with CO2 catalytic activity, carbon-based supported metal oxide with CO2 catalytic activity, carbon-based supported single-atom catalyst with CO2 catalytic activity, and carbon-based supported molecular catalyst.
[0019] b5) The second polymer is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride and perfluorosulfonic acid;
[0020] b6) The mass ratio of the second catalytic active substance to the second polymer is 2:3 to 15:1, such as 2:3 to 3:1, 3:1 to 5:1, 5:1 to 10:1 or 10:1 to 15:1.
[0021] More preferably, it also includes at least one of the following technical features:
[0022] c1) In feature b1) or feature b4), the metal with CO2 catalytic activity is selected from at least one of Ag, Au, Cu, Sn, Bi and Zn;
[0023] c2) In feature b1) or feature b4), the metal oxide with CO2 catalytic activity is selected from at least one of Ag, Au, Cu, Sn, Bi and Zn oxides;
[0024] c3) In feature b1) or feature b4), the carbon substrate is selected from at least one of conductive carbon black, Ketjen black, acetylene black, carbon nanotubes and graphene;
[0025] c4) In feature b1) or feature b4), the single-atom catalyst with CO2 catalytic activity is selected from at least one of Fe, Co and Ni single-atom catalysts;
[0026] c5) In feature b1) or feature b4), the molecular catalyst is selected from at least one of cobalt phthalocyanine, iron phthalocyanine and nickel phthalocyanine;
[0027] c6) In feature b1), the loading rate of at least one of the following: a metal with CO2 catalytic activity, a metal oxide with CO2 catalytic activity, a single-atom catalyst with CO2 catalytic activity, and a molecular catalyst is 20%–80%, such as 20%–50%, 50%–66.7%, 66.7%–70%, or 70%–80%. For example, when the first catalytically active material is a carbon-based supported metal with CO2 catalytic activity, the loading rate of the CO2-catalyzing metal is the mass percentage of the CO2-catalyzing metal to the carbon-based supported CO2-catalyzing metal; when the first catalytically active material is a carbon-based supported metal oxide with CO2 catalytic activity, the loading rate of the CO2-catalyzing metal oxide is the mass percentage of the CO2-catalyzing metal to the carbon-based supported CO2-catalyzing metal. The percentage by mass of CO2-catalyzing metal oxides relative to the total mass of CO2-catalyzing metal oxides supported on a carbon substrate; when the first catalytically active material is a carbon-based supported molecular catalyst, the molecular catalyst loading rate is the percentage by mass of the molecular catalyst relative to the total mass of the carbon-based supported molecular catalyst; when the first catalytically active material is a carbon-based supported metal and a carbon-based supported metal oxide, the loading rate of the CO2-catalyzing metal and the CO2-catalyzing metal oxide is the percentage by mass of the total mass of the CO2-catalyzing metal and the CO2-catalyzing metal oxide supported on a carbon substrate.
[0028] c7) In feature b4), the loading rate of at least one of the following: a metal with CO2 catalytic activity, a metal oxide with CO2 catalytic activity, a single-atom catalyst with CO2 catalytic activity, and a molecular catalyst is 20%–80%, such as 20%–50%, 50%–70%, or 70%–80%. For example, when the second catalytic active material is a carbon-based supported metal with CO2 catalytic activity, the loading rate of the CO2-catalyzing metal is the mass percentage of the CO2-catalyzing metal to the carbon-based supported CO2-catalyzing metal; when the second catalytic active material is a carbon-based supported metal oxide with CO2 catalytic activity, the loading rate of the CO2-catalyzing metal oxide is the mass percentage of the CO2-catalyzing metal. The percentage by mass of the active metal oxides on the carbon substrate that have CO2 catalytic activity; when the second catalytic active material is a carbon substrate-supported molecular catalyst, the molecular catalyst loading rate is the percentage by mass of the molecular catalyst on the carbon substrate-supported molecular catalyst, etc.; when the second catalytic active material is a carbon substrate-supported metal with CO2 catalytic activity and a carbon substrate-supported metal oxide with CO2 catalytic activity, the loading rate of the CO2 catalytic active metal and the CO2 catalytic active metal oxide is the percentage by mass of the total mass of the CO2 catalytic active metal and the CO2 catalytic active metal oxide on the carbon substrate-supported metal with CO2 catalytic activity and the carbon substrate-supported metal oxide with CO2 catalytic activity.
[0029] A second aspect of the present invention provides a method for preparing the above-mentioned gas diffusion electrode, comprising the following steps:
[0030] 1) A first slurry comprising the first catalytic active material and the first polymer is coated onto the surface of the current collector, and then subjected to cold pressing and annealing to construct the catalytic diffusion layer;
[0031] 2) A second slurry comprising the second catalytically active substance and the second polymer is coated onto the surface of the catalytic diffusion layer to construct the catalytic layer;
[0032] 3) Dry the electrode obtained in step 2) to obtain the gas diffusion electrode.
[0033] Preferably, it further includes at least one of the following technical features:
[0034] 11) In step 1), the first slurry further includes at least one selected from organic solvents and water;
[0035] 12) In step 1), the solid content of the first slurry is 2% to 20%, such as 2% to 13%, 13% to 15%, 15% to 16%, 16% to 18%, or 18% to 20%;
[0036] 13) In step 1), the pressure of the cold pressing process is 1MPa to 5MPa, such as 1MPa to 3MPa or 3MPa to 5MPa;
[0037] 14) In step 1), the cold pressing time is 1 min to 5 min;
[0038] 15) In step 1), the annealing temperature is 320℃~350℃, such as 320℃~340℃ or 340℃~350℃;
[0039] 16) In step 1), the annealing time is 30 min to 90 min;
[0040] 21) In step 2), the second slurry further includes at least one selected from organic solvents and water;
[0041] 22) In step 2), the solid content of the second slurry is 2% to 20%, such as 2% to 2.4%, 2.4% to 5%, or 5% to 8%;
[0042] 31) In step 3), the drying temperature is 40℃~70℃, such as 40℃~50℃ or 50℃~70℃.
[0043] More preferably, in feature 11), the organic solvent in the first slurry is selected from at least one of methanol, ethanol, ethylene glycol, n-butanol, isopropanol, N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).
[0044] More preferably, in feature 21), the organic solvent in the second slurry is selected from at least one of methanol, ethanol, ethylene glycol, n-butanol, isopropanol, N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).
[0045] A third aspect of the present invention provides the application of the above-described gas diffusion electrode in the electrochemical reduction of carbon dioxide.
[0046] As described above, the present invention has at least one of the following beneficial effects:
[0047] 1) The gas diffusion electrode of this invention has high dispersibility, good stability, and high mechanical strength;
[0048] 2) The porous structure of the catalytic diffusion layer filled with the current collector in the gas diffusion electrode of the present invention includes a first catalytic active material and a first polymer, which can realize dual functions of catalysis and gas diffusion;
[0049] 3) In the gas diffusion electrode of the present invention, the catalyst layer is loaded on the catalytic diffusion layer, including a second catalytically active material and a second polymer, which can realize the catalytic function;
[0050] 4) The method for preparing the gas diffusion electrode of the present invention involves coating a first slurry comprising the first catalytic active material and the first polymer onto the surface of the current collector, followed by cold pressing to uniformly fill the porous structure of the current collector with the first slurry. Through annealing, the first polymer condenses to form a porous structure, creating gas channels that facilitate CO2 diffusion and adsorption; simultaneously, it achieves hydrophobic properties, which is beneficial for constructing a gas-liquid-solid three-phase interface and preventing electrode flooding. The first catalytic active material performs partial catalytic function, reducing the dispersion of the gas diffusion electrode and improving the efficiency of both the gas diffusion electrode and CO2 utilization.
[0051] 5) The method for preparing the gas diffusion electrode of the present invention involves coating a second slurry, comprising a second catalytic active material and a second polymer, onto the surface of a catalytic diffusion layer to construct a catalytic layer. The catalytic layer can adjust the hydrophilicity and hydrophobicity of the gas diffusion electrode surface, construct ion transport channels, and adjust the surface proton concentration by adjusting the type and proportion of the second polymer, thereby controlling the concentration of reactants and products in CO2 reduction. This is beneficial for reducing the occurrence of hydrogen evolution side reactions and water flooding.
[0052] 6) The gas diffusion electrode of the present invention exhibits stable electrochemical performance, with high CO2 reduction selectivity and low overpotential, and good stability. Attached Figure Description
[0053] Figure 1 Scanning electron microscope image of the gas diffusion electrode prepared in Example 1.
[0054] Figure 2 The graph shows the changes in tank voltage and selectivity as a function of current density in the proton exchange membrane electrode structure tested in Example 1.
[0055] Figure 3 The graph shows the voltage and selectivity as a function of current density in Example 1, tested in a flow battery structure.
[0056] Figure 4 The graph shows the change of cell voltage over time during the constant current test of the gas diffusion electrode prepared in Example 1.
[0057] Figure 5 Scanning electron microscope image of the gas diffusion electrode prepared in Example 2.
[0058] Figure 6 This is a scanning electron microscope image of the Ag / C catalyst in Example 3.
[0059] Figure 7 The graph shows the changes in tank voltage and selectivity with current density in the proton exchange membrane electrode structure tested in Example 3. Detailed Implementation
[0060] The present invention is further illustrated below with reference to the embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods and reagents not specified in the following embodiments, unless otherwise stated, were performed or prepared under conventional conditions or conditions recommended by the manufacturer.
[0061] Example 1
[0062] 1g of commercial nano silver, 0.5g of conductive carbon black (Vulcan XC72R) and 0.625g of polytetrafluoroethylene (PTFE) emulsion (60wt%) were dispersed in 12.5mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, a stir bar was added and stirred for 30 minutes to obtain the first slurry with a solid content of 16%.
[0063] The first slurry was uniformly coated onto a 10cm × 10cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0064] 100 mg of commercial nano silver, 100 mg of conductive carbon black (Vulcan XC72R), and 0.8 mL of Nafion solution (5 wt%) were dispersed in 8 mL of water and ethanol solution (water and ethanol volume ratio of 1:1) to prepare a slurry. The slurry was then dispersed in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2.4%.
[0065] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0066] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with an Ag loading of 0.5 mg / cm³. 2 Scanning electron microscope images can be found Figure 1 .
[0067] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0068] The current collector is made of nickel foam with a porous structure;
[0069] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black supported on silver nanoparticles, with a silver nanoparticle loading rate of 66.7%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 8:3. The mass ratio of the catalytic diffusion layer to the current collector is 1:3.
[0070] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black supported on silver nanoparticles, with a silver nanoparticle loading rate of 50%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 3:1. The mass ratio of the catalyst layer to the current collector is 1:25.
[0071] The tensile strength of commonly used carbon paper (Toray TGP-H-060) is 0.05 MPa, while the tensile strength of nickel foam can reach 8–50 MPa, exhibiting better mechanical properties. This gas diffusion electrode can be repeatedly bent without breaking.
[0072] The gas diffusion electrode was applied to CO2 reduction testing in membrane electrode structures and flow battery structures. The cell voltage and selectivity versus current density in the proton exchange membrane electrode structure are shown in the figure below. Figure 2 As shown in the figure, the voltage and selectivity as a function of current density in the flow battery structure are as follows. Figure 3 As shown, all exhibit stable electrochemical performance, with high CO selectivity and low overpotential. The cell voltage change over time during the electrode constant current test is shown in the figure. Figure 4 As shown, it maintains a low tank pressure over 24 hours, exhibiting good stability.
[0073] Example 2
[0074] Take 1g of commercial nano copper, 0.5g of conductive carbon black (Vulcan XC72R) and 0.625g of PTFE emulsion (60wt%) and disperse them in 12.5mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, add a stir bar and stir for 30 minutes to obtain the first slurry with a solid content of 16%.
[0075] The first slurry was uniformly coated onto a 10cm × 10cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0076] 100 mg of commercial nano copper, 100 mg of conductive carbon black (Vulcan XC72R), and 0.8 mL of Nafion solution (5 wt%) were dispersed in 8 mL of water and ethanol solution (water and ethanol volume ratio of 1:1) to prepare a slurry. The slurry was then dispersed in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2.4%.
[0077] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0078] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with a Cu loading of 0.5 mg / cm³. 2 Scanning electron microscope images can be found Figure 5 .
[0079] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0080] The current collector is made of nickel foam with a porous structure;
[0081] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black supported on copper nanoparticles, with a copper nanoparticle loading rate of 66.7%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 8:3. The mass ratio of the catalytic diffusion layer to the current collector is 1:3.
[0082] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black supported on copper nanoparticles, with a copper nanoparticle loading rate of 50%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 3:1. The mass ratio of the catalyst layer to the current collector is 1:25.
[0083] Gas diffusion electrodes were applied to CO2 reduction tests in membrane electrode structures, and all exhibited stable electrochemical performance. At 50 mA cm⁻¹ -2 up to 300mA cm -2 The constant current electrolysis test results are shown in Table 1.
[0084] Table 1
[0085] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO2RR / %]]> <![CDATA[FE H2 / %]]> 50 2.16 54 46 100 2.38 40 60 200 2.67 33 67 300 2.82 32 68
[0086] Example 3
[0087] 40 mg of conductive carbon black (Vulcan XC72R) was dispersed in 50 mL of deionized water and sonicated for 30 min. 20 mL of AgNO3 was then added, followed by glycerol and NaOH, to achieve a final solution concentration of 1 M glycerol and 0.1 M NaOH. The reaction was carried out at room temperature for 24 hours. The precipitate was filtered off, washed three times with water and ethanol, and then vacuum dried at 80 °C for at least 8 hours to obtain the catalytically active material, i.e., the Ag / C catalyst.
[0088] Take 50 mg of the above Ag / C catalyst and disperse it with 21 mg of PTFE emulsion (60 wt%) in 0.5 mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in ultrasound for 1 hour, add a stir bar and stir for 30 min to obtain the first slurry with a solid mass content of 13%.
[0089] The first slurry was uniformly coated onto a 1cm × 2cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0090] Take 20 mg of the above Ag / C catalyst and 80 μL of Nafion solution (5 wt%) and disperse it in 0.8 mL of water and ethanol solution (water and ethanol volume ratio of 1:1) to prepare a slurry. Disperse the slurry in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2.4%.
[0091] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0092] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with an Ag / C loading of 1 mg / cm³. 2 Scanning electron microscope images can be found Figure 6 .
[0093] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0094] The current collector is made of nickel foam with a porous structure;
[0095] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is an Ag / C catalyst with an Ag loading rate of 70%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 8:1. The mass ratio of the catalytic diffusion layer to the current collector is 1:2.
[0096] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is an Ag / C catalyst with an Ag loading rate of 70%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 5:1. The mass ratio of the catalyst layer to the current collector is 1:35.
[0097] The gas diffusion electrode was applied to CO2 reduction testing in a membrane electrode structure. The cell voltage and selectivity as a function of current density in the proton exchange membrane electrode structure are shown in the figure below. Figure 7 As shown, it exhibits stable electrochemical performance, with high CO selectivity and low cell voltage.
[0098] Example 4
[0099] Take 0.2g of commercial nano silver, 0.8g of conductive carbon black (Vulcan XC72R) and 0.5g of polytetrafluoroethylene (PTFE) emulsion (60wt%) and disperse them in 5mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, add a stir bar and stir for 30 minutes to obtain the first slurry with a solid content of 20%.
[0100] The first slurry was uniformly coated onto a 10cm × 10cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0101] Take 20 mg of commercial nano silver, 80 mg of conductive carbon black (Vulcan XC72R), and 32 μL of Nafion solution (5 wt%) and disperse them in 2 mL of NMP solution to prepare a slurry. Disperse the slurry in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 5%.
[0102] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0103] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with an Ag loading of 0.5 mg / cm³. 2 .
[0104] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0105] The current collector is made of nickel foam with a porous structure;
[0106] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black loaded with nano-silver, and the loading rate of nano-silver is 20%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 2:3. The mass ratio of the catalytic diffusion layer to the current collector is 1:3.
[0107] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black supported on silver nanoparticles, with a silver nanoparticle loading rate of 20%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 15:1. The mass ratio of the catalyst layer to the current collector is 1:12.
[0108] Gas diffusion electrodes were applied to CO2 reduction tests in proton exchange membrane electrode structures, and all exhibited stable electrochemical performance. At 50 mA cm⁻¹ -2 up to 400mA cm -2The constant current electrolysis test results are shown in Table 2.
[0109] Table 2
[0110] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO / %]]> <![CDATA[FE H2 / %]]> 50 2.44 62 35 100 2.64 59 41 200 2.99 55 46 300 3.15 47 53 400 3.46 36 64
[0111] Example 5
[0112] 0.8 g of commercial nano silver, 0.2 g of conductive carbon black (Vulcan XC72R), and 90 mg of polytetrafluoroethylene (PTFE) emulsion (60 wt%) were dispersed in 6.4 mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, a stir bar was added and stirred for 30 minutes to obtain the first slurry with a solid content of 15%.
[0113] The first slurry was uniformly coated onto a 10cm×10cm stainless steel mesh, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0114] 80 mg of commercial nano silver, 20 mg of conductive carbon black (Vulcan XC72R), and 127 μL of Nafion solution (5 wt%) were dispersed in 4.9 mL of NMP solution to prepare a slurry. The slurry was then dispersed in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2%.
[0115] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0116] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with an Ag loading of 0.5 mg / cm³. 2 .
[0117] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0118] The current collector is made of stainless steel mesh with a porous structure;
[0119] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black supported on silver nanoparticles, with a silver nanoparticle loading rate of 80%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 15:1. The mass ratio of the catalytic diffusion layer to the current collector is 1:10.
[0120] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black supported on silver nanoparticles, with a silver nanoparticle loading rate of 80%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 15:1. The mass ratio of the catalyst layer to the current collector is 1:48.
[0121] Gas diffusion electrodes were applied to CO2 reduction tests in membrane electrode structures, and all exhibited stable electrochemical performance. At 50 mA cm⁻¹ -2 Up to 200mA cm -2 The constant current electrolysis test results are shown in Table 3.
[0122] Table 3
[0123] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO / %]]> <![CDATA[FE H2 / %]]> 50 2.44 34 67 100 2.66 42 58 200 3.11 30 74
[0124] Example 6
[0125] 0.5g of commercial nano copper, 0.5g of conductive carbon black (Vulcan XC72R) and 0.8g of polytetrafluoroethylene (PTFE) emulsion (60wt%) were dispersed in 6.4mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, a stir bar was added and stirred for 30 minutes to obtain the first slurry with a solid content of 15%.
[0126] The first slurry was uniformly coated onto a 10cm×10cm copper mesh, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0127] Take 50 mg of commercial nano copper, 50 mg of conductive carbon black (Vulcan XC72R) and 127 μL of Nafion solution (5 wt%) and disperse them in 1.4 mL of ethanol and aqueous solution (water and ethanol volume ratio of 1:1) to prepare a slurry. Disperse the slurry in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 8%.
[0128] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0129] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with a Cu loading of 0.5 mg / cm³. 2 .
[0130] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0131] The current collector is made of copper mesh with a porous structure;
[0132] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black supported on copper nanoparticles, with a copper nanoparticle loading rate of 50%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 1:1. The mass ratio of the catalytic diffusion layer to the current collector is 1:4.
[0133] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black supported on copper nanoparticles, with a copper nanoparticle loading rate of 50%. The second polymer is Nafion. The mass ratio of the second catalytic active material to the second polymer is 10:1. The mass ratio of the catalyst layer to the current collector is 1:100.
[0134] Gas diffusion electrodes were applied to CO2 reduction tests in membrane electrode structures, and all exhibited stable electrochemical performance. At 50 mA cm⁻¹ -2 Up to 200mA cm -2 The constant current electrolysis test results are shown in Table 4.
[0135] Table 4
[0136] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO2RR / %]]> <![CDATA[FE H2 / %]]> 50 2.30 54 42 100 2.62 55 40 200 3.02 40 57
[0137] Example 7
[0138] 50 mg Ag2O, 50 mg conductive carbon black (Vulcan XC72R), and 41.6 mg PTFE emulsion (60 wt%) were dispersed in 0.6 mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, a stir bar was added and stirred for 30 minutes to obtain the first slurry with a solid content of 18%.
[0139] The first slurry was uniformly coated onto a 1cm × 2cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0140] Take 10 mg of the above Ag2O catalyst, 10 mg of conductive carbon black (Vulcan XC72R), and 80 μL of Nafion solution (5 wt%) and disperse them in 0.8 mL of water and ethanol solution (water and ethanol volume ratio of 1:1) to prepare a slurry. Disperse the slurry in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2.4%.
[0141] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0142] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode with an Ag₂O loading of 1 mg / cm³. 2 .
[0143] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0144] The current collector is made of nickel foam with a porous structure;
[0145] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is Ag2O supported on conductive carbon black, and the loading rate of Ag2O is 50%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 2:1. The mass ratio of the catalytic diffusion layer to the current collector is 1:3.
[0146] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is Ag2O supported on conductive carbon black, and the loading rate of Ag2O is 50%. The second polymer is Nafion. The mass ratio of the second catalytic active material and the second polymer is 3:1. The mass ratio of the catalyst layer to the current collector is 1:17.
[0147] The gas diffusion electrode was applied to CO2 reduction testing in the membrane electrode structure and exhibited stable electrochemical performance, as shown in Table 5.
[0148] Table 5
[0149] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO / %]]> <![CDATA[FE H2 / %]]> 50 2.47 75 25 100 2.97 70 30
[0150] Example 8
[0151] 1g of cobalt phthalocyanine molecules, 0.5g of conductive carbon black (Vulcan XC72R), and 0.625g of polytetrafluoroethylene (PTFE) emulsion (60wt%) were dispersed in 12.5mL of isopropanol and aqueous solution (isopropanol and water volume ratio of 1:1) to prepare a slurry. After dispersing in an ultrasonic bath for 1 hour, a stir bar was added and stirred for 30 minutes to obtain the first slurry with a solid content of 16%.
[0152] The first slurry was uniformly coated onto a 10cm × 10cm nickel foam, and then cold-pressed at 3MPa for 1 min. It was then placed in a muffle furnace and annealed at 340℃ for 30 min with a heating rate of 2.5℃ / min to construct the catalytic diffusion layer.
[0153] 100 mg of cobalt phthalocyanine molecules, 100 mg of conductive carbon black (Vulcan XC72R), and 0.8 mL of Nafion solution (5 wt%) were dispersed in 8 mL of water and ethanol solution (water and ethanol volume ratio of 1:1) to prepare a slurry. The slurry was then dispersed in an ultrasonic environment for 1 hour to obtain a second slurry with a solid content of 2.4%.
[0154] The second slurry is scraped onto the surface of the catalytic diffusion layer to construct the catalytic layer.
[0155] Then, it was dried in an oven at 50°C for 30 minutes to obtain a gas diffusion electrode, in which the loading of cobalt phthalocyanine molecules was 0.5 mg / cm³. 2 .
[0156] The gas diffusion electrode includes a current collector, a catalytic diffusion layer, and a catalytic layer;
[0157] The current collector is made of nickel foam with a porous structure;
[0158] The catalytic diffusion layer is filled with a porous structure. The catalytic diffusion layer includes a first catalytic active material and a first polymer. The first catalytic active material is conductive carbon black loaded with cobalt phthalocyanine molecules, and the loading rate of cobalt phthalocyanine molecules is 66.7%. The first polymer is polytetrafluoroethylene. The mass ratio of the first catalytic active material to the first polymer is 8:3. The mass ratio of the catalytic diffusion layer to the current collector is 3:8.
[0159] The catalyst layer is supported on the catalytic diffusion layer. The catalyst layer includes a second catalytic active material and a second polymer. The second catalytic active material is conductive carbon black loaded with cobalt phthalocyanine molecules, and the loading rate of cobalt phthalocyanine molecules is 50%. The second polymer is Nafion. The mass ratio of the second catalytic active material and the second polymer is 3:1. The mass ratio of the catalyst layer to the current collector is 1:35.
[0160] The gas diffusion electrode was applied to CO2 reduction testing in the membrane electrode structure and exhibited stable electrochemical performance, as shown in Table 6.
[0161] Table 6
[0162] <![CDATA[Current density / mA cm -2 > Slot pressure / V <![CDATA[FE CO / %]]> <![CDATA[FE H2 / %]]> 50 1.99 56 44 100 2.22 55 45 200 2.57 40 60
[0163] The above embodiments are for illustrating the implementation schemes disclosed in this invention and should not be construed as limiting the invention. Furthermore, various modifications listed herein, as well as variations in the methods and compositions of the invention, will be apparent to those skilled in the art without departing from the scope and spirit of the invention. Although the invention has been specifically described in conjunction with various specific preferred embodiments, it should be understood that the invention should not be limited to these specific embodiments. In fact, various modifications as described above that are obvious to those skilled in the art to obtain the invention should be included within the scope of this invention.
Claims
1. A gas diffusion electrode, characterized in that, Includes current collector, catalytic diffusion layer, and catalytic layer; The current collector has a porous structure; The catalytic diffusion layer fills the porous structure, and the catalytic diffusion layer includes a first catalytically active substance and a first polymer; The catalytic diffusion layer is a catalytic diffusion layer formed by coating a first slurry comprising the first catalytic active substance and the first polymer onto the surface of the current collector, cold pressing, and annealing. The catalyst layer is supported on the catalytic diffusion layer, and the catalyst layer includes a second catalytically active material and a second polymer; The first catalytically active material is selected from at least one of carbon-based supported metals with CO2 catalytic activity, carbon-based supported metal oxides with CO2 catalytic activity, and carbon-based supported molecular catalysts.
2. The gas diffusion electrode as described in claim 1, characterized in that, It also includes at least one of the following technical features: a1) The mass ratio of the catalytic diffusion layer to the current collector is 1:2 to 1:10; a2) The mass ratio of the catalyst layer to the current collector is 1:10 to 1:100; a3) The current collector is selected from at least one of nickel foam, copper foam, stainless steel mesh, copper mesh, nickel mesh, metal-based nano-polypropylene film, and metal-based nano-polytetrafluoroethylene film.
3. The gas diffusion electrode as described in claim 2, characterized in that, In feature a3), the metal base is Ag or Cu nanoparticles.
4. The gas diffusion electrode as described in claim 1, characterized in that, It also includes at least one of the following technical features: b1) The first polymer is selected from at least one of polytetrafluoroethylene and polyvinylidene fluoride; b2) The mass ratio of the first catalytic active substance to the first polymer is 2:3 to 15:1; b3) The second catalytically active material is selected from at least one of the following: carbon-based supported metal with CO2 catalytic activity, carbon-based supported metal oxide with CO2 catalytic activity, carbon-based supported single-atom catalyst with CO2 catalytic activity, and carbon-based supported molecular catalyst. b4) The second polymer is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride and perfluorosulfonic acid; b5) The mass ratio of the second catalytic active substance to the second polymer is 2:3 to 15:
1.
5. The gas diffusion electrode as described in claim 4, characterized in that, It also includes at least one of the following technical features: c1) The metal with CO2 catalytic activity is selected from at least one of Ag, Au, Cu, Sn, Bi and Zn; c2) The metal oxide with CO2 catalytic activity is selected from at least one of Ag, Au, Cu, Sn, Bi and Zn oxides; c3) The carbon substrate is selected from at least one of conductive carbon black, Ketjen black, acetylene black, carbon nanotubes and graphene; c4) The molecular catalyst is selected from at least one of cobalt phthalocyanine, iron phthalocyanine, and nickel phthalocyanine; c5) is selected from at least one of the following: metals with CO2 catalytic activity, metal oxides with CO2 catalytic activity, and molecular catalysts, with a loading rate of 20% to 80%.
6. The method for preparing a gas diffusion electrode according to any one of claims 1 to 5, characterized in that, Includes the following steps: 1) A first slurry comprising the first catalytic active material and the first polymer is coated onto the surface of the current collector, and then subjected to cold pressing and annealing to construct the catalytic diffusion layer filling the porous structure of the current collector; 2) A second slurry comprising the second catalytically active substance and the second polymer is coated onto the surface of the catalytic diffusion layer to construct the catalytic layer; 3) Dry the electrode obtained in step 2) to obtain the gas diffusion electrode.
7. The method for preparing the gas diffusion electrode as described in claim 6, characterized in that, It also includes at least one of the following technical features: 11) In step 1), the first slurry further includes at least one selected from organic solvents and water; 12) In step 1), the solid content of the first slurry is 2%~20% by mass; 13) In step 1), the pressure for cold pressing is 1 MPa to 5 MPa; 14) In step 1), the cold pressing time is 1 min to 5 min; 15) In step 1), the annealing temperature is 320℃~350℃; 16) In step 1), the annealing time is 30 min to 90 min; 21) In step 2), the second slurry further includes at least one selected from organic solvents and water; 22) In step 2), the solid content of the second slurry is 2%~20% by mass; 31) In step 3), the drying temperature is 40℃~70℃.
8. The method for preparing the gas diffusion electrode as described in claim 7, characterized in that, In feature 11), the organic solvent in the first slurry is selected from at least one of methanol, ethanol, ethylene glycol, n-butanol, isopropanol, N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.
9. The method for preparing the gas diffusion electrode as described in claim 7, characterized in that, In feature 21), the organic solvent in the second slurry is selected from at least one of methanol, ethanol, ethylene glycol, n-butanol, isopropanol, N,N-dimethylformamide, N-methylpyrrolidone, and dimethyl sulfoxide.
10. The application of the gas diffusion electrode as described in any one of claims 1 to 5 in the electrochemical reduction of carbon dioxide.
Citation Information
Patent Citations
Method for preparing hydrocarbon-selective gas diffusion electrodes based on copper-containing catalysts
CN107923052A
Gas diffusion electrode for preparing carbon monoxide by electrolyzing carbon dioxide and preparation method of gas diffusion electrode
CN113445064A