A flexible water electrolysis film, a preparation method and application thereof
By preparing porous polylactic acid nanowire conductive polymer films and electrochemically depositing electrocatalytic materials on their surfaces, the problem of poor flexibility of metal substrates was solved, resulting in a larger catalytic surface area and higher electrocatalytic efficiency.
Patent Information
- Application Number
- CN202310990456.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-08
AI Technical Summary
Existing electrocatalytic materials have limited applications due to the poor flexibility and easy corrosion of the metal substrate, and the waste and corrosion of the metal substrate also affect the electrocatalytic efficiency.
Porous polylactic acid nanowire conductive polymer films were prepared by coaxial electrospinning of polypyrrole and polylactic acid solutions, and electrocatalytic materials were electrochemically deposited on their surfaces to form flexible water electrolysis films.
It increases the catalytic surface area, enhances the catalytic performance of the material, reduces the charge transfer resistance, and expands the application range of polymer materials in the field of electrocatalysis.
Smart Images

Figure CN117004976B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of interdisciplinary technology of electrocatalytic metal materials and polymer materials, and more specifically, to a flexible water electrolysis thin film, its preparation method and application. Background Technology
[0002] Hydrogen energy, as a high-energy-density, zero-emission, and renewable green new energy source, is one of the important ways to solve the current energy crisis and environmental pollution. Electrolysis of water to produce hydrogen is simple, easy to build, and has a high energy conversion rate, making it an important pathway for industrial hydrogen production. Commonly used electrocatalysts are mostly precious or transition metals, and their catalyst substrates are also metal, such as sheets, rods, or foams. Since electrocatalysis is a surface reaction, only a very thin surface layer plays a catalytic role, while the much larger metal substrate only serves as support and conductor, resulting in significant waste. During the electrocatalytic reaction, the metal substrate corrodes upon contact with water. This not only causes metal loss but also adversely affects the electrocatalytic efficiency. Furthermore, the poor flexibility of the metal substrate severely limits its application. Existing electrocatalytic materials are mainly synthesized on metal substrates, and therefore, due to the inherent properties of the metal substrate (such as poor flexibility, easy corrosion, and high cost), they cannot be used in large sizes, further limiting their application areas. Summary of the Invention
[0003] In view of the problems existing in the background art, the purpose of the present invention is to provide a flexible water electrolysis thin film, its preparation method and application, which can obtain a larger catalytic surface area and improve the catalytic performance of the material.
[0004] To achieve the above objectives, the present invention provides a method for preparing a flexible water electrolysis film, wherein a synthesized polypyrrole and polylactic acid solution are coaxially electrospun to obtain a conductive polymer film composed of polylactic acid nanowires with a porous polypyrrole structure on the surface; an electrocatalytic material is electrochemically deposited on the surface of the conductive polymer film to obtain a flexible water electrolysis film.
[0005] Optionally, the synthesis method of pyrrole includes the following steps: preparing an aqueous solution of 0.01-0.2M pyrrole and 0.01-0.2M sodium bis(2-ethylhexyl)sulfosuccinate and stirring continuously in an ice-water bath; adding 0.01-0.05M ammonium persulfate solution dropwise to the above solution and continuing to stir for 12-24 hours; centrifuging the mixed solution at 2000-5000 rpm for 5-20 minutes and washing it three times with deionized water; and drying the centrifuged polypyrrole in a vacuum oven at 50-80 degrees Celsius for 12-24 hours.
[0006] Optionally, a polypyrrole hexafluoroisopropanol solution (mass ratio 5-10%) is prepared, magnetically stirred for 2-10 hours, and then filtered with a filter head; a polylactic acid hexafluoroisopropanol solution (mass ratio 5-10%) is prepared and stirred for 2-10 hours; the two solutions are then coaxially electrospun to obtain a conductive polymer film.
[0007] Optionally, coaxial electrospinning can be performed at a voltage of 20 kV and a push rate of 1 mL / h.
[0008] Optionally, the filter head has a pore size of 0.22µm.
[0009] Optionally, the electrocatalytic material is one of nano-iron, cobalt, or nickel particles.
[0010] Optionally, the electrocatalytic material is iron nanoparticles.
[0011] Optionally, the method for electrochemically depositing nano-iron particles on the surface of a conductive polymer film includes the following steps: using a conductive polymer film as the working electrode, a platinum sheet as the counter electrode, and a silver chloride electrode as the reference electrode, depositing the material for 100 to 500 s in a mixed solution of 5–20 mM ferrous chloride + 50–200 mM potassium chloride at -0.8 to -1 V, and then rinsing with deionized water to obtain an electrolyzed water film material.
[0012] The present invention also provides a flexible water electrolysis film prepared by the above-described preparation method.
[0013] The present invention also provides an application of the flexible water electrolysis film prepared by the above preparation method as an electrocatalytic water splitting material.
[0014] The beneficial effects of this invention are as follows:
[0015] Because polymeric thin film materials generally have poor or even non-conductive conductivity and weak bonding with metals, they cannot be directly used as substrates for electrocatalytic reactions. This invention, however, involves coaxial spinning of synthesized polypyrrole and polylactic acid (PLA) using electrospinning technology to obtain a conductive polymeric thin film composed of PLA nanowires with a porous polypyrrole structure. Electrocatalytic materials are then electrochemically deposited on the surface of this film, thereby achieving the preparation of a flexible water electrolysis thin film. This invention uses a flexible polymeric material thin film as a substrate, expanding the application of polymeric materials in the field of electrocatalysis. Attached Figure Description
[0016] Figure 1 The results of scanning electron microscopy (SEM) tests on samples obtained from Comparative Example 1, Comparative Example 2, and Example 1 are shown below. Figure 1 a, Figure 1 b and Figure 1 c.
[0017] Figure 2 The following are linear sweep voltammetric curves of the samples obtained in Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3 in 1M KOH electrolyte. Figure 2 a represents the electrocatalytic oxygen evolution performance curve. Figure 2 b represents the electrocatalytic hydrogen evolution performance curve.
[0018] Figure 3 The Nyquist impedance curves of Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3 in 1M KOH electrolyte are shown. Detailed Implementation
[0019] To make the above-mentioned objects, features and advantages of the invention more apparent and understandable, the specific embodiments of the invention are described in detail below.
[0020] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0021] According to the preparation method of the flexible water electrolysis film of the present invention, the synthesized polypyrrole (PPy) and polylactic acid (PLLA) solution are coaxially electrospun to obtain a conductive polymer film composed of polylactic acid nanowires with porous polypyrrole structure on the surface; an electrocatalytic material is electrochemically deposited on the surface of the conductive polymer film to obtain a flexible water electrolysis film.
[0022] Electrospinning is a mature polymer film preparation technology capable of producing large-sized films. However, it is difficult to produce highly flexible and conductive polymer films. This invention, however, uses a mixture of PLLA and PPy for coaxial spinning to obtain a polymer film composed of conductive nanowires. This retains the flexibility of the PLLA polymer film while providing a porous conductive structure on the surface, laying the foundation for subsequent electrochemical deposition. Electrochemical deposition, a type of chemical deposition technique, is a commonly used method for preparing electrocatalytic materials. However, it is often limited by the morphology of the metal substrate, making it difficult to obtain a large specific surface area. This invention electrochemically deposits nanoparticles on a substrate with porous nanowires on the initial surface, achieving a larger catalytic surface area compared to ordinary metal substrates, thereby improving the catalytic performance of the material.
[0023] In the preparation method of the flexible electrolytic water film according to the present invention, the synthesis method of pyrrole may include the following steps: preparing an aqueous solution of 0.01-0.2M pyrrole and 0.01-0.2M sodium bis(2-ethylhexyl)sulfosuccinate and stirring continuously in an ice-water bath; adding 0.01-0.05M ammonium persulfate solution dropwise to the above solution and continuing to stir for 12-24 hours; centrifuging the mixed solution at 2000-5000 rpm for 5-20 minutes and washing it three times with deionized water; and drying the centrifuged polypyrrole in a vacuum oven at 50-80 degrees Celsius for 12-24 hours.
[0024] In the preparation method of the flexible electrolytic water film according to the present invention, a polypyrrole hexafluoroisopropanol solution (mass ratio of 5-10%) can be prepared, magnetically stirred for 2-10 hours and then filtered with a filter head; a polylactic acid hexafluoroisopropanol solution (mass ratio of 5-10%) can be prepared and stirred for 2-10 hours; the above two solutions are coaxially electrospun to obtain a conductive polymer film.
[0025] In the preparation method of the flexible electrolytic water film according to the present invention, coaxial electrospinning can be carried out under the conditions of voltage 20kV and pushing speed 1mL / h.
[0026] In the preparation method of the flexible electrolytic water film according to the present invention, the pore size of the filter head can be 0.22 μm.
[0027] In the preparation method of the flexible water electrolysis film according to the present invention, the electrocatalytic material may be one of nano-iron, cobalt, or nickel particles. Nano-iron particles are preferred.
[0028] In the preparation method of the flexible electrolytic water film according to the present invention, the method of electrochemically depositing nano-iron particles on the surface of the conductive polymer film may include the following steps: using the conductive polymer film as the working electrode, a platinum sheet as the counter electrode, and a silver chloride electrode as the reference electrode, depositing for 100 to 500 s in a mixed solution of 5 to 20 mM ferrous chloride + 50 to 200 mM potassium chloride under conditions of -0.8 to -1 V, and rinsing with deionized water to obtain the electrolytic water film material.
[0029] The flexible electrolytic water film according to the present invention is prepared by the above-described preparation method.
[0030] The application of the flexible water electrolysis film according to the present invention is as an electrocatalytic water splitting material.
[0031] The following describes the flexible water electrolysis film of the present invention, its preparation method, and its application in detail with reference to specific embodiments.
[0032] Example 1
[0033] (1) Synthesis of polypyrrole: Prepare an aqueous solution of 0.1M pyrrole and 0.15M sodium bis(2-ethylhexyl)sulfosuccinate and stir continuously in an ice-water bath. Add 0.025M ammonium persulfate solution dropwise to the above solution and continue stirring for 24 hours. Then centrifuge the mixed solution at 4000 rpm for 10 minutes and wash it three times with deionized water. Place the centrifuged polypyrrole in a vacuum oven at 60 degrees Celsius and dry it for 24 hours.
[0034] (2) Preparation of conductive polymer films: First, a polypyrrole hexafluoroisopropanol solution (mass ratio 10%) was prepared, magnetically stirred for 6 h, and then filtered through a 0.22 μm filter. Subsequently, a PLLA hexafluoroisopropanol solution (mass ratio 10%) was prepared and stirred for 6 h. The two solutions were then coaxially electrospun at a voltage of 20 kV and a spinning rate of 1 mL / h to obtain conductive polymer films.
[0035] (3) Preparation of water electrolysis film material: The above-mentioned conductive polymer film is used as the working electrode, the platinum sheet is used as the counter electrode, and the silver chloride electrode is used as the reference electrode. It is deposited in a mixed solution of 10mM ferrous chloride + 100mM potassium chloride at -1V for 300s. After rinsing with deionized water, the water electrolysis film material is obtained.
[0036] Example 2
[0037] The difference from Example 1 is that deposition was carried out for 300 s at -1V in a mixed solution of 10 mM nickel chloride and 100 mM potassium chloride.
[0038] Example 3
[0039] The difference from Example 1 is that deposition was carried out for 300 s at -0.8 V in a mixed solution of 10 mM ferrous chloride and 100 mM potassium chloride.
[0040] Comparative Example 1
[0041] A PLLA solution in hexafluoroisopropanol (10% by mass) was prepared and stirred for 6 hours. PLLA films were then obtained by coaxial electrospinning at a voltage of 20 kV and a spinning speed of 1 mL / h.
[0042] Comparative Example 2
[0043] The conductive polymer film prepared by steps (1) and (2) of Example 1.
[0044] Performance Tests and Results
[0045] 1. The samples obtained from Comparative Example 1, Comparative Example 2, and Example 1 were subjected to scanning electron microscopy testing. The test results are as follows: Figure 1As shown, the scanning electron microscope images of Comparative Example 1, Comparative Example 2, and Example 1 are respectively... Figure 1 a, Figure 1 b and Figure 1 c.
[0046] Figure 1 a is a SEM image of PLLA electrospinning in Comparative Example 1. As can be seen from the SEM image of Comparative Example 2, the conductive polymer film uses PLLA nanowires as a carrier, with porous polypyrrole PLLA nanowires coated on the surface, forming a conductive polymer film composed of nanowires. This solves the problem of polypyrrole being difficult to mold, such as... Figure 1 As shown in b. In Example 1, after electrochemically depositing iron, a layer of nano-iron particles was coated onto the surface of the porous polypyrrole structure, thereby increasing the catalytic reaction area for water electrolysis, as shown in Figure 1. Figure 1 As shown in c.
[0047] 2. Electrolysis performance test: Linear sweep voltammetry and impedance test were performed respectively.
[0048] Figure 2 The following are linear sweep voltammetry curves of the samples obtained in Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3 in 1M KOH electrolyte. Figure 2 (a) shows the electrocatalytic oxygen evolution performance curve. Figure 2 (b) shows the electrocatalytic hydrogen evolution performance curve.
[0049] Figure 3 The Nyquist impedance curves of the samples obtained from Comparative Example 1, Comparative Example 2, Example 1, Example 2, and Example 3 in 1M KOH electrolyte are shown.
[0050] like Figure 2 As shown in the linear sweep voltammetry test, it can be seen that, regardless of whether it is the oxygen evolution reaction (OER) or the hydrogen evolution reaction (HER) in the water electrolysis process, the current curve of the non-conductive PLLA film in Comparative Example 1 shows almost no change with the increase of voltage. The curve of the conductive polymer film in Comparative Example 2 shows only a slight change. In Examples 1 and 3, due to the deposition of nano-iron particles, the catalytic curves change significantly. In Example 1, OER and HER are at 10 mA / cm². 2 The overpotentials at current densities decreased to 295mV and 110mV, respectively. In Example 3, the OER and HER were at 10mA / cm². 2 The overpotentials at the current densities decreased to 315 mV and 138 mV, respectively, both exhibiting good electrocatalytic effects. In Example 2, due to the deposition of nickel nanoparticles, the catalytic curves changed significantly, with OER and HER showing good performance at 10 mA / cm². 2The overpotentials at the current densities decreased to 307 mV and 124 mV, respectively, demonstrating good electrocatalytic performance. This indicates that Comparative Examples 1 and 2 had no catalytic effect, while the water splitting effect was significantly improved after the deposition of nanoparticles. This is partly because the porous nanowire films provided by the PLLA and PPy substrates have a large specific surface area, increasing the catalytic area for water splitting; and partly because the nanoparticles deposited on the surface greatly reduce the charge transfer resistance of the catalytic material. Figure 3 As shown, PLLA exhibits typical insulator properties. After coating with polypyrrole, the charge transfer resistance is reduced to several hundred ohms, and after depositing nanoparticles, the charge transfer resistance is further reduced to tens of ohms.
[0051] While specific embodiments of the invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art should understand that modifications can be made to the above embodiments without departing from the scope and spirit of the invention. The scope of the invention is defined by the appended claims.
Claims
1. A method for preparing a flexible water electrolysis thin film, characterized in that, The synthesized polypyrrole and polylactic acid solutions were coaxially electrospun to obtain a conductive polymer film composed of polylactic acid nanowires with a porous polypyrrole structure on the surface; an electrocatalytic material, which is one of nano-iron, cobalt, and nickel particles, was electrochemically deposited on the surface of the conductive polymer film to obtain a flexible water electrolysis film.
2. The method for preparing the flexible water electrolysis film according to claim 1, characterized in that, The synthesis method of pyrrole includes the following steps: preparing an aqueous solution of 0.01~0.2 M pyrrole and 0.01~0.2 M sodium bis(2-ethylhexyl)sulfosuccinate and stirring continuously in an ice-water bath; adding 0.01~0.05 M ammonium persulfate solution dropwise to the above solution and continuing to stir for 12~24 h; centrifuging the mixed solution at 2000~5000 rpm for 5~20 minutes and washing it three times with deionized water; and drying the centrifuged polypyrrole in a vacuum oven at 50~80 degrees for 12~24 h.
3. The method for preparing the flexible water electrolysis film according to claim 2, characterized in that, Prepare a polypyrrole hexafluoroisopropanol solution, stir magnetically for 2-10 h, and then filter it with a filter head; prepare a polylactic acid hexafluoroisopropanol solution and stir for 2-10 h; then coaxially electrospin the two solutions to obtain a conductive polymer film.
4. The method for preparing the flexible water electrolysis film according to claim 3, characterized in that, Coaxial electrospinning was performed at a voltage of 20 kV and a push speed of 1 mL / h.
5. The method for preparing the flexible water electrolysis film according to claim 3, characterized in that, The filter head has a pore size of 0.22 μm.
6. The method for preparing the flexible water electrolysis thin film according to claim 1, characterized in that, The electrocatalytic material is nano-iron particles.
7. The method for preparing the flexible water electrolysis film according to claim 6, characterized in that, The method for electrochemically depositing nano-iron particles on the surface of a conductive polymer film includes the following steps: using a conductive polymer film as the working electrode, a platinum sheet as the counter electrode, and a silver chloride electrode as the reference electrode, depositing the material for 100 to 500 s in a mixed solution of 5 to 20 mM ferrous chloride and 50 to 200 mM potassium chloride at -0.8 to -1 V, and rinsing with deionized water to obtain an electrolyzed water film material.
8. The flexible electrolyzed water film prepared by the preparation method according to any one of claims 1-7.
9. The application of the flexible water electrolysis film prepared by the preparation method according to any one of claims 1-7 as an electrocatalytic water splitting material.