A device with micro-nano optical structure on the surface and a preparation method thereof
By fabricating and transferring micro- and nano-optical structures, including surface plasmon resonance structures and metal nanocaps, on the end face of optical fibers, the problems of detection limit and transfer difficulty of plasmon resonance sensors on the end face of optical fibers were solved, and a high signal-to-noise ratio sensing effect was achieved.
Patent Information
- Application Number
- CN202210493993.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-04-29
AI Technical Summary
The detection limit of existing fiber end-face plasmon sensors is difficult to further reduce, and the transfer of their basic building blocks from the substrate is difficult, so their performance needs to be improved.
A device with a surface having a micro/nano optical structure is provided, including a support and a micro/nano optical structure bonded thereto. The micro/nano optical structure includes a surface plasmon resonance structure and a metal nanocap, which is transferred from a substrate to the support by an adhesive, and optionally combined with a Fabry-Perot microcavity to improve coupling efficiency.
The transfer and integration of three-dimensional micro-nano optical structures have been realized, which has improved the signal-to-noise ratio of fiber end-face plasmon sensing, especially the signal-to-noise ratio of refractive index sensing by an order of magnitude.
Smart Images

Figure CN117008230B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of optics, sensing and micro / nano fabrication, and relates to a device with micro / nano optical structures on its surface and its fabrication method. Background Technology
[0002] Surface plasmon polaritons (SPPs) are surface waves formed by the coupling of surface charges and optical fields on a metal surface. The resonance conditions of these surface waves, such as wavelength, intensity, and emission angle, vary with the refractive index of their surrounding environment. Therefore, surface plasmon resonance (SPR) is used to measure the refractive index of the environment and has been widely studied and applied in the fields of refractive index, molecular, and acoustic field sensing. How to combine SPR with optical fibers to conveniently excite SPR and perform sensing using fiber optic waveguide technology, thereby obtaining novel applications including point-of-care medical diagnosis and agricultural product testing, has been a pursuit for many years. In particular, the technology of integrating sensor devices onto the end face of an optical fiber can fully leverage the convenience and speed of optical fiber detection. Such sensors can be directly inserted into trace biological or medical samples or read molecular, optical, and acoustic information in a minimally invasive manner. The SPP microcavity, constructed from a nanogroove array on a metal thin film, and its integration into a sensor device formed on the end face of a single-mode fiber, represents the fiber end-face plasmon resonance sensing technology with the highest signal-to-noise ratio (SNR) to date. Its refractive index detection SNR is two orders of magnitude higher or more than that of other reported fiber end-face plasmon resonance sensing technologies. This SPP microcavity can be constructed from a central coupling region and adjacent reflective regions (US 11,022,752 B2), or from a periodic structure and embedded defect structures (ZL201610754423.1, US11,137,353 B2). Integration of both structures with the single-mode fiber end face can achieve a refractive index of 10-1. -6 The noise equivalent detection limit is in the RIU range.
[0003] While the aforementioned devices have significantly reduced the detection limit of fiber endface plasmon sensing, their fundamental building block—the nanogroove array on a metal thin film—is a two-dimensional structure, limiting further reductions in the detection limit. Furthermore, their fabrication process, based on peeling and precisely transferring a metal thin film with nanogrooves from a large-area substrate to the fiber endface, is currently limited to the transfer of two-dimensional metal thin film structures.
[0004] Therefore, how to provide a new device with micro-nano optical structures on the surface and its fabrication method, including a new optical fiber device with micro-nano optical structures on the end face and its fabrication method, in order to further reduce the detection limit of this type of surface plasmon sensing technology, and to develop a transfer fabrication process for three-dimensional or quasi-three-dimensional micro-nano structures from the substrate to the support surface, has become an important technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a device and a method for fabricating a device with a micro-nano optical structure on its surface, in order to solve the problems of difficulty in transferring the basic building blocks of optical fiber end face or other end face plasmon sensing from the substrate and the need to improve performance in the prior art.
[0006] To achieve the above and other related objectives, the present invention provides a device with a surface having a micro / nano optical structure, comprising:
[0007] The support has a bearing surface;
[0008] A micro / nano optical structure is incorporated into the bearing surface, the micro / nano optical structure comprising a surface plasmon resonance structure and a metal nanocap.
[0009] The surface plasmon polariton resonant structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film, wherein the nano-openings are filled with a non-metallic medium.
[0010] The metal nanocap protrudes from the side of the metal film away from the support, facing the nano opening, and is attached to the side of the non-metallic medium away from the support.
[0011] The non-metallic medium protrudes from the side of the metal film opposite to the support, and the metal nanocap completely or partially covers the protruding portion of the non-metallic medium; or the non-metallic medium is recessed or flush with the side of the metal film opposite to the support, and the distance between the side of the non-metallic medium opposite to the support and the side of the metal film opposite to the support is less than 10 nm.
[0012] When light waves are incident on the micro-nano optical structure from the side facing the support, they can excite surface plasmon resonances along the side of the metal thin film facing away from the support.
[0013] Optionally, the nano-opening includes at least one of nanopores and nanogrooves, and the sidewalls of the nano-opening are vertical or inclined.
[0014] Optionally, the material of the metal thin film includes one or more of gold, silver, copper and aluminum, the material of the metal nanocap includes one or more of gold, silver, copper and aluminum, and an adhesion layer is provided at the interface between the metal nanocap and the non-metallic medium.
[0015] Optionally, the support includes an optical fiber, the bearing surface is a planar optical fiber end face, the micro / nano optical structure is bonded to the optical fiber end face, and the metal film is parallel to the optical fiber end face.
[0016] Optionally, the surface plasmon resonance structure includes a central region and a surrounding region. The array of nano-apertures divides the metal film located in the central region into a first periodic structure and the metal film located in the surrounding region into a second periodic structure. The periods of the first periodic structure and the second periodic structure are different. The first periodic structure is aligned with the fiber core.
[0017] Optionally, the surface plasmon resonance structure includes a periodic structure and a defect structure embedded in the periodic structure, wherein the array of nano-apertures divides the metal thin film into the periodic structure and the defect structure embedded in the periodic structure, the defect structure disrupts the local periodicity of the periodic structure, and the defect structure is aligned with the fiber core.
[0018] Optionally, the optical fiber is a single-mode fiber at the operating wavelength.
[0019] Optionally, the micro / nano optical structure further includes a Fabry-Perot microcavity located between the bearing surface and the surface plasmon resonance structure. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance. The Fabry-Perot microcavity includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is parallel to the first substrate.
[0020] Optionally, the second substrate includes a thin film made of a metallic material, and an adhesion layer is provided at the interface between the metallic thin film and the dielectric layer.
[0021] Optionally, the material of the dielectric layer includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials, and the thickness of the dielectric layer ranges from 5 nm to 100 μm.
[0022] The present invention also provides a method for fabricating a device with a surface having micro / nano optical structures as described in any of the above claims, comprising the following steps:
[0023] A substrate is provided, and the micro / nano optical structure is formed on the substrate, wherein the metal thin film and the metal nanocap are in direct contact with the substrate;
[0024] The support is provided, and the side of the micro / nano optical structure facing away from the substrate is bonded to the bearing surface of the support by an adhesive.
[0025] The support, together with the micro / nano optical structure, is peeled off from the substrate, so that the micro / nano optical structure is transferred from the substrate to the bearing surface of the support.
[0026] Optionally, forming the micro / nano optical structure on the substrate includes the following steps:
[0027] A first metal thin film layer is formed on the substrate;
[0028] A mask layer is formed and patterned on the first metal thin film layer. The patterned mask layer is used as a mask to etch the first metal thin film layer to obtain a nano-opening that penetrates the first metal thin film layer, and the etching is carried into the substrate to obtain a recessed structure of a predetermined depth.
[0029] Remove the mask layer;
[0030] A second metal thin film layer is formed, which covers the surface of the first metal thin film layer and the bottom surface of the recessed structure;
[0031] A non-metallic medium is formed, which fills the nano-opening.
[0032] Optionally, before forming the non-metallic medium, the step of forming an adhesion layer on the surface of the second metal thin film layer is further included.
[0033] Optionally, the substrate material includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials.
[0034] This invention also provides a method for fabricating a device with micro / nano optical structures on its surface, comprising the following steps:
[0035] A substrate is provided, on which a micro / nano optical structure is formed. The micro / nano optical structure includes a surface plasmon resonance structure (SPR) and a metal nanocap. The SPR includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film facing the substrate, directly opposite the nano-openings, and is attached to the side of the non-metallic medium facing the substrate. The non-metallic medium protrudes from the side of the metal thin film facing the substrate, and the metal nanocap completely or partially covers the protruding portion of the non-metallic medium; or the non-metallic medium is recessed or flush with the side of the metal thin film facing the substrate, and the distance between the side of the non-metallic medium facing the substrate and the side of the metal thin film facing the substrate is less than 10 nm. Both the metal thin film and the metal nanocap are in direct contact with the substrate.
[0036] The support is provided, and the side of the micro / nano optical structure facing away from the substrate is bonded to the bearing surface of the support by an adhesive.
[0037] The support, together with the micro / nano optical structure, is peeled off from the substrate, and the micro / nano optical structure is transferred from the substrate to the support surface of the support.
[0038] Remove the nanocap.
[0039] Optionally, the material of the metal thin film includes one or more of gold, silver, copper and aluminum, the material of the metal nanocap includes one or more of gold, silver, copper and aluminum, an adhesion layer is provided at the interface between the metal nanocap and the non-metallic medium, and the material of the substrate includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials and organic materials.
[0040] Optionally, the micro / nano optical structure further includes a Fabry-Perot microcavity, which includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is located on the side of the first substrate away from the substrate and parallel to the first substrate. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance.
[0041] The present invention also provides a device having a micro / nano optical structure on its surface, comprising:
[0042] The support has a bearing surface;
[0043] A micro-nano optical structure is incorporated into the bearing surface, the micro-nano optical structure comprising a surface plasmon resonance structure and a Fabry-Perot microcavity;
[0044] The surface plasmon polariton resonant structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film.
[0045] The Fabry-Perot microcavity is located between the support surface and the surface plasmon resonance structure. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance. The Fabry-Perot microcavity includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is located on the side of the first substrate facing the support and is parallel to the first substrate.
[0046] When light waves are incident on the micro-nano optical structure from the side facing the support, they can excite surface plasmon resonances along the side of the metal thin film facing away from the support.
[0047] Optionally, the support includes optical fibers;
[0048] Optionally, the optical fiber is a single-mode fiber at the operating wavelength.
[0049] Optionally, the second substrate includes a thin film made of a metallic material.
[0050] As described above, the device with a micro / nano optical structure on its surface according to the present invention includes a support and a micro / nano optical structure bonded to the support surface. The micro / nano optical structure includes a surface plasmon resonance structure and a metal nanocap. The surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film opposite to the support, faces the nano-openings, and is attached to the side of the non-metallic medium opposite to the support. When light waves are incident from the side of the micro / nano optical structure facing the support towards the micro / nano optical structure, surface plasmon resonances can be excited along the side of the metal thin film opposite to the support. This invention combines a metal nanocap with a metal thin film having nano-openings to fabricate a three-dimensional micro / nano optical structure containing the metal thin film on a substrate with low adhesion to the metal. This allows for the peeling and transfer of the three-dimensional structure from the substrate to a support. Simultaneously, it enables resonant coupling between light waves incident from the support and surface plasmon polaritons (SIPs) on the metal thin film. The metal nanocap can be retained or removed after transfer as needed. Furthermore, this three-dimensional micro / nano optical structure may include a Fabry-Perot microcavity disposed between the support and the SIP resonant structure. Through the Fano resonance between the SIP resonant structure and the Fabry-Perot microcavity, the coupling efficiency between the incident light waves and the SIPs on the metal thin film can be improved, achieving high signal-to-noise ratio SIP sensing, including refractive index sensing, molecular sensing, and acoustic field sensing. Compared to a two-dimensional metal thin film structure, the signal-to-noise ratio of single-mode fiber end-face SIP refractive index sensing with the Fabry-Perot microcavity three-dimensional structure can be improved by an order of magnitude. Furthermore, the preparation method of the present invention can also achieve the integration of various other complex three-dimensional micro / nano optical structures with fiber end faces. Attached Figure Description
[0051] Figure 1 The diagram shown is a schematic representation of the device with micro / nano optical structures on its surface according to the present invention.
[0052] Figure 2 Displayed as Figure 1 Enlarged view of the area indicated by the dashed box.
[0053] Figure 3 The diagram shown illustrates a surface plasmon resonance structure used in the device with micro / nano optical structures on its surface according to the present invention.
[0054] Figure 4 Displayed as Figure 3 The electron microscope image of the surface plasmon resonance structure shown shows the boundary between the central region and the adjacent region.
[0055] Figure 5 The diagram shown is a schematic of another surface plasmon resonance structure used in the device with micro / nano optical structures on the surface according to the present invention.
[0056] Figure 6 The diagram shows a method for fabricating a device with a micro / nano optical structure on its surface according to the present invention, in which a substrate is provided and a first metal thin film layer is formed on the substrate.
[0057] Figure 7 The diagram shows a method for fabricating a device with a micro / nano optical structure on the surface according to the present invention, in which a mask layer is formed on the first metal thin film layer, the mask layer is patterned, and the first metal thin film layer and the substrate are etched.
[0058] Figure 8 The diagram shown illustrates the removal of the mask layer during the fabrication method of the device with a micro / nano optical structure on the surface according to the present invention.
[0059] Figure 9 The diagram shows a second metal thin film layer and a first adhesion layer being formed sequentially in the fabrication method of the device with a micro / nano optical structure on the surface according to the present invention.
[0060] Figure 10 The diagram shows a method for fabricating a device with a micro / nano optical structure on its surface according to the present invention, in which a non-metallic dielectric and a Fabry-Perot microcavity dielectric layer are formed, and a second adhesion layer and a third metal thin film layer are sequentially formed on the Fabry-Perot microcavity dielectric layer.
[0061] Figure 11 The diagram shows the process of peeling and transferring the micro-nano optical structure from the substrate in the fabrication method of the device with a surface having a micro-nano optical structure according to the present invention.
[0062] Figure 12 The image shown is a microscope image of the micro-nano optical structure transfer process in the fabrication method of the device with micro-nano optical structures on the surface according to the present invention.
[0063] Figure 13 The image shown is an atomic force microscope image of the nanocap after the transfer of the micro-nano optical structure in the fabrication method of the device with a surface having a micro-nano optical structure according to the present invention.
[0064] Figure 14 The diagram shows a schematic of an experimental apparatus for measuring the refractive index of a liquid using a device with a micro / nano optical structure on its surface, as described in this invention.
[0065] Figure 15 The normalized reflectance spectra of the end face of the device having a micro / nano optical structure as described in this invention are shown when inserted into methanol, water, acetone, ethanol, and isopropanol.
[0066] Figure 16 This shows the variation of each resonant wavelength with respect to the refractive index.
[0067] Figure 17 The results show the changes in the wavelength of surface plasmon resonance as a function of concentration when the end face of the device with a micro / nano optical structure of the present invention is inserted into a phosphate buffer solution of bovine serum albumin at different concentrations.
[0068] Figure 18 Displayed as baseline noise.
[0069] Component designation explanation
[0070] 10 Support
[0071] 20 Surface plasmon polariton resonant structures
[0072] 201 Metal Thin Film Layer
[0073] 2010 First Metal Thin Film Layer
[0074] 2011 Second Metal Thin Film Layer
[0075] 202 Non-metallic media
[0076] 21. Middle Area
[0077] 22. Surrounding area
[0078] 23 Periodic Structures
[0079] 24 Defect Structure
[0080] 30 Metal Nanocaps
[0081] 40 Fabry-Perot microcavities
[0082] 401 First substrate
[0083] 402 Dielectric Layer
[0084] 403 Second substrate
[0085] 4030 Third Metal Thin Film Layer
[0086] 404 First Adhesion Layer
[0087] 405 Second Adhesion Layer
[0088] 50 Adhesive layer
[0089] 60 substrate
[0090] 70 mask layers Detailed Implementation
[0091] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0092] Please see Figures 1 to 18 It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0093] Example 1
[0094] This embodiment provides a device with a surface having micro / nano optical structures, such as Figures 1 to 2 The diagram shows a schematic and a partial enlarged view of the device, including a support 10 and a micro / nano optical structure. The support 10 has a bearing surface, and the micro / nano optical structure is integrated into the bearing surface. It includes a surface plasmon resonance structure 20 and a metal nanocap 30. The surface plasmon resonance structure 20 includes a metal thin film 201 and nano-openings or an array of nano-openings formed in the metal thin film 201. The nano-openings are filled with a non-metallic medium 202. The metal nanocap 30 protrudes from the side of the metal thin film 201 facing away from the support 10, directly opposite the nano-openings, and is attached to the side of the non-metallic medium 202 facing away from the support 10. When light waves are incident on the micro / nano optical structure from the side facing the support 10, surface plasmon resonances can be excited along the side of the metal thin film 201 facing away from the support 10.
[0095] As an example, the non-metallic medium 202 protrudes from the side of the metallic film 201 opposite to the support 10 (e.g., Figure 2 As shown, the metal nanocap 30 completely or partially covers the protruding portion of the non-metallic medium 202. In this embodiment, the distance between the side of the non-metallic medium 202 facing away from the support 10 and the side of the metal film 201 facing away from the support 10 is less than 200 nm. In a preferred example, the distance between the side of the non-metallic medium 202 facing away from the support 10 and the side of the metal film 201 facing away from the support 10 is 8 nm, that is, the spacing between the metal nanocap 30 and the metal film 201 is 8 nm.
[0096] As an example, the non-metallic dielectric 202 may also be recessed or flush with the side of the metal film facing away from the support (not shown), wherein the non-metallic dielectric 202 is recessed on the side of the metal film facing away from the support, i.e., the nanocap 30 is partially embedded in the nano-opening. In this embodiment, the distance between the side of the non-metallic dielectric 202 facing away from the support 10 and the side of the metal film 201 facing away from the support 10 is less than 10 nm.
[0097] As an example, the nano-aperture includes at least one of nanopores and nanogrooves. Specifically, a nanopore refers to a nano-aperture in the plane dimension of the metal thin film where the longest side and the shortest side passing through the center of the nano-aperture are equal in length or nearly equal in length, and its shape includes, but is not limited to, circles, triangles, squares, and hexagons. A nanogrooves refer to a nano-aperture in the plane dimension of the metal thin film where the longest side passing through the center of the nano-aperture is much larger than the shortest side, and its shape is such as a strip.
[0098] As an example, the length of the shortest side passing through the center of the nano-aperture in the plane dimension of the metal thin film ranges from 5 to 200 nm. For example, if it is a circular nanopore, the length of the shortest side refers to the diameter of the circular nanopore; if it is a square nanopore, the length of the shortest side refers to the side length of the square nanopore; and if it is a rectangular nanogroove, the length of the shortest side refers to the width of the short side of the rectangular nanogroove. In this embodiment, the nano-aperture is a rectangular nanogroove with a short side width of 50 nm, and the nano-aperture is filled with SiO2 dielectric.
[0099] As an example, the sidewalls of the nano-openings are vertical or inclined.
[0100] As an example, the support 10 includes an optical fiber, the bearing surface is a planar optical fiber end face, the micro-nano optical structure is bonded to the optical fiber end face, and the metal thin film 201 is parallel to the optical fiber end face.
[0101] As an example, the optical fiber is a single-mode fiber at the working wavelength, and the angle between the fiber end face and the fiber axis is in the range of 80° to 100°, further 82° to 98°, preferably 88° to 92°.
[0102] As an example, such as Figure 3As shown, the surface plasmon polariton resonant structure 20 includes a central region 21 and a side region 22 surrounding the central region 21. The array of nano-apertures divides the metal film located in the central region 21 into a first periodic structure and the metal film located in the side region 22 into a second periodic structure. The periods of the first periodic structure and the second periodic structure are different. The position of the central region 21 is aligned with the fiber core.
[0103] As an example, such as Figure 4 The image shown is an electron microscope image of the surface plasmon resonance structure 20, depicting the boundary between the central region 21 and the adjacent region 22. The period P1 of the first periodic structure in the central region 21 is 645 nm, approximately equal to the wavelength of the surface plasmon resonance on the metal thin film. The period P2 of the second periodic structure in the adjacent region 22 is 315 nm, approximately equal to half the wavelength of the surface plasmon resonance on the metal thin film. When light is incident from the core of the optical fiber, the central region 21 couples with the incident optical fiber waveguide to form surface plasmons (on the gold thin film), and the adjacent region 22 reflects these surface plasmons.
[0104] It is important to note that Figure 4 The number of periods presented does not perfectly match the above description and is for illustrative purposes only. When the device with the micro-nano optical structure on its surface is immersed in water, its material and structural properties enable it to generate a surface plasmon polariton resonance corresponding to a free-space wavelength of approximately 850 nm. The optical fiber described above is a single-mode fiber at this wavelength. In specific embodiments, "approximately equal to" in this invention indicates that the numerical deviation is within ±10%.
[0105] In some other embodiments, such as Figure 5As shown, the surface plasmon resonance structure includes a periodic structure 23 and a defect structure 24 embedded in the periodic structure. The nano-apertures divide the metal thin film into the periodic structure 23 and the defect structure 24 embedded in the periodic structure 23. The defect structure 24 disrupts the local periodicity of the periodic structure 23 and is aligned with the fiber core. The nano-apertures penetrate the upper and lower surfaces of the metal thin film, dividing it into multiple metal thin film units. Some of these units are periodically arranged to form the periodic structure 23. These periodically arranged metal thin film units are polygonal, including triangles, squares, rectangles, and hexagons. Another portion of the metal thin film units are embedded within the periodically arranged metal thin film units to form the defect structure 24. The surface plasmon polaritons along the metal thin film can resonate in the defect structure or in the defect structure and its vicinity. The incident light wave is coupled to the surface plasmon polaritons through the first-order Fourier component of the spatial Fourier transform of the periodic structure, and the second-order Fourier component is used to restrict the oscillation of the surface plasmon polaritons in the space near the defect structure.
[0106] In some other embodiments, the surface plasmon resonance structure 20 may also employ other periodic structures or microcavity structures, without regard to... Figure 3 or Figure 5 The presentation is limited.
[0107] As an example, the material of the metal thin film 201 includes, but is not limited to, one or more of gold, silver, copper, and aluminum, with a thickness ranging from 5 to 200 nm. The material of the metal nanocap includes, but is not limited to, one or more of gold, silver, copper, and aluminum, with a thickness ranging from 5 to 200 nm. Specifically, in this embodiment, the metal thin film is a gold film with a thickness of 55 nm, and the metal nanocap is a gold nanocap with a thickness of 5 nm.
[0108] As an example, an adhesion layer is provided at the interface between the metal nanocap 30 and the non-metallic medium 202. The material of the adhesion layer includes, but is not limited to, one or more of titanium, chromium, and nickel. In this embodiment, the adhesion layer is a titanium layer, and the thickness of the adhesion layer is 2 nm.
[0109] As an example, the surface plasmon resonance spectrum of the surface plasmon resonance structure 20 shifts with the change in refractive index sensed by the surface plasmon resonance structure 20, and is used to sense changes in the refractive index of the environment, the binding of molecules on the structure, and to sense sound fields through integration with acoustically sensitive materials.
[0110] As an example, the micro / nano optical structure further includes a Fabry-Perot microcavity 40, which is located between the bearing surface and the surface plasmon resonance structure 20. The surface plasmon resonance structure 20 and the Fabry-Perot microcavity 40 are coupled to form a Fano resonance. The Fabry-Perot microcavity includes a first substrate 401, a second substrate 403, and a dielectric layer 402 located between the first substrate 401 and the second substrate 403. The first substrate 401 is composed of the surface plasmon resonance structure 20, and the second substrate 403 is parallel to the first substrate 401.
[0111] Specifically, by coupling the surface plasmon resonant structure 20 and the Fabry-Perot microcavity 40, the coupling efficiency between the fiber waveguide and the surface plasmon resonator can be improved, thereby enhancing the signal-to-noise ratio of the refractive index sensing.
[0112] As an example, the second substrate 403 includes a thin film made of a metal material, such as one or more of gold film, silver film, copper film and aluminum film. The thickness of the second substrate 403 ranges from 5 to 200 nm. In this embodiment, the second substrate 403 is selected as a gold film with a thickness of 20 nm.
[0113] As an example, the material of the dielectric layer 402 includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials, and the thickness of the dielectric layer 402 ranges from 5 nm to 100 μm. In this embodiment, the dielectric layer 402 is selected as a SiO2 layer with a thickness of 230 nm.
[0114] As an example, a first adhesion layer 404 is provided at the interface between the metal thin film 201 and the dielectric layer 402, and a second adhesion layer 405 is provided at the interface between the second substrate 403 and the dielectric layer 402. The adhesion layers are used to improve the adhesion between the dielectric layer 402 and the first substrate 401 and the second substrate 403. The material of the adhesion layer includes, but is not limited to, one or more of titanium, chromium, and nickel. In this embodiment, the adhesion layer is a titanium layer, and the thickness of the adhesion layer is 2 nm.
[0115] As an example, an adhesive layer 50 is provided between the support 10 and the second substrate 403, the adhesive layer 50 being used to bond the support 10 and the micro / nano optical structure. In this embodiment, the adhesive layer 50 is a UV-curable adhesive.
[0116] In summary, the device with a micro / nano optical structure on its surface provided in this embodiment includes a support and a micro / nano optical structure bonded to the support surface. The micro / nano optical structure includes a surface plasmon resonance structure and a metal nanocap. The surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film opposite to the support, faces the nano-openings, and is attached to the side of the non-metallic medium opposite to the support. When light waves are incident on the micro / nano optical structure from the side facing the support, they can excite surface plasmon resonances along the side of the metal thin film opposite to the support. The micro / nano optical structure may further include a Fabry-Perot microcavity disposed between the support and the surface plasmon resonance structure. Through the Fano resonance between the surface plasmon resonance structure and the Fabry-Perot microcavity, the coupling efficiency between the incident light wave and the surface plasmons on the metal thin film can be improved, realizing surface plasmon sensing with high signal-to-noise ratio, including refractive index sensing, molecular sensing, and acoustic field sensing. Among these, compared with the two-dimensional metal thin film structure, the signal-to-noise ratio of surface plasmon refractive index sensing at the end face of a single-mode fiber with a three-dimensional Fabry-Perot microcavity structure can be improved by an order of magnitude.
[0117] Example 2
[0118] This embodiment provides a method for fabricating a device with a surface having micro-nano optical structures, used to fabricate the device with a surface having micro-nano optical structures as described in Embodiment 1. The method includes the following steps:
[0119] S1: A substrate is provided, and the micro / nano optical structure is formed on the substrate, wherein the metal thin film and the metal nanocap are in direct contact with the substrate;
[0120] S2: Provide the support body, and use an adhesive to bond the side of the micro / nano optical structure away from the substrate to the bearing surface of the support body;
[0121] S3: Peel the support along with the micro / nano optical structure from the substrate, so that the micro / nano optical structure is transferred from the substrate to the bearing surface of the support.
[0122] As an example, forming the micro / nano optical structure on the substrate includes the following steps:
[0123] (1) As Figure 6 As shown, a substrate 60 is provided, on which a first metal thin film layer 2010 is formed.
[0124] As an example, the substrate 60 material includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials and organic materials. Considering the requirements for substrate rigidity and surface nano-smoothness, this embodiment preferably uses a quartz glass substrate.
[0125] As an example, the first metal thin film layer 2010 has low adhesion to the substrate 60. The material of the first metal thin film layer 2010 includes, but is not limited to, one or more of gold, silver, copper and aluminum. In this embodiment, the first metal thin film layer 2010 is a gold thin film layer, which can be formed by electron beam evaporation or other suitable methods.
[0126] (2) Figure 7 As shown, a mask layer 70 is formed and patterned on the first metal thin film layer 2010. The first metal thin film layer 2010 is etched using the patterned mask layer 70 as a mask to obtain a nano-opening penetrating the first metal thin film layer 2010, and etched into the substrate 60 to obtain a recessed structure of a predetermined depth.
[0127] As an example, the mask layer 70 includes, but is not limited to, a polymer layer and a photoresist layer. Specifically, in this embodiment, the mask layer 70 is selected as a polymethyl methacrylate (PMMA) layer, which can be formed by spin coating or other suitable methods.
[0128] As an example, the mask layer 70 is etched using electron beam lithography to form an array pattern of nano-openings. The first metal thin film layer 2010 is etched using argon ion beam etching or other suitable methods with the patterned mask layer 70 as a mask. The speed and time of argon ion beam etching are controlled to etch through the first metal thin film layer 2010 and extend into the substrate 60, forming a recessed structure with a depth of about 15 nm in the substrate 60.
[0129] As an example, the sidewalls of the nano-openings can be made vertical or tilted by adjusting the etching parameters as needed.
[0130] (3) Figure 8 As shown, the mask layer 70 is removed.
[0131] As an example, the mask layer 70 may be removed by oxygen plasma cleaning or other suitable methods.
[0132] (4) Figure 9 As shown, a second metal thin film layer 2011 is formed, which covers the surface of the first metal thin film layer 2010 and the bottom surface of the recessed structure.
[0133] As an example, the material of the second metal thin film layer 2011 includes, but is not limited to, one or more of gold, silver, copper, and aluminum. In this embodiment, the second metal thin film layer 2011 is a gold thin film layer, which can be formed by electron beam evaporation or other suitable methods.
[0134] (5) Figure 10 As shown, a non-metallic medium 202 is formed, which fills the nano-opening.
[0135] Specifically, the second metal thin film layer 2011 within the recessed structure in the substrate constitutes the metal nanocap 30.
[0136] As an example, before forming the non-metallic medium 202, the method further includes forming a first adhesion layer 404 on the surface of the second metal thin film layer 2011. The first adhesion layer 404 is used to increase the adhesion between the non-metallic medium 202 and the second metal thin film layer 2011. In this embodiment, the first adhesion layer 404 is formed by electron beam evaporation.
[0137] As an example, when the micro / nano optical structure further includes the Fabry-Perot microcavity 40, the first substrate 401 of the Fabry-Perot microcavity 40 is composed of the surface plasmon resonance structure 20, and the metal thin film 201 of the surface plasmon resonance structure 20 is composed of the first metal thin film layer 2010 and the second metal thin film layer 2011 located on the surface of the first metal thin film layer 2010. Forming the Fabry-Perot microcavity 40 further includes the following steps: Figure 10 As shown, a dielectric layer 402 is formed on the Fabry-Perot microcavity 40, and a second adhesion layer 405 and a third metal thin film layer 4030 are sequentially formed on the dielectric layer 402 of the Fabry-Perot microcavity. The third metal thin film layer 4030 constitutes the second substrate 403 of the Fabry-Perot microcavity 40.
[0138] As an example, the dielectric layer 402 can be formed simultaneously with the non-metallic dielectric 202 or formed in stages.
[0139] As an example, the dielectric layer 402 is formed by plasma-enhanced chemical vapor deposition at a temperature of 65°C, and the second adhesion layer 405 is formed by electron beam evaporation.
[0140] As an example, step S2, which involves bonding the side of the micro / nano optical structure away from the substrate 60 to the bearing surface of the support 10 using an adhesive, includes the following steps:
[0141] (1) Apply an adhesive to the side of the bearing surface or the micro / nano optical structure away from the substrate 60.
[0142] As an example, the adhesive is cured using ultraviolet light, and the adhesive is cured under ultraviolet light irradiation. In this embodiment, the adhesive is methyl acrylate, which is transparent to the light wavelength used for sensing, and its ultraviolet curing wavelength range is 100–400 nm, with a curing light intensity of 1–2000 J / cm². 2 The curing time is 5–600 s, preferably, the curing wavelength is around 320 nm, and the curing light intensity is 100 J / cm². 2 The curing time is 300 seconds. In this embodiment, an ultraviolet light source is selected, with a curing light center wavelength of 320 nm and a maximum irradiation power of 2000 J / cm². 2 .
[0143] (2) Adjust the position of the support 10 so that the bearing surface is aligned with the position of the micro-nano optical structure and is in contact with it through the adhesive.
[0144] As an example, the substrate 60 (quartz glass) is a transparent substrate, and the support 10 is an optical fiber. The method for aligning the end face of the optical fiber with the micro / nano optical structure includes: observing and aligning the position of the optical fiber end face with the micro / nano optical structure from the side of the substrate 60 without the micro / nano optical structure. Specifically, on the side of the substrate 60 without the micro / nano optical structure, a microscopic system is constructed using lenses and imaging elements to display a magnified image of the optical fiber end face and the micro / nano optical structure. The position of the optical fiber end face and the micro / nano optical structure is adjusted and aligned based on the displayed image.
[0145] In some other examples, the method of aligning the fiber endface with the micro / nanostructure includes: injecting broadband light into the fiber, the broadband light propagating along the fiber and exiting from the fiber endface, then being reflected by the micro / nanostructure and returning into the fiber; moving the relative position of the fiber and the micro / nanostructure and measuring the spectrum of the reflected light during the movement; and comparing the spectrum of the reflected light with the expected reflection spectrum under perfect alignment to determine whether alignment is achieved. Specifically, broadband light is injected into the fiber using a broadband light source (e.g., a superluminescent diode), the broadband light propagating along the fiber, passing through a fiber optic directional coupler, and then exiting from the fiber endface. The broadband light is then reflected by the micro / nano optical structure and returns into the fiber. The reflected light passes through the fiber optic directional coupler and enters a spectrometer. The relative position of the fiber and the micro / nanostructure is moved and the spectrum of the reflected light during the movement is measured. The spectrum of the reflected light is measured by the spectrometer, and the alignment of the fiber endface and the metal micro / nanostructure can be determined and adjusted by comparing the spectrum of the reflected light with the expected reflection spectrum under perfect alignment.
[0146] Specifically, the alignment method between the fiber end face and the micro / nano optical structure shall be operated according to the actual situation and is not limited to this embodiment.
[0147] (3) Irradiate the adhesive with adhesive curing light through the substrate from the side of the substrate 60 without the micro-nano optical structure to cure it.
[0148] As an example, such as Figure 11 The diagram shows a schematic of step S3 in which the support 10, together with the micro / nano optical structure, is peeled off from the substrate 60, and the micro / nano optical structure is transferred from the substrate to the bearing surface of the support 10.
[0149] As an example, such as Figure 12 The image shown is an optical micrograph of the micro / nano optical structure during the transfer process. The support is an optical fiber, the bearing surface is the end face of the optical fiber, the micro / nano optical structure is disk-shaped and has been transferred to the end face of the optical fiber, and the surface plasmon resonance structure and nanocap are shown as a shadowed area located in the center of the disk. Figure 12 The image includes the micro / nano optical structure of the optical fiber and its end face (lower right of the image), the mirror image of the micro / nano optical structure of the optical fiber and its end face in the substrate (upper right of the image), and the position of the micro / nano optical structure on the substrate before transfer, which appears as a dark disk-shaped area (middle of the image). Figure 13 The image shown is an atomic force microscope image of the micro / nano optical structure after it has been transferred to the support surface of the support, demonstrating the nanocap array.
[0150] It is important to emphasize that the non-metallic medium 202 filling the nano-apertures prevents adhesive from entering the nano-apertures during the transfer process, thus affecting the peeling efficiency of the micro / nano optical structure from the substrate 60. The nanocap 30 is crucial for forming a low-bonding interface between the micro / nano optical structure and the substrate 60. For example, the nanocap 30 is made of gold, a noble metal. The bonding force between noble metals and many substrate materials (such as SiO2) largely originates from van der Waals forces, resulting in low bonding strength, which facilitates the peeling of the micro / nano optical structure from the substrate 60. Without the nanocap 30, the non-metallic medium deposited in the nano-apertures would be firmly bonded to the substrate, preventing the transfer from being completed. Furthermore, while effectively reducing the bonding force between the micro / nano optical structure and the substrate to facilitate transfer, the nanocap 30 of this invention still retains the characteristic of surface plasmon polaritons resonating and tunneling through the nano-apertures to the metal thin film, thereby achieving coupling between surface plasmon resonance and incident light waves from the support direction. Based on this micro-nano optical structure and fabrication method, it is possible to peel off a three-dimensional structure containing a metal thin film from a planar substrate and transfer it to the end face of an optical fiber, and to achieve resonant tunneling coupling between the optical fiber waveguide and the plasmon polaritons on the other side of the metal thin film. At the same time, based on the integration of the three-dimensional micro-nano optical structure (such as the Fabry-Perot microcavity 40) on the end face of the optical fiber, the surface plasmon sensing of the optical fiber end face can have an unprecedentedly high signal-to-noise ratio.
[0151] Example 3
[0152] This embodiment uses a device with a micro / nano optical structure on its surface, prepared in Example 2, to perform a refractive index measurement experiment. In a specific example, the support is an optical fiber, which is a single-mode fiber at the working wavelength. The micro / nano optical structure includes a surface plasmon resonance structure, a Fabry-Perot microcavity, and a metal nanocap. The surface plasmon resonance structure includes a central region and surrounding regions. The central region is aligned with the fiber core. The array of nano-apertures divides the metal film in the central region into a first periodic structure with a period of 645 nm and the metal film in the surrounding regions into a second periodic structure with a period of 315 nm. The nano-apertures are rectangular nanogrooves with a short side width of 50 nm. The nano-apertures are filled with SiO2 dielectric, which protrudes from the side of the metal film facing away from the optical fiber. The distance between the side of the SiO2 dielectric facing away from the optical fiber and the side of the metal film 201 facing away from the optical fiber is 8 nm. The metal film is a 55 nm thick gold film, and the metal nanocap is a 5 nm thick gold nanocap. A 2 nm thick titanium adhesion layer is provided at the interface between the metal nanocap and the non-metallic dielectric. The second substrate is a 20 nm thick gold film, and the dielectric layer is a 230 nm thick SiO2 layer. A 2 nm thick titanium adhesion layer is provided between the metal film and the dielectric layer, and a 2 nm thick titanium adhesion layer is provided between the second substrate and the dielectric layer. The second substrate and the end face of the optical fiber are bonded with UV-curable adhesive.
[0153] As an example, such as Figure 14 The diagram shows an experimental setup for measuring the refractive index of a liquid using a device with a micro / nano optical structure on its surface, as described in this invention. The single-mode fiber used in the experiment operates at a wavelength of 780–970 nm, and the light source is a super-luminescent diode (SLD), a broadband light source. The light output from the light source is guided into the liquid to be tested through a 50%:50% fiber optic directional coupler, and the reflected signal is then guided through the same coupler to a CCD fiber optic spectrometer for analysis.
[0154] As an example, five liquids—methanol, water, acetone, ethanol, and isopropanol—were tested, and their normalized reflectance spectra are shown below. Figure 15As shown, without the Fabry-Perot microcavity, directly coupling the surface plasmon resonance structure with the fiber waveguide (US 11,022,752B2, ZL201610754423.1, US 11,137,353B2) will only result in a shallow surface plasmon resonance reflection valley in the fiber waveguide's reflection spectrum. This means the coupling efficiency between the fiber waveguide and the surface plasmon resonance microcavity is very limited; simulation results show the valley depth is no more than about 15%. However, in this embodiment, by coupling the surface plasmon resonance structure with the Fabry-Perot microcavity to form a Fano resonance, a resonance valley with a depth of up to about 55% is obtained, along with a resonance peak of about 46%. This indicates a significant improvement in the coupling efficiency between the fiber waveguide and the surface plasmon resonance. By corresponding their respective resonance wavelengths with the refractive indices of the solutions, we can obtain... Figure 16 The scatter plot (experimental value) of the resonant wavelength versus refractive index shows that the resonant wavelength changes linearly with respect to the refractive index. The sensitivity obtained after linear fitting is 411 nm RIU. -1 .
[0155] As an example, the end face of the device with micro / nano optical structures on its surface was also immersed in phosphate buffered saline (PBS) solutions of different concentrations of bovine serum albumin (BSA). The wavelength of the surface plasmon resonance (SPR) was measured as a function of concentration using the same method described above. The physical adsorption of BSA molecules on the sensor surface was read in real time by observing the change in the SPR wavelength. Specifically, the BSA concentration was increased sequentially from 10 ng / mL to 100 μg / mL, increasing tenfold each time. Simultaneously, the sample reciprocated along the optical fiber at a speed of 80 mm / s. The measurement results are as follows: Figure 17 As shown, a concentration of 10 ng / mL can be measured. The baseline noise of the surface plasmon resonance wavelength over time is shown in the figure. Figure 18 As shown, the noise equivalent detection limit for 1 second integration is calculated using the signal-to-noise ratio (SNR) to be 1.9 × 10⁻⁶. - 7 RIU is about an order of magnitude lower than the best reported level to date.
[0156] Furthermore, the pressure in the environment surrounding the fiber end face can be measured by observing the changes in the refractive index or geometric parameters of the material near the fiber end face as a function of pressure. For example, the pressure can originate from sound waves, ultrasound, or infrasound, and the material can be an adhesive or other substance between the micro / nano optical structure and the fiber end face, or a substance attached to the surface of a metal film or the fiber end face.
[0157] Example 4
[0158] In Embodiment 2, after the micro / nano optical structure is peeled off from the substrate, the nanocap 30 is retained within the micro / nano optical structure. However, the nanocap can also be removed as needed to more smoothly excite surface plasmon resonances along the side of the metal thin film 201 facing away from the support 10. This embodiment provides a method for fabricating a device with a micro / nano optical structure on its surface, comprising the following steps:
[0159] S1: A substrate is provided, and a micro / nano optical structure is formed on the substrate. The micro / nano optical structure includes a surface plasmon resonance structure and a metal nanocap. The surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film facing the substrate, directly opposite the nano-openings, and is attached to the side of the non-metallic medium facing the substrate. The non-metallic medium protrudes from the side of the metal thin film facing the substrate, and the metal nanocap completely or partially covers the protruding portion of the non-metallic medium. Alternatively, the non-metallic medium is recessed or flush with the side of the metal thin film facing the substrate, and the distance between the side of the non-metallic medium facing the substrate and the side of the metal thin film facing the substrate is less than 10 nm. Both the metal thin film and the metal nanocap are in direct contact with the substrate.
[0160] S2: Provide the support body, and use an adhesive to bond the side of the micro / nano optical structure away from the substrate to the bearing surface of the support body;
[0161] S3: Peel the support along with the micro / nano optical structure from the substrate, so that the micro / nano optical structure is transferred from the substrate to the support surface of the support;
[0162] S4: Remove the nanocap.
[0163] As an example, methods for removing the nanocaps may include grinding, ultrasonic vibration, adhesion removal, or peeling.
[0164] As an example, the material of the metal thin film includes one or more of gold, silver, copper and aluminum, and the material of the metal nanocap includes one or more of gold, silver, copper and aluminum.
[0165] As an example, an adhesion layer is provided at the interface between the metal nanocap and the non-metallic medium, and the substrate material includes one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials.
[0166] As an example, the micro / nano optical structure further includes a Fabry-Perot microcavity, which includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is located on the side of the first substrate away from the substrate and parallel to the first substrate. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance.
[0167] As an example, an adhesion layer is provided at the interface between the metal thin film and the dielectric layer, and an adhesion layer is provided at the interface between the second substrate and the dielectric layer.
[0168] Example 5
[0169] This embodiment provides a device with a micro / nano optical structure on its surface, which can be fabricated using the fabrication method in Embodiment 4 or other suitable fabrication methods. The device with a micro / nano optical structure includes a support and a micro / nano optical structure. The support has a bearing surface, and the micro / nano optical structure is attached to the bearing surface. The micro / nano optical structure includes a surface plasmon resonance structure and a Fabry-Perot microcavity.
[0170] Specifically, the surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film; the Fabry-Perot microcavity is located between the support surface and the surface plasmon resonance structure, and the surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance. The Fabry-Perot microcavity includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is located on the side of the first substrate facing the support and is parallel to the first substrate. When light waves are incident from the side of the micro / nano optical structure facing the support towards the micro / nano optical structure, surface plasmon resonances can be excited along the side of the metal thin film facing away from the support.
[0171] As an example, the support includes an optical fiber, which is a single-mode fiber at the operating wavelength.
[0172] As an example, the second substrate includes a thin film made of a metallic material.
[0173] In the device with a micro / nano optical structure on the surface in this embodiment, the micro / nano optical structure includes a surface plasmon resonance structure and a Fabry-Perot microcavity, but does not include a metal nanocap, which can more smoothly excite the surface plasmon resonance along the side of the metal film away from the support.
[0174] In summary, the device with a micro / nano optical structure on its surface according to the present invention includes a support and a micro / nano optical structure bonded to the support surface. The micro / nano optical structure includes a surface plasmon resonance structure and a metal nanocap. The surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film opposite to the support, faces the nano-openings, and is attached to the side of the non-metallic medium opposite to the support. When light waves are incident on the micro / nano optical structure from the side facing the support, surface plasmon resonances can be excited along the side of the metal thin film opposite to the support. This invention combines a metal nanocap with a metal thin film having nano-openings to fabricate a three-dimensional micro / nano optical structure containing the metal thin film on a substrate with low adhesion to the metal. This allows for the peeling and transfer of the three-dimensional structure from the substrate to a support. Simultaneously, it enables resonant coupling between light waves incident from the support and surface plasmon polaritons (SIPs) on the metal thin film. The metal nanocap can be retained or removed after transfer as needed. Furthermore, this three-dimensional micro / nano optical structure may include a Fabry-Perot microcavity disposed between the support and the SIP resonant structure. Through the Fano resonance between the SIP resonant structure and the Fabry-Perot microcavity, the coupling efficiency between the incident light waves and the SIPs on the metal thin film can be improved, achieving high signal-to-noise ratio SIP sensing, including refractive index sensing, molecular sensing, and acoustic field sensing. Compared to a two-dimensional metal thin film structure, the signal-to-noise ratio of single-mode fiber end-face SIP refractive index sensing with the Fabry-Perot microcavity three-dimensional structure can be improved by an order of magnitude. Furthermore, the preparation method of this invention can also achieve the integration of various other complex three-dimensional micro / nano optical structures with fiber end faces. Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial application value.
[0175] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A device having a micro- and nano-optical structure on a surface, characterized in that, include: The support has a bearing surface; A micro / nano optical structure is incorporated into the bearing surface, the micro / nano optical structure comprising a surface plasmon resonance structure and a metal nanocap. The surface plasmon polariton resonant structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film, wherein the nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal film away from the support, facing the nano opening, and is attached to the side of the non-metallic medium away from the support. The non-metallic medium protrudes from the side of the metal film opposite to the support, and the metal nanocap completely or partially covers the protruding portion of the non-metallic medium; or the non-metallic medium is recessed or flush with the side of the metal film opposite to the support, and the distance between the side of the non-metallic medium opposite to the support and the side of the metal film opposite to the support is less than 10 nm. When light waves are incident on the micro-nano optical structure from the side facing the support, they can excite surface plasmon resonances along the side of the metal film away from the support. The support includes an optical fiber, the bearing surface is a planar optical fiber end face, the micro-nano optical structure is bonded to the optical fiber end face, and the metal film is parallel to the optical fiber end face. The metal thin film is composed of a first metal thin film layer and a second metal thin film layer located on the surface of the first metal thin film layer. The second metal thin film layer covers the side of the first metal thin film layer facing the optical fiber and covers the side of the non-metallic medium facing away from the optical fiber. The portion of the second metal thin film layer facing the nano-opening forms the metal nanocap. The micro / nano optical structure further includes a Fabry-Perot microcavity located between the bearing surface and the surface plasmon resonance structure. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance. The Fabry-Perot microcavity includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is parallel to the first substrate.
2. The device with micro- and nano-optical structures on the surface according to claim 1, characterized in that: The metal nanocap is removed so that the micro / nano optical structure does not include the metal nanocap.
3. The device with micro- and nano-optical structures on the surface according to claim 1, characterized in that: The nano-opening includes at least one of nanopores and nanogrooves, and the sidewalls of the nano-opening are vertical or inclined.
4. The device with a micro / nano optical structure on its surface according to claim 1, characterized in that: The metal thin film is made of one or more of gold, silver, copper and aluminum, and the metal nanocap is made of one or more of gold, silver, copper and aluminum. An adhesion layer is provided at the interface between the metal nanocap and the non-metallic medium.
5. The device with a surface having a micro / nano optical structure according to claim 1, characterized in that: The surface plasmon polariton resonant structure includes a central region and a surrounding region. The array of nano-apertures divides the metal film located in the central region into a first periodic structure and the metal film located in the surrounding region into a second periodic structure. The periods of the first periodic structure and the second periodic structure are different. The first periodic structure is aligned with the fiber core.
6. The device with a surface having a micro / nano optical structure according to claim 1, characterized in that: The surface plasmon polariton resonant structure includes a periodic structure and a defect structure embedded in the periodic structure. The array of nano-apertures divides the metal thin film into the periodic structure and the defect structure embedded in the periodic structure. The defect structure disrupts the local periodicity of the periodic structure and is aligned with the fiber core.
7. The device with a surface having a micro / nano optical structure according to claim 1, characterized in that: The optical fiber is a single-mode fiber at the operating wavelength.
8. The device with a surface having a micro / nano optical structure according to claim 1, characterized in that: An adhesion layer is provided at the interface between the metal thin film and the dielectric layer, and the second substrate includes a thin film made of a metal material.
9. The device with a micro / nano optical structure on its surface according to claim 1, characterized in that: The dielectric layer is made of one or more of the following materials: metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials. The thickness of the dielectric layer ranges from 5 nm to 100 mm.
10. A method for fabricating a device with a micro / nano optical structure on its surface, characterized in that, Includes the following steps: A substrate is provided, and a micro / nano optical structure is formed on the substrate. The micro / nano optical structure includes a surface plasmon resonance structure and a metal nanocap. The surface plasmon resonance structure includes a metal thin film and nano-openings or an array of nano-openings formed in the metal thin film. The nano-openings are filled with a non-metallic medium. The metal nanocap protrudes from the side of the metal thin film facing the substrate, directly opposite the nano-openings, and is attached to the side of the non-metallic medium facing the substrate. The non-metallic medium protrudes from the side of the metal thin film facing the substrate, and the metal nanocap completely or partially covers the protruding portion of the non-metallic medium. Alternatively, the non-metallic medium is recessed or flush with the side of the metal thin film facing the substrate, and the distance between the side of the non-metallic medium facing the substrate and the side of the metal thin film facing the substrate is less than 10 nm; both the metal thin film and the metal nanocap are in direct contact with the substrate. A support is provided, and the side of the micro / nano optical structure facing away from the substrate is bonded to the support surface of the support by an adhesive. The support, together with the micro / nano optical structure, is peeled off from the substrate, and the micro / nano optical structure is transferred from the substrate to the support surface of the support. Remove the metal nanocap; The metal thin film is composed of a first metal thin film layer and a second metal thin film layer located on the surface of the first metal thin film layer. The second metal thin film layer covers the side of the first metal thin film layer facing the support and covers the side of the non-metallic medium facing away from the support. The portion of the second metal thin film layer facing the nano-opening forms the metal nanocap.
11. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 10, characterized in that: After the micro / nano optical structure is peeled off from the substrate, the metal nanocap is not removed so that the metal nanocap is retained in the micro / nano optical structure.
12. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 10 or 11, characterized in that: The metal thin film is made of one or more of gold, silver, copper and aluminum, the metal nanocap is made of one or more of gold, silver, copper and aluminum, an adhesion layer is provided at the interface between the metal nanocap and the non-metallic medium, and the substrate is made of one or more of metal oxides, metal nitrides, silicon dioxide, semiconductor materials and organic materials.
13. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 10 or 11, characterized in that: The micro / nano optical structure further includes a Fabry-Perot microcavity, which includes a first substrate, a second substrate, and a dielectric layer located between the first substrate and the second substrate. The first substrate is composed of the surface plasmon resonance structure, and the second substrate is located on the side of the first substrate away from the substrate and parallel to the first substrate. The surface plasmon resonance structure and the Fabry-Perot microcavity are coupled to form a Fano resonance.
14. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 10 or 11, characterized in that, Forming the micro / nano optical structure on the substrate includes the following steps: A first metal thin film layer is formed on the substrate; A mask layer is formed and patterned on the first metal thin film layer. The patterned mask layer is used as a mask to etch the first metal thin film layer to obtain a nano-opening that penetrates the first metal thin film layer, and the etching is carried into the substrate to obtain a recessed structure of a predetermined depth. Remove the mask layer; A second metal thin film layer is formed, which covers the surface of the first metal thin film layer and the bottom surface of the recessed structure; A non-metallic medium is formed, which fills the nano-opening.
15. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 14, characterized in that: Before forming the non-metallic medium, the method further includes the step of forming an adhesion layer on the surface of the second metal thin film layer.
16. The method for fabricating a device with a micro / nano optical structure on its surface according to claim 10 or 11, characterized in that: The substrate material includes one or more of the following: metal oxides, metal nitrides, silicon dioxide, semiconductor materials, and organic materials.
Citation Information
Patent Citations
Optical fibers having metallic micro / nano-structure on end-facet, and fabrication method, and application method thereof
US11022752B2