A methacrylate-based polymer electrolyte, and a preparation method and application thereof
By using methacrylate-based polymer electrolytes in lithium-ion batteries, the problems of low polymerization conversion rate and poor stability have been solved, resulting in improved performance of lithium-ion batteries with high energy density and high safety.
Patent Information
- Application Number
- CN202311042073.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-17
AI Technical Summary
The energy density, performance, and safety of existing lithium-ion batteries are insufficient to meet the requirements of high energy density and high performance. Solid polymer electrolytes prepared by in-situ curing methods have problems such as low polymerization conversion rate, high residual monomer content, poor oxidation stability, and insufficient cycle stability.
A polymer electrolyte with high polymerization conversion rate is generated by using polymer monomers composed of methacrylate, urea and fluoroalkyl groups in a lithium-ion battery through an in-situ solidification reaction. Porous support materials, lithium salts, solvents and initiators are added.
It improves the stability and safety of polymer electrolytes, enhances the stability of the electrode/electrolyte interface, inhibits lithium dendrite growth, and improves the cycle stability and safety performance of batteries, making it suitable for high-voltage, high-energy-density lithium-ion batteries.
Smart Images

Figure CN117013064B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery electrolyte technology, specifically to a methacrylate-based polymer electrolyte, its preparation method, and its application. Background Technology
[0002] With the continuous growth of the new energy industry, especially the current demand for higher energy density and performance from the electric vehicle industry for lithium-ion batteries, the energy density, performance, and safety of traditional lithium-ion batteries are far from meeting these requirements. Therefore, the industry has begun to seek battery systems with higher energy density, such as using high-nickel ternary cathodes and silicon-carbon anodes. However, currently commercially available high-energy-density lithium-ion batteries often use flammable liquid carbonate electrolytes, which are inherently unstable and prone to rapid capacity decay, even posing safety hazards such as fire and explosion. To simultaneously improve the safety and energy density of lithium-ion batteries, academia and industry have proposed a series of optimization schemes, including replacing traditional electrolyte solvents with high-performance flame-retardant electrolytes and replacing liquid electrolytes with solid electrolytes. However, flame-retardant electrolytes, being inherently liquid, can still burn at high temperatures and release harmful gases. All-solid-state electrolytes, due to their high interfacial impedance, poor ion transport capabilities, and incompatibility with current production lines, still face many key technical challenges before industrialization and are currently difficult to mass-produce.
[0003] In-situ curing methods for preparing solid polymer electrolytes have attracted widespread attention from academia and industry due to their high processability and production line compatibility, high energy density, high interfacial compatibility, and better safety. However, current solid polymer electrolytes prepared by in-situ curing methods suffer from the following problems: low in-situ polymerization conversion rate, a large amount of residual monomers after curing, low oxidative stability of the prepared electrolyte, and poor cycle stability of the assembled battery, indicating significant room for performance improvement. Therefore, developing methacrylate-based polymer precursors with higher stability and better electrochemical performance for the commercial application of high-safety and high-energy-density lithium-ion batteries prepared by in-situ curing methods is of great significance. Summary of the Invention
[0004] To address the problems existing in the background technology, the present invention provides a methacrylate-based polymer electrolyte, its preparation method and application. The methacrylate-based polymer electrolyte has a high polymerization conversion rate, a wide electrochemical window, good cycle performance and good safety, and can be applied to battery systems such as high-voltage lithium-ion batteries, high-energy-density lithium-ion batteries and high-safety lithium-ion batteries.
[0005] The technical solution of the present invention to solve the above-mentioned technical problems is as follows:
[0006] In a first aspect, the present invention provides a methacrylate-based polymer electrolyte, comprising a polymer matrix. The polymer matrix is a polymer formed by in-situ self-polymerization of polymer monomers composed of three building blocks: methacrylate, urea, and fluoroalkyl groups; or a polymer formed by in-situ copolymerization of polymer monomers composed of three building blocks (methacrylate, urea, and fluoroalkyl groups) with monomers containing carbon-carbon double bonds. The polymer monomers composed of the three building blocks (methacrylate, urea, and fluoroalkyl groups) are:
[0007]
[0008] In the formula, R is selected from One of them.
[0009] Furthermore, the monomer containing carbon-carbon double bonds is polyethylene glycol monomethyl ether methacrylate, polyethylene glycol diacrylate, methyl methacrylate, acrylonitrile, polytetrahydrofuran dimethacrylate, maleic anhydride, vinyl acetate, acrylamide, cyanoacrylate, lithium acrylate, or sodium acrylate.
[0010] Furthermore, in the polymer matrix, by mass percentage, polymer monomers composed of three building blocks—methacrylate groups, urea groups, and fluoroalkyl groups—account for 50% to 100% of the polymer matrix components, while other monomers account for 0% to 50% of the polymer matrix components.
[0011] Furthermore, the methacrylate-based polymer electrolyte also includes a porous support material, a lithium salt, a solvent, and an initiator.
[0012] Furthermore, the methacrylate-based polymer electrolyte comprises, by mass percentage: 10-80% polymer matrix, 5-60% porous support material, 10-70% lithium salt and solvent, and 0.01%-1% initiator.
[0013] Furthermore, the solvent accounts for 20% to 80% of the mass of the lithium salt and the solvent.
[0014] Furthermore, the porous support material is one of polyethylene terephthalate film, cellulose nonwoven film, polypropylene nonwoven film, glass fiber nonwoven film, seaweed fiber nonwoven film, polyethylene nonwoven film, aramid nonwoven film, polyarylsulfone amide nonwoven film, and polyimide nonwoven film.
[0015] And / or, the lithium salt is one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalate-borate), lithium bis(fluorosulfonyl)imide, lithium di(fluorooxalate-borate), and lithium trifluoromethanesulfonate.
[0016] And / or, the solvent is one or more of methyl ethyl carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, vinylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, and dioxolane.
[0017] And / or, the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, tert-butyl peroxide, and methyl ethyl ketone peroxide.
[0018] Secondly, the present invention also provides a method for preparing the above-mentioned methacrylate-based polymer electrolyte, wherein a porous support material is disposed between the positive and negative electrodes of a lithium-ion battery, and then a polymer matrix, lithium salt, solvent and initiator are mixed and injected into a lithium-ion battery, and the methacrylate-based polymer electrolyte is generated by in-situ solidification reaction at 30 to 100°C for 1 to 48 hours.
[0019] Thirdly, the present invention provides the application of the above-mentioned methacrylate-based polymer electrolyte in the preparation of lithium-ion batteries.
[0020] The beneficial effects of this invention are:
[0021] This invention improves the polymerization conversion rate of polymer monomers prepared by existing in-situ curing methods. A polymerization conversion rate of over 95% can reduce the residual amount of monomers in the electrolyte and improve the overall stability and safety of the electrolyte.
[0022] The polymer electrolyte of the present invention has high room temperature ionic conductivity and a wide electrochemical window, and can be applied to battery systems such as high-voltage lithium-ion batteries, high-energy-density lithium-ion batteries, and high-safety lithium-ion batteries. The fluorinated monomer can form a fluorinated SEI layer during battery cycling. When applied, a LiF-rich SEI film can be formed at the positive electrode and lithium metal / electrolyte interface to improve the stability of the electrode / electrolyte interface and inhibit lithium dendrite growth, thereby significantly improving safety performance.
[0023] A lithium-ion battery assembled using the polymer electrolyte of this invention, with lithium metal as the negative electrode and ternary 811 material as the positive electrode, can operate at 0.5C (1C = 200mAh g / L). -1 After 300 cycles at a current density of 0.5, it still has a high capacity retention rate and excellent cycle stability. Attached Figure Description
[0024] Figure 1 The conductivity curve of the polymer electrolyte in Example 1 of this invention is shown.
[0025] Figure 2 The linear sweep voltammetry curve of the polymer electrolyte in Example 1 of this invention is shown below.
[0026] Figure 3 The ternary 811 lithium metal full cell assembled with polymer electrolyte in Example 1 of this invention was tested at 0.5C (1C = 200 mAh g). -1 Cyclic performance at room temperature under current density;
[0027] Figure 4 The lithium-lithium symmetric battery assembled with polymer electrolyte in Example 6 of this invention operates at a current density of 0.5 mA / cm². -2 The following is a long-cycle performance graph. Detailed Implementation
[0028] The principles and features of the present invention are described below with reference to the accompanying drawings and specific embodiments. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0029] The technical solution of the present invention to solve the above-mentioned technical problems is as follows:
[0030] In a first aspect, the present invention provides a methacrylate-based polymer electrolyte, comprising a polymer matrix. The polymer matrix is a polymer formed by in-situ self-polymerization of polymer monomers composed of three building blocks: methacrylate, urea, and fluoroalkyl groups; or a polymer formed by in-situ copolymerization of polymer monomers composed of three building blocks (methacrylate, urea, and fluoroalkyl groups) with monomers containing carbon-carbon double bonds. The polymer monomers composed of the three building blocks (methacrylate, urea, and fluoroalkyl groups) are:
[0031]
[0032] In the formula, R is selected from One of them.
[0033] Furthermore, the monomer containing carbon-carbon double bonds is polyethylene glycol monomethyl ether methacrylate, polyethylene glycol diacrylate, methyl methacrylate, acrylonitrile, polytetrahydrofuran dimethacrylate, maleic anhydride, vinyl acetate, acrylamide, cyanoacrylate, lithium acrylate, or sodium acrylate.
[0034] Furthermore, in the polymer matrix, by mass percentage, polymer monomers composed of three building blocks—methacrylate groups, urea groups, and fluoroalkyl groups—account for 50% to 100% of the polymer matrix components, while other monomers account for 0% to 50% of the polymer matrix components.
[0035] Furthermore, the methacrylate-based polymer electrolyte also includes a porous support material, a lithium salt, a solvent, and an initiator.
[0036] Furthermore, the methacrylate-based polymer electrolyte comprises, by mass percentage: 10-80% polymer matrix, 5-60% porous support material, 10-70% lithium salt and solvent, and 0.01%-1% initiator.
[0037] Furthermore, the solvent accounts for 20% to 80% of the mass of the lithium salt and the solvent.
[0038] Furthermore, the porous support material is one of polyethylene terephthalate film, cellulose nonwoven film, polypropylene nonwoven film, glass fiber nonwoven film, seaweed fiber nonwoven film, polyethylene nonwoven film, aramid nonwoven film, polyarylsulfone amide nonwoven film, and polyimide nonwoven film.
[0039] And / or, the lithium salt is one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalate-borate), lithium bis(fluorosulfonyl)imide, lithium di(fluorooxalate-borate), and lithium trifluoromethanesulfonate.
[0040] And / or, the solvent is one or more of methyl ethyl carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, vinylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, and dioxolane.
[0041] And / or, the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, tert-butyl peroxide, and methyl ethyl ketone peroxide.
[0042] Secondly, the present invention also provides a method for preparing the above-mentioned methacrylate-based polymer electrolyte, wherein a porous support material is disposed between the positive and negative electrodes of a lithium-ion battery, and then a polymer matrix, lithium salt, solvent and initiator are mixed and injected into a lithium-ion battery, and the methacrylate-based polymer electrolyte is generated by in-situ solidification reaction at 30°C to 100°C for 1 to 48 hours.
[0043] Thirdly, the present invention provides the application of the above-mentioned methacrylate-based polymer electrolyte in the preparation of lithium-ion batteries.
[0044] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0045] Example 1
[0046] The raw material formulations used to prepare the polymer electrolyte are shown in Table 1. An electrolyte solution of lithium salt and solvent was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix and the in-situ curing initiator, the solution was completely dissolved and injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material). The battery was placed at 60°C to allow in-situ polymerization. After 8 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0047] Table 1
[0048]
[0049] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 96% after polymerization.
[0050] The conductivity of the polymer electrolyte prepared in this embodiment was tested. The test method was as follows: a coin cell was constructed using a stainless steel inert electrode as the working electrode and a stainless steel inert electrode as the counter electrode. The test frequency was 1MHz to 100mHz, and the test was performed using an EC-lab electrochemical workstation. The test results are shown in [Figure number missing]. Figure 1 As can be seen from the figure, the room temperature conductivity of the electrolyte is 10. -4 S cm -1 .
[0051] The polymer electrolyte prepared in this embodiment was subjected to electrochemical window testing. The testing method was as follows: a coin cell was constructed using a stainless steel inert electrode as the working electrode and a lithium sheet as the counter electrode. Under room temperature conditions, the test voltage range was 0–6 V, and the test was performed using an EC-lab electrochemical workstation at a scan rate of 1 mV / s. The test results are shown in [Figure number missing]. Figure 2 As can be seen from the figure, the electrolyte has a voltage range of 0–5.0 V (vs. Li / Li). + The electrochemical window of the polymer electrolyte indicates that it has high electrochemical stability and the potential to operate at high voltages.
[0052] The polymer electrolyte prepared in this embodiment is used to assemble lithium metal batteries. The specific method is as follows: Polyvinylidene fluoride (PVDF) with a concentration of 0.1–1.5 mol / L is dissolved in N-methylpyrrolidone. PVDF, conductive carbon black (such as Kolmogorov-Dazs, acetylene black, or SuperP), and lithium iron phosphate active material are mixed at a mass ratio of 10:10:80 and ground for at least 1 hour. The resulting positive electrode slurry is uniformly coated onto aluminum foil or carbon-coated aluminum foil, dried in a vacuum oven at 60–120°C, rolled, punched, and stored in a glove box for later use. Lithium metal foil is purchased and stored in a glove box for later use. The prepared separator, lithium metal sheet, and ternary 811 positive electrode sheet were sequentially placed into a 2016 coin cell casing. An electrolyte solution containing a mixture of lithium salt and solvent was then injected. Polymer monomers and an in-situ curing initiator were added and completely dissolved. This solution was then injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator. The battery was placed at 60°C for in-situ polymerization, and after 8 hours, the desired polymer electrolyte lithium-ion battery was obtained. After assembly, a long-cycle charge-discharge test was performed at room temperature, charging at a constant current of 0.5C (1C = 200mAh g1) to 4.3V and then discharging to 2.8V. The test results are shown in [Figure number missing]. Figure 3 As can be seen from the figure, the assembled full cell can cycle stably for more than 300 cycles, indicating that the polymer electrolyte prepared in this embodiment has high cycle stability and can be used in high-performance lithium-ion batteries.
[0053] Example 2
[0054] The raw material formulations used to prepare the polymer electrolyte are shown in Table 2. An electrolyte solution of lithium salt and solvent was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix and the in-situ curing initiator, the solution was completely dissolved and injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material). The battery was placed at 50°C to allow in-situ polymerization. After 3 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0055] Table 2
[0056]
[0057] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 95%. Taking the polymer electrolyte obtained in this embodiment as an example, its electrochemical performance is similar to that in Example 1 when used as a lithium-ion battery electrolyte.
[0058] Example 3
[0059] The raw material formulations used to prepare the polymer electrolyte are shown in Table 3. An electrolyte solution of lithium salt and solvent was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix and the in-situ curing initiator, the solution was completely dissolved and injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material). The battery was placed at 90°C to allow in-situ polymerization. After 2 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0060] Table 3
[0061]
[0062] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 98%. Taking the polymer electrolyte obtained in this embodiment as an example, its electrochemical performance is similar to that in Example 1 when used as a lithium-ion battery electrolyte.
[0063] Example 4
[0064] The proportions of the raw materials used to prepare the polymer electrolyte are shown in Table 4. An electrolyte solution, mixed with lithium salt and solvent, was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix, an in-situ curing initiator was added. After complete dissolution, the solution was injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material), and placed at 50°C for in-situ polymerization. After 24 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0065] Table 4
[0066]
[0067]
[0068] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 99%. Taking the polymer electrolyte obtained in this embodiment as an example, its electrochemical performance is similar to that in Example 1 when used as a lithium-ion battery electrolyte.
[0069] Example 5
[0070] The proportions of the raw materials used to prepare the polymer electrolyte are shown in Table 3. An electrolyte solution, mixed with lithium salt and solvent, was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix, an in-situ curing initiator was added. After complete dissolution, the solution was injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material), and placed at 100°C for in-situ polymerization. After 48 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0071] Table 5
[0072]
[0073] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 97%. Taking the polymer electrolyte obtained in this embodiment as an example, its electrochemical performance is similar to that in Example 1 when used as a lithium-ion battery electrolyte.
[0074] Example 6
[0075] The raw material formulations used to prepare the polymer electrolyte are shown in Table 1. An electrolyte solution of lithium salt and solvent was prepared in an argon-filled glove box. After adding the monomers used to form the polymer matrix and the in-situ curing initiator, the solution was completely dissolved and injected into a lithium-ion battery containing positive and negative electrode materials and a battery separator (porous support material). The battery was placed at 60°C to allow in-situ polymerization. After 8 hours, the desired polymer electrolyte lithium-ion battery was obtained.
[0076] Table 6
[0077]
[0078]
[0079] The polymer electrolyte prepared in this embodiment has a polymerization conversion rate of 95% after polymerization. Taking the polymer electrolyte obtained in this embodiment as an example, its electrochemical performance is similar to that of Example 1 when used as a lithium-ion battery electrolyte. The polymer electrolyte prepared in this embodiment was tested as a lithium-lithium symmetric battery. The test method was as follows: a coin cell was constructed using a lithium sheet electrode as the working electrode and a lithium sheet as the counter electrode. Under room temperature conditions, the test voltage range was 0.5 mA cm⁻¹. -2 The current density and scan rate of charge-discharge over 1 hour were measured using an EC-lab electrochemical workstation. The test results are shown in [Figure number missing]. Figure 4 As can be seen from the figure, the assembled lithium-lithium symmetric battery can cycle stably for more than 3000 hours, indicating its extremely high stability to lithium and its perfect applicability to lithium metal batteries. The performance of the full cell is similar to that of Example 1.
[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A methacrylate-based polymer electrolyte, characterized by, The polymer matrix includes a polymer formed by in-situ self-polymerization of polymer monomers composed of three building blocks: methacrylate groups, urea groups, and fluoroalkyl groups; or a polymer formed by in-situ copolymerization of polymer monomers composed of three building blocks: methacrylate groups, urea groups, and fluoroalkyl groups, and monomers containing carbon-carbon double bonds. The polymer monomers composed of the three building blocks: methacrylate groups, urea groups, and fluoroalkyl groups are: wherein R is selected from one of the following:
2. The methacrylate-based polymer electrolyte according to claim 1, characterized in that, The monomers containing carbon-carbon double bonds are polyethylene glycol monomethyl ether methacrylate, polyethylene glycol diacrylate, methyl methacrylate, acrylonitrile, polytetrahydrofuran dimethacrylate, maleic anhydride, vinyl acetate, acrylamide, cyanoacrylate, lithium acrylate, or sodium acrylate.
3. The methacrylate-based polymer electrolyte according to claim 1 or 2, characterized in that, In the polymer matrix, by mass percentage, polymer monomers composed of three building blocks—methacrylate groups, urea groups, and fluoroalkyl groups—account for 50-100% of the polymer matrix components, while other monomers containing carbon-carbon double bonds account for 0-50% of the polymer matrix components.
4. The methacrylate-based polymer electrolyte according to claim 1, characterized in that, It also includes porous support materials, lithium salts and solvents and initiators.
5. The methacrylate-based polymer electrolyte according to claim 4, characterized in that, By weight percentage, it comprises: 10-80% polymer matrix, 5-60% porous support material, 10-70% lithium salt and solvent, and 0.01%-1% initiator.
6. The methacrylate-based polymer electrolyte according to claim 5, characterized in that, The solvent accounts for 20% to 80% of the mass of the lithium salt and the solvent.
7. The methacrylate-based polymer electrolyte according to any one of claims 4-6, characterized in that, The porous support material is one of the following: polyethylene terephthalate film, cellulose nonwoven film, polypropylene nonwoven film, glass fiber nonwoven film, seaweed fiber nonwoven film, polyethylene nonwoven film, aramid nonwoven film, polyarylsulfamide nonwoven film, and polyimide nonwoven film. And / or, the lithium salt is one or more of lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalate-borate), lithium bis(fluorosulfonyl)imide, lithium di(fluorooxalate-borate), and lithium trifluoromethanesulfonate. And / or, the solvent is one or more of methyl ethyl carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, vinylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, and dioxolane. And / or, the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, tert-butyl peroxide, and methyl ethyl ketone peroxide.
8. The method for preparing the methacrylate-based polymer electrolyte according to any one of claims 1-7, characterized in that, A porous support material is placed between the positive and negative electrodes of a lithium-ion battery. Then, the monomers, lithium salts, solvents and initiators used to form the polymer matrix are mixed and injected into the lithium-ion battery. The methacrylate-based polymer electrolyte is generated by in-situ solidification reaction at 30-100°C for 1-48 hours.
9. The use of the methacrylate-based polymer electrolyte according to any one of claims 1-7 in the preparation of lithium-ion batteries.
Citation Information
Patent Citations
Polymer electrolyte, method of preparing the polymer electrolyte, and lithium metal battery including the same
CN107546412A
Intrinsic high-tensile multifunctional polymer ion conductor as well as preparation method and application thereof
CN114824285A