Hermetically sealed battery
By forming a Ni coating on the surface of the negative electrode lead and controlling the Cu concentration at the weld, combined with laser welding, the solidification crack problem at the weld between the negative electrode lead and the outer can was solved, improving the output and reliability of the sealed battery.
Patent Information
- Application Number
- CN202280019569.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-17
- Filing Date
- 2022-03-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-03-08
AI Technical Summary
In existing technologies, the weld between the negative electrode lead and the outer can is prone to solidification cracks, which affect the bonding strength and reliability of the sealed battery, and high output poses a short circuit risk.
The negative electrode lead is made of Cu as the main component and a Ni coating is formed on its surface. During welding, the Cu concentration of the welding part is controlled to be below 10% by mass. The outer can and the negative electrode lead are connected by laser welding.
It effectively suppressed solidification cracks in the welded parts, improved the output and reliability of the sealed battery, and reduced the risk of short circuits.
Smart Images

Figure CN117015904B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to sealed batteries. Background Technology
[0002] As a negative electrode lead connecting the negative electrode to the outer can inside a sealed battery, a cladding material is used, consisting of a Ni lead and a Ni cladding layer with a thickness approximately equal to that of the Cu core. Patent Document 1 discloses a secondary battery in which the negative electrode is connected to the outer can by a Ni-plated Cu negative electrode lead, with the negative electrode lead and the outer can being connected by resistance welding. In resistance welding, since the bonding only occurs near the interface between the negative electrode lead and the outer can, it is difficult to improve the bonding strength. To improve the bonding strength, increasing the output of the resistance welding can lead to sputtering inside the battery, which also increases the risk of short circuits. Patent Document 2 discloses a method for welding the negative electrode lead and the outer can using a laser to prevent sputtering.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-176490
[0006] Patent Document 2: Japanese Patent Application Publication No. 2010-3686 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] In recent years, there has been a desire for high-output sealed batteries. To achieve this, the negative electrode lead is preferably composed primarily of Cu, which has low resistivity. However, because Cu forms a morphological alloy with Fe, the main component of the outer can, during the molten solidification process of laser welding the outer can and the negative electrode lead, Fe and Cu undergo phase separation, making solidification cracks more likely to occur at the weld between the negative electrode lead and the outer can. The technologies described in Patent Documents 1 and 2 do not address solidification cracks and therefore have room for improvement.
[0009] The purpose of this invention is to provide a low-resistance sealed battery that suppresses solidification cracks at the weld between the negative electrode lead and the outer can.
[0010] Methods for solving problems
[0011] The sealed battery, as an embodiment of the present invention, is characterized by comprising: an electrode body formed by winding a positive electrode and a negative electrode with a spacer between them; a bottomed cylindrical outer can for housing the electrode body; and a sealing body for blocking the opening of the outer can; a negative electrode lead connected to the negative electrode and the outer can are welded together by a welded portion formed from the outer surface of the outer can to the negative electrode lead; the outer can contains a metal containing Fe; the negative electrode lead contains a metal mainly composed of Cu; and the Cu concentration of the welded portion is 10% by mass or less.
[0012] Invention Effects
[0013] According to the sealed battery as one aspect of the present invention, output and reliability can be improved. Attached Figure Description
[0014] Figure 1 This is an axial cross-sectional view of a cylindrical secondary battery as an example of an implementation method.
[0015] Figure 2 This is an enlarged cross-sectional view of the welded portion between the outer can and the negative lead in one embodiment. Detailed Implementation
[0016] Hereinafter, a cylindrical non-aqueous electrolyte secondary battery (hereinafter referred to as a secondary battery) as an example of an embodiment of the sealed battery of the present invention will be described in detail with reference to the accompanying drawings. In the following description, specific shapes, materials, values, orientations, etc., are used for ease of understanding of the illustrative purpose of the present invention and may be appropriately modified accordingly with respect to the specifications of the cylindrical secondary battery. In addition, the outer can is not limited to a cylindrical shape, and may be, for example, square or the like. Furthermore, in the following description, where multiple embodiments and modifications are included, it is envisioned from the outset that their characteristic parts be appropriately combined and used.
[0017] Figure 1 This is an axial cross-sectional view of a secondary battery 10 as an example of an implementation. Figure 1In the secondary battery 10 shown, the electrode body 14 and the non-aqueous electrolyte (not shown) are housed in an outer container 15. The non-aqueous solvent (organic solvent) used as the electrolyte can be carbonates, lactones, ethers, ketones, esters, etc., and two or more of these solvents can be mixed. When two or more solvents are mixed, a mixed solvent containing cyclic carbonates and chain carbonates is preferred. For example, ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), etc., can be used as cyclic carbonates, and dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), etc., can be used as chain carbonates. The electrolyte salt used as the electrolyte can be LiPF6, LiBF4, LiCF3SO3, etc., and mixtures thereof. The solubility of the electrolyte salt relative to the non-aqueous solvent can be, for example, set to 0.5 to 2.0 mol / L. It should be noted that, for ease of explanation, the side of the sealing body 16 will be referred to as "upper" and the bottom side of the outer can 15 as "lower" in the following description.
[0018] The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound together with a spacer 13. The positive electrode 11, the negative electrode 12 and the spacer 13 are all formed in the shape of strips and are wound into a spiral shape around a core arranged along the winding axis, thereby forming an alternating layer in the radial direction of the electrode body 14.
[0019] The positive electrode 11 has a strip-shaped positive current collector and positive electrode flux layers formed on both sides of the positive current collector. The positive current collector may be, for example, a foil of a metal such as aluminum, or a film obtained by depositing the metal on the surface. The thickness of the positive current collector is, for example, 10 μm to 30 μm.
[0020] The positive electrode binder layer preferably comprises a positive electrode active material, a conductive agent, and a binder. The positive electrode binder layer can be manufactured, for example, by coating a positive electrode binder slurry containing a positive electrode active material, a conductive agent, a binder, and a solvent such as N-methyl-2-pyrrolidone (NMP) onto both sides of the positive electrode current collector, drying it, and then calendering it.
[0021] A positive electrode exposed portion is provided on the surface of the positive electrode current collector of the positive electrode 11. The positive electrode exposed portion is the part that connects to the positive electrode lead 19 (described later), and is the part of the surface of the positive electrode current collector that is not covered by the positive electrode flux layer. It is suitable that the positive electrode exposed portions are provided on both sides of the positive electrode 11 in an overlapping manner along the thickness direction of the positive electrode 11. The positive electrode lead 19 is joined to the positive electrode exposed portion, for example, by ultrasonic welding.
[0022] The positive electrode exposed portion is provided, for example, at a position approximately equidistant from the inner and outer ends of the electrode body 14. This improves current collection performance. By connecting the positive electrode lead 19 to the positive electrode exposed portion at such a location, the positive electrode lead 19 is positioned so that, during the winding of the electrode body 14, it protrudes upwards from its end face in the width direction at approximately the center of the electrode body 14 in the radial direction. The positive electrode exposed portion is provided, for example, by intermittently coating a portion of the positive electrode current collector without applying the positive electrode slurry.
[0023] Examples of positive electrode active materials contained in the positive electrode additive layer include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Lithium transition metal oxides are, for example, Li. x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z Li x Ni 1-y M y O z Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). These can be used alone or in combination. For the purpose of achieving high capacity in non-aqueous electrolyte secondary batteries, the positive electrode active material preferably contains Li. x NiO2, Li x Co y Ni 1-y O2, Li x Ni 1-y M y O z (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3) and other lithium-nickel composite oxides.
[0024] Examples of conductive agents contained in the positive electrode layer include carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based particles. These can be used alone or in combination of two or more.
[0025] Examples of binders contained in the positive electrode binder layer include fluorinated resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, and polyolefin resins. These can be used individually or in combination of two or more. When preparing the positive electrode binder slurry with an aqueous solvent, styrene-butadiene rubber (SBR), nitrile rubber (NBR), CMC or its salts, polyacrylic acid or its salts, and polyvinyl alcohol can also be used.
[0026] The negative electrode 12 has a strip-shaped negative electrode current collector and negative electrode flux layers formed on both sides of the negative electrode current collector. The negative electrode current collector can be, for example, a foil of metal such as copper, or a film obtained by depositing the metal on the surface. The thickness of the negative electrode current collector is, for example, 5 μm to 30 μm.
[0027] The negative electrode binder layer may include, for example, a negative electrode active material and a binder. The negative electrode binder layer may be manufactured, for example, by coating a negative electrode binder slurry containing a negative electrode active material, a binder, and a solvent such as water onto both sides of the negative electrode current collector, drying it, and then calendering it.
[0028] The negative electrode 12 has a negative electrode exposed portion where the surface of the negative electrode current collector is exposed. The negative electrode exposed portion is the part that connects to the negative electrode lead 20 (described later), and is the part of the surface of the negative electrode current collector that is not covered by the negative electrode binder layer. It is suitable that the negative electrode exposed portions are provided on both sides of the negative electrode 12 in an overlapping manner along the thickness direction of the negative electrode 12. The negative electrode lead 20 is joined to the negative electrode exposed portion, for example, by ultrasonic welding.
[0029] The negative electrode exposed portion is provided, for example, at the inner end or outer end of the winding of the electrode body 14. The negative electrode lead 20 can be connected to either the inner end or the outer end of the winding of the electrode body 14. Alternatively, the negative electrode lead 20 can also be connected to both the inner end and the outer end of the winding of the negative electrode 12. In this case, the current collection performance is improved. By connecting the negative electrode exposed portion at the outer end of the winding of the negative electrode 12 to the outer can 15 (see reference 15)... Figure 1 The inner circumferential surface of the negative electrode 12 is in contact with the negative electrode, so that the outer end of the negative electrode 12 can be electrically connected to the outer can 15 without using the negative electrode lead 20. The exposed negative electrode portion is provided, for example, by intermittently coating a portion of the negative electrode current collector without coating it with the negative electrode slurry.
[0030] The negative electrode active material contained in the negative electrode compound layer is not particularly limited if it is a material that can reversibly absorb, store, and release lithium ions. It can be carbon-based materials such as natural graphite and artificial graphite, metals such as Si and Sn alloyed with lithium, or alloys or oxides containing these.
[0031] Examples of binders contained in the negative electrode binder layer include styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or its salts, polyacrylic acid (PAA) or its salts (PAA-Na, PAA-K, etc., and also partially neutralized salts), polyvinyl alcohol (PVA), etc. Additionally, binders may also include fluorinated resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, etc. These can be used individually or in combination of two or more.
[0032] Next, refer to Figure 1 The positive electrode lead 19 and the negative electrode lead 20 will be described. The positive electrode lead 19 extends axially from approximately the center in the radial direction between the center and the outermost periphery at the upper end of the electrode body 14. The positive electrode lead 19 is, for example, made of Al.
[0033] The negative electrode lead 20 extends axially from near the winding shaft at the lower end of the electrode body 14. The negative electrode lead 20 contains a metal with Cu as its main component. This reduces resistance and improves the battery's output.
[0034] The negative electrode lead 20 may have a Ni coating on its surface. That is, the negative electrode lead 20 may have a Ni coating on the surface of a metal with Cu as the main component. This can suppress the oxidation of Cu. From the viewpoint of suppressing Cu oxidation, the Ni coating is preferably formed on both sides of the metal with Cu as the main component. It should be noted that, in the following, when the Ni coating is formed on both sides of the metal with Cu as the main component, the thickness of the Ni coating refers to the thickness of one side of the metal with Cu as the main component.
[0035] In the portion of the negative electrode lead 20 excluding the Ni plating, elements other than Cu are present only at the impurity level, or it may consist primarily of Cu. The content of elements other than Cu in the portion of the negative electrode lead 20 excluding the Ni plating is preferably 1% by mass or less, more preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less.
[0036] The thickness of the negative electrode lead 20 (Cu thickness + Ni plating thickness) is, for example, 50 μm to 200 μm. Furthermore, the thickness of the Ni plating is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 10 μm, and particularly preferably 0.5 μm to 5 μm. If the thickness of the Ni plating is 0.1 μm or more, Cu oxidation can be suppressed. From the viewpoint of cost reduction, the thickness of the Ni plating is preferably as thin as possible within the range that can suppress Cu oxidation. The ratio of the Ni plating thickness to the thickness of the negative electrode lead 20 (Ni plating thickness / negative electrode lead thickness) is, for example, 0.005 to 0.2.
[0037] Next, use Figure 1 The connection method between the outer can 15 and the sealing body 16 inside the secondary battery 10 and the electrode body 14 is described.
[0038] The outer container 15 is a bottomed cylindrical container that houses the electrode body 14, non-aqueous electrolyte, etc. The outer container 15 also contains a metal containing Fe. For example, the outer container 15 is made of carbon steel. The thickness of the outer container 15 is, for example, 0.2 mm to 0.8 mm. Furthermore, the outer container 15 may have a Ni plating on its surface, or both its inner and outer surfaces. The thickness of the Ni plating on the surface of the outer container 15 is, for example, 0.1 μm to 10 μm.
[0039] The interior of the secondary battery 10 is sealed by blocking the upper end of the outer can 15 with the sealing body 16. Insulating plates 17 and 18 are respectively provided above and below the electrode body 14. The positive electrode lead 19 extends upward through the through hole of the insulating plate 17 and is welded to the lower surface of the bottom plate of the sealing body 16, i.e., the filter element 22. In the secondary battery 10, the top plate of the sealing body 16, i.e., the cover 26, which is electrically connected to the filter element 22, serves as the positive terminal. On the other hand, the negative electrode lead 20 extends to the bottom side of the outer can 15 through the through hole of the insulating plate 18 and is welded to the inner bottom surface of the outer can 15. In the secondary battery 10, the outer can 15 serves as the negative terminal.
[0040] A gasket 27 is provided between the outer can 15 and the sealing body 16 to ensure the internal airtightness of the secondary battery 10. The outer can 15, for example, has a groove 21 formed by pressing the side portion from the outside to support the sealing body 16. The groove 21 is preferably formed in a ring shape along the circumference of the outer can 15, and supports the sealing body 16 on its upper surface.
[0041] The sealing body 16 comprises a filter element 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26, stacked sequentially from the electrode body 14 side. Each component constituting the sealing body 16 has, for example, a circular or annular shape, and all components except the insulating member 24 are electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective central portions, with the insulating member 24 sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heating, for example, the lower valve body 23 breaks, thereby causing the upper valve body 25 to bulge towards the cover 26 and separate from the lower valve body 23, thus severing the electrical connection between them. If the internal pressure rises further, the upper valve body 25 breaks, and gas is discharged from the opening 26a of the cover 26.
[0042] Next, refer to Figure 2 The connection method between the external can 15 and the negative lead 20 is explained. Figure 2 This is an enlarged cross-sectional view of the welded portion 30 between the outer can 15 and the negative lead 20 in one embodiment.
[0043] The outer can 15 and the negative electrode lead 20 are welded together using a weld portion 30 formed from the outer surface of the outer can 15 to the negative electrode lead 20. The weld portion 30 extends through the bottom of the outer can 15 and reaches the interior of the negative electrode lead 20 from the outer surface of the outer can 15. The weld portion 30 is, for example, a molten and solidified portion of the outer can 15 and the negative electrode lead 20 formed by irradiating the outer surface of the outer can 15 with a laser. That is, the weld portion 30 can be formed by irradiating the bottom of the outer can 15 from the outside of the secondary battery 10 while the negative electrode lead 20 is in contact with the inner surface of the outer can 15. The wavelength of the laser is not particularly limited as long as it is within the range absorbed by the outer can 15, for example, 1060 nm to 1080 nm. It should be noted that there is no particular limitation on the laser output as long as the weld portion 30 described above is formed.
[0044] The Cu concentration in the contact portion 30a between the negative electrode lead 20 and the outer can 15 in the welded portion 30 is preferably 10 mass% or less, more preferably 8.6 mass% or less. The welded portion 30 is an alloy formed by melting and solidifying the Fe-containing metal constituting the outer can 15 and the Cu-based metal constituting the negative electrode lead 20. The Cu concentration in the welded portion 30 can be measured using an electron probe microanalyzer (EPMA). Depending on the welding conditions, the composition of the alloy formed in the welded portion may be non-uniform. Therefore, the measurement of the Cu concentration is preferably performed at the center of the contact portion 30a where the negative electrode lead 20 and the outer can 15 in the welded portion 30 contact each other immediately before welding. The measurement range is, for example, a range within 100 μm from the center of the contact portion 30a. By controlling the Cu concentration measured in this way within the above range, solidification cracks in the welded portion 30 are effectively suppressed. It should be noted that the contact portion 30a is a portion corresponding to the contact surface between the negative electrode lead 20 and the outer can 15 in the welded portion 30 immediately before welding and its vicinity. The presence or absence of solidification cracks in the welded portion 30 can be confirmed, for example, by observing the welded portion 30 with a scanning electron microscope (SEM).
[0045] Examples
[0046] Hereinafter, the present invention will be further described by way of Examples, but the present invention is not limited to these Examples.
[0047] <Example 1>
[0048] [Production of Positive Electrode]
[0049] As the positive electrode active material, a lithium transition metal oxide represented by LiNi 0.8 Co 0.15 Al 0.05 O2 is used. 100 parts by mass of this positive electrode active material, 2.5 parts by mass of acetylene black (AB) as a conductive agent, and 1.7 parts by mass of polyvinylidene fluoride (PVdF) as a binder are mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) is further added to prepare a positive electrode mixture slurry. Next, this positive electrode mixture slurry is applied to both surfaces of a positive electrode current collector formed of an aluminum foil and dried, then cut to a predetermined electrode size, and rolled with a roller to obtain a belt-shaped positive electrode. In addition, an uncoated portion where no active material is formed is formed at one end in the longitudinal direction of the positive electrode, and one end of an Al positive electrode lead is fixed to this uncoated portion by ultrasonic welding.
[0050] [Production of Negative Electrode]
[0051] Easily graphitizable carbon was used as the negative electrode active material. 100 parts by weight of this negative electrode active material, 0.6 parts by weight of styrene-butadiene rubber (SBR) as a binder, and 1 part by weight of carboxymethyl cellulose (CMC) as a thickener were mixed, and water was added as needed to prepare a negative electrode slurry. Next, the negative electrode slurry was coated onto both sides of a negative electrode current collector formed from copper foil and dried. The specified electrode size was then cut, and the strip-shaped negative electrode was obtained by calendering using rollers. At this point, an uncoated portion without active material was formed at one end of the negative electrode along its length. Furthermore, a negative electrode lead with a thickness of 0.1 mm, obtained by forming a 1 μm thick Ni plating layer on each side of the Cu, was prepared. One end of the negative electrode lead was fixed to the uncoated portion by ultrasonic welding.
[0052] [Preparation of non-aqueous electrolytes]
[0053] Ethyl carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of EC:EMC:DMC = 3:3:4. LiPF6 was then added to the resulting mixed solvent at a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte.
[0054] [Making a Sealed Battery]
[0055] A spiral electrode body is fabricated by winding the positive and negative electrodes into a spiral shape, separated by a spacer made of polyolefin resin. Insulating plates are placed above and below the electrode body, which is then housed in a bottomed cylindrical metal outer can. The outer can has a thickness of 0.4 mm and a 1 μm thick Ni plating layer on both sides. Next, a 1070 nm wavelength fiber laser is irradiated from the outside of the outer can onto its bottom, and the negative electrode lead protruding from the electrode body is welded to the bottom of the outer can. A groove is formed in the opening of the outer can by stamping, and a non-aqueous electrolyte is injected into the interior of the outer can. A gasket is placed on top of the groove, and after welding the sealing body to the positive electrode lead, the opening of the outer can is sealed by riveting the sealing body through the gasket, thus creating a sealed battery.
[0056] <Example 2>
[0057] In the fabrication of the negative electrode, a negative electrode lead with a thickness of 0.1 mm is obtained by forming a Ni plating layer with a thickness of 3 μm on both sides of Cu. Except as described above, the battery is fabricated in the same manner as in Example 1.
[0058] <Example 3>
[0059] In the fabrication of the negative electrode, a negative electrode lead with a thickness of 0.1 mm is obtained by forming a Ni plating layer with a thickness of 5 μm on both sides of Cu. Except as described above, the battery is fabricated in the same manner as in Example 1.
[0060] <Example 4>
[0061] In the fabrication of the negative electrode, a negative electrode lead with a thickness of 0.1 mm is obtained by forming a Ni plating layer with a thickness of 10 μm on both sides of Cu. Except as described above, the battery is fabricated in the same manner as in Example 1.
[0062] <Example 5>
[0063] In the fabrication of the negative electrode, a negative electrode lead with a thickness of 0.1 mm without a Ni coating on the surface is used. Except as described above, the battery is fabricated in the same manner as in Example 1.
[0064] <Comparative Example 1>
[0065] In the fabrication of the sealed battery, the output of the fiber laser is increased, and the battery is fabricated in the same manner as in Example 1, except as described above.
[0066] <Comparative Example 2>
[0067] In the fabrication of the sealed battery, the output of the fiber laser was set to be the same as in Comparative Example 1, and the battery was fabricated in the same manner as in Example 2, except as described above.
[0068] <Comparative Example 3>
[0069] In the fabrication of the sealed battery, the output of the fiber laser was set to be the same as in Comparative Example 1, and the battery was fabricated in the same manner as in Example 3, except as described above.
[0070] <Comparative Example 4>
[0071] In the fabrication of the sealed battery, the output of the fiber laser was set to be the same as in Comparative Example 1, and the battery was fabricated in the same manner as in Example 4, except as described above.
[0072] <Comparative Example 5>
[0073] In the fabrication of the sealed battery, the output of the fiber laser was set to be the same as in Comparative Example 1, and the battery was fabricated in the same manner as in Example 5, except as described above.
[0074] [Evaluation of the Welding Section]
[0075] After cutting out the outer casing near the bottom of the batteries from the examples and comparative examples, embedding it in epoxy resin, and then cutting and grinding it, it became possible to observe... Figure 2 The cross-section is shown. Subsequently, the weld was observed using SEM to confirm the presence of solidification cracks; if solidification cracks were present, their lengths were measured. Additionally, the Cu concentration in the weld was measured using EPMA.
[0076] The evaluation results of the examples and comparative examples are shown in Table 1.
[0077] [Table 1]
[0078]
[0079] In Examples 1-5, by controlling the Cu concentration in the welded portion to below 10% by mass, the formation of solidification cracks was suppressed compared to Comparative Examples 1-5. It should be noted that in Example 5, although solidification cracks occurred, they were not large enough to cause the negative electrode lead to peel off.
[0080] Explanation of reference numerals in the attached figures
[0081] 10 Secondary battery; 11 Positive electrode; Inner end of the roll; 12 Negative electrode; 13 Spacer; 14 Electrode body; 15 Outer casing; 16 Sealing body; 17, 18 Insulating plate; 19 Positive lead; 20 Negative lead; 21 Groove; 22 Filter element; 23 Lower valve body; 24 Insulating component; 25 Upper valve body; 26 Cover; 26a Opening; 27 Gasket; 30 Welded part; 30a Abutment part
Claims
1. A sealed battery comprising: an electrode body formed by winding a positive electrode and a negative electrode with a spacer between them; a bottomed cylindrical outer can for housing the electrode body; and a sealing body for blocking the opening of the outer can. The negative electrode lead connected to the negative electrode and the outer can are welded together using a weld joint formed from the outer surface of the outer can to the negative electrode lead. The welded portion is a molten and solidified portion, which is formed by irradiating the outer surface of the outer can with a laser. The outer can contains a metal containing Fe, the negative electrode lead contains a metal with Cu as the main component, and the Cu concentration of the welded part is less than 10% by mass. The Cu concentration is measured at the center of the contact area between the negative electrode lead and the outer can just before welding, and the measurement range is within 100 μm from the center of the contact area.
2. The sealed battery according to claim 1, wherein, The Cu concentration in the welded part is below 8.6% by mass.
3. The sealed battery according to claim 1 or 2, wherein, The negative electrode lead has a Ni plating layer on its surface.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2001176490A
Secondary battery and its manufacturing method
JP2010003686A
Manufacturing method for sealed battery, and sealed battery
WO2019177081A1