Process for producing a catalyst comprising at least one group VIB metal, at least one group VIII metal and a support based on oxides
By extracting the degraded catalyst metal in acidic or aqueous solvents and impregnating it with a new support, the problems of low catalyst activity and complex recovery are solved, achieving efficient and economical catalyst regeneration and recovery, and simplifying industrial operations.
Patent Information
- Application Number
- CN202180084635.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2021-12-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-12-02
AI Technical Summary
Existing technologies for regenerating hydrogenation catalysts exhibit lower activity than fresh catalysts, and the metal recovery process is complex and uneconomical, making it difficult to carry out efficiently on an industrial scale.
By extracting metals from exhausted catalysts in acidic or aqueous solvents to form an impregnation solution, and then impregnating a new support to prepare a recycled catalyst, solid precipitation and filtration operations are avoided, and acidic and coordinating organic compounds are used to improve metal dissolution efficiency.
This technology simplifies the metal recovery process on an industrial scale, improves the metal recovery rate, produces recycled catalysts with performance close to that of fresh catalysts, and reduces operational complexity and cost.
Smart Images

Figure CN117042880B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the production of catalysts comprising at least one Group VIB metal, at least one Group VIII metal, and a support based on metal and / or silicon oxides. These catalysts are particularly intended for use in hydrocarbon hydrotreating or hydroconversion units. Existing technology
[0002] The term "hydrotreatment" refers to all purification methods that remove various impurities from hydrocarbon feedstocks using the action of hydrogen. Hydrotreatment methods allow the removal of impurities present in the feedstock, such as nitrogen (then called hydronitrogenation), sulfur (then called hydrosulfurization), oxygen (then called hydrodeoxygenation), and metal-containing compounds that can poison the catalyst and cause operational problems downstream (then called hydrodemetallization). Therefore, hydrotreatment can bring hydrocarbons and petroleum products to the required specifications (sulfur content, aromatic compound content, etc.) for a given application (motor vehicle fuel, gasoline or diesel fuel, household fuel oil, etc.). In particular, automotive standards have imposed very strong reductions in sulfur in diesel and gasoline fuels, and hydrotreatment enables these products to meet the required specifications.
[0003] Hydrotreating improves the quality of hydrocarbons by reducing the content of certain compounds and elements considered impurities, but it can also reduce the content of aromatics and thus improve the cetane number of the hydrocarbons. Small amounts of fuel gas and light fractions, such as LPG (liquefied petroleum gas) and naphtha, can also be produced during the hydrotreating process.
[0004] The hydrocarbon feedstocks targeted by this type of processing are particularly fractions from coal or natural gas, optionally as mixtures, or hydrocarbon fractions from biomass. They can also be heavy synthetic or petroleum fractions, such as kerosene, gas oil, or distillates obtained by atmospheric and vacuum distillation to produce kerosene, gas oil, or vacuum distillates, which can be upgraded in storage units (pools) receiving the same type of product or in downstream units such as catalytic cracking units, where the feedstock is "cracked" to produce hydrocarbons with shorter chains. Typically, hydrotreatment methods are actually the initial stage of processing the feedstock through hydroconversion / hydrocracking-type methods.
[0005] It should be noted that hydrocracking of heavy petroleum fractions (also referred to by the term hydroconversion) is a key method in refining, enabling the production of lighter fractions desired by refiners, such as gasoline, jet fuel, and light gas oil, from surplus and difficult-to-redegrade heavy feedstocks, thus adapting production to demand. Some hydrocracking methods can also yield highly purified residue oils, which can form excellent base oils.
[0006] More specifically, the feedstocks used in hydrotreating processes are, for example, gasoline, gas oil, vacuum gas oil, atmospheric residue, vacuum residue, atmospheric distillate, vacuum distillate, heavy fuel oil, oil, wax and paraffin, waste oil, deasphalted residue or crude oil, feedstocks derived from thermal or catalytic conversion processes, lignocellulosic feedstocks, or more commonly feedstocks derived from biomass, such as vegetable oils. The feedstocks being treated, particularly those mentioned above, typically contain heteroatoms such as sulfur, oxygen, and nitrogen, and for heavy feedstocks, they often also contain metals.
[0007] For example, patent EP3339401 can be mentioned, which describes a hydrotreating and hydroconversion apparatus with conventional fractionation for producing at least one of the following products: naphtha (light and / or heavy), diesel oil, kerosene, distillate, and residue oil.
[0008] Also mentioned is patent FR2966835, which describes a method having at least one hydrotreating step, and includes various alternative forms, including hydrotreating, hydrocracking, hydrotreating followed by hydrocracking without separation between hydrotreating and hydrocracking (also known as single-step hydrocracking), hydrotreating followed by hydrocracking with intermediate separation, or hydrotreating followed by first hydrocracking, product separation, and treatment of the unconverted fraction by another hydrocracking step (also known as two-step hydrocracking). This patent suggests, in the case of nitrogen-containing feedstocks, recycling a portion of the hydrotreating or hydrocracking effluent to the hydrotreating or hydrocracking step after stripping with hydrogen or other inert gases.
[0009] Also mentioned is patent WO 2015 / 078675, which describes the hydrotreating of two hydrocarbon fractions, each containing sulfur and nitrogen compounds, using different or the same catalyst for each fraction, and recycling the hydrogen recovered from the effluents of the two hydrotreating processes to hydrotreate one of the two fractions.
[0010] Conventional hydrotreating catalysts typically comprise an oxide support and an active phase based on Group VIB and Group VIII metals, as well as phosphorus, in oxide form. The preparation of these catalysts generally involves impregnating the metal and phosphorus onto the support, followed by drying and calcination to obtain the active phase in oxide form. These catalysts are also typically subjected to sulfidation before being used in hydrotreating and / or hydrocracking reactions.
[0011] To improve the activity of hydrotreating catalysts, it is also known to add organic additives, especially for catalysts prepared by impregnation followed by drying without subsequent calcination. These catalysts are often referred to as "additive-impregnated dry catalysts".
[0012] The catalysts used in hydrocracking are bifunctional, meaning they combine acid and hydrogenation functions. The acid function is characterized by a high specific surface area (typically 150-800 m²) with high acidity. 2 .g -1 The support is provided by, for example, halogenated (especially chlorinated or fluorinated) alumina, combinations of oxides of boron and aluminum, amorphous silica-alumina, and zeolites. The hydrogenation function is provided by one or more metals of Group VIII of the periodic table, or by a combination of at least one metal of Group VIB and at least one metal of Group VIII, used in the presence of sulfur. The balance between the acid and hydrogenation functions controls the activity and selectivity of the catalyst.
[0013] During the operation of catalysts in hydrotreating and / or hydrocracking processes, the catalysts become deactivated due to the accumulation of coke and / or sulfur-based compounds or compounds containing other impurities on the catalyst surface. After a certain period of time, they need to be replaced.
[0014] To overcome these drawbacks, the regeneration (also known as mild calcination) of hydrotreatment catalysts is an economically and ecologically advantageous method because it allows these catalysts to be reused in industrial units instead of being landfilled or recycled (metal recovery). Regeneration involves heat treatment, typically at 350°C to 550°C, in the presence of pure or diluted oxygen, with the aim of removing at least a portion of the coke present on the degraded catalyst through combustion. This regeneration allows the catalyst, referred to as "regenerated," to regain its hydrodesulfurization activity. However, regenerated catalysts are generally less active than the starting catalyst (also known as "fresh"). Therefore, their cycle time in the hydrotreatment unit is thus reduced compared to fresh catalysts. Optionally, it can be reused in less demanding applications.
[0015] To overcome the insufficient hydrodesulfurization activity of regenerated catalysts, an additional treatment known as "reversion" can be applied. Reversion methods involve re-impregnating the regenerated catalyst with a solution containing organic or inorganic additives and / or metal precursors. These "reversion" methods are well-known, particularly in the field of middle distillates. Although more efficient than simple regeneration, in most cases, catalyst reversion results in a catalyst with lower activity than fresh catalyst. Finally, some spent catalysts cannot form a body that can be reused through regeneration or reversion because their integrity is compromised (too low size or mechanical strength) or because they contain excessive contaminants, resulting in inadequate performance of the regenerated or reverted product.
[0016] Typically, the metals contained in spent hydrotreating or hydroconversion catalysts are not currently industrially recycled for the manufacture of new catalysts: they are essentially reused in the manufacture of special alloys, which requires complex purification operations, particularly the removal of compounds considered contaminants, such as arsenic, or problematic compounds from the perspective of the target application, such as phosphorus, which interfere with the properties of, for example, chromium steel alloys.
[0017] Furthermore, methods for recovering metals from catalysts have been developed for recycling them in the manufacture of new catalysts. This is exemplified by the method described, for instance, in patent application US 2007 / 0167321, which provides for recovering molybdenum from spent catalysts to produce new catalysts. According to this method, the spent catalyst is dispersed in an alkaline solution, and contaminants / compounds (arsenic, phosphorus) contained in the spent catalyst are removed from the solution by precipitating it and then filtering the solution. Molybdenum is then precipitated by changing the pH of the solution to an acidic pH. The molybdenum precipitate is filtered out so that it can be reused by dispersing it in an impregnation solution, which also contains precursors of other metals, such as cesium, antimony, or vanadium, and precursors of other components necessary for constructing a new catalyst by impregnation of a support.
[0018] Patent application EP2064358 provides a very similar method for selectively recovering Group VIB metals from spent catalysts containing both Group VIB and Group VIII metals for reuse in the manufacture of new catalysts. The provided method involves oxidizing the spent catalyst by calcination at 600°C, physically separating the oxides of the Group VIB metals from those of the Group VIII metals, dissolving the Group VIB metal oxides in an alkaline solution, oxidizing the solution with a peroxide-type oxidant, precipitating the Group VIB metal oxides by adding alkaline earth metal ions, filtering the precipitate, and then converting it to a solid metal compound by adding acid. This solid metal compound is then dissolved in an impregnation solution also containing Group VIII metal compounds to impregnate a support and thereby produce a new catalyst.
[0019] These methods are technically advantageous, but they are not without drawbacks. This is because they require a large number of operations, and the process of extracting the target metal from the exhausted catalyst for reuse in the new catalyst remains complex, making their implementation complicated and therefore not very profitable.
[0020] Therefore, the object of this invention is to provide a novel method for recycling metals contained in exhausted catalysts to produce new catalysts. This invention relates to the development of improved methods that are particularly simpler to implement on an industrial scale, while enabling high metal recovery rates. Invention Overview
[0022] The subject of this invention is primarily a method for producing a recycled catalyst comprising at least one metal M1 from Group VIB and / or at least one metal M2 from Group VIII, optionally phosphorus and / or sulfur, and a support based on one or more oxides, characterized in that the method comprises at least a portion of one or more metals of a recycled source catalyst comprising metal M1 and / or metal M2 common to the recycled catalyst to be produced, the method comprising: - extracting metal M1 and / or metal M2 from the source catalyst by an extraction solution to obtain a solution of the extracted one or more metals, and then - impregnating a support with an impregnation solution obtained from the solution of the extracted one or more metals to obtain an impregnated substrate, wherein the extracted one or more metals are maintained in a liquid phase from extraction to impregnation.
[0023] According to the present invention, it should be understood that the impregnation solution “generated” from the extraction solution means that there is no intermediate treatment in which one or more metals extracted are in the solid phase, nor is there any liquid / liquid extraction treatment of such metal / these metals.
[0024] Therefore, the impregnation solution and the extraction solution preferably have at least one common solvent.
[0025] They can have the same solvent or a mixture of solvents, or in the case of a mixture, the proportion of solvents can vary. It can involve, for example, water, or a mixture of solvents that mainly or substantially contain aqueous solvents.
[0026] According to the present invention, "extraction" should be understood as the existence of an extraction step, but the extraction can be performed by one extraction operation or multiple consecutive extraction operations.
[0027] According to the present invention, "impregnation" should be understood as referring to the presence of an impregnation step, but the impregnation can be performed by one impregnation or multiple consecutive impregnation operations.
[0028] According to the present invention, "source" catalyst should be understood to mean a spent catalyst, i.e., a catalyst that has already been used in production, particularly in hydrocracking or hydroconversion units. This catalyst may optionally have been regenerated or restored before its recycling. The term should also be understood to mean a catalyst that has not yet been used in production but is outside specifications, for example because it contains insufficient amounts of one or more metals, or is smaller than the desired size (e.g., "fine powder" of catalyst particles).
[0029] According to the present invention, “support” (which is impregnated with an impregnation solution produced from a solution of one or more extracted metals) should be understood to mean a “new” oxide support, as well as a support that has been impregnated with another impregnation solution (referred to as a pre-impregnated support) or a support that is actually a catalyst (a support with metals) but contains insufficient amounts of metal, such as a depleted or regenerated catalyst.
[0030] This invention is advantageously applied to the recycling of metals from hydrotreating catalysts.
[0031] Preferably, the extraction solution and / or impregnation solution are acidic media.
[0032] When these media are aqueous, the acidity of the media is expressed by pH value, especially at most 6, for example 0.5-6. When these media are organic, the acidity can be expressed by the content of inorganic or organic acids.
[0033] Advantageously, the impregnation solution does not contain alkali metal elements (column IA of the periodic table according to Chemical Abstracts Service nomenclature, corresponding to column 1 according to IUPAC nomenclature). This is because alkali metals have been shown to tend to act as poisons for hydrotreating catalysts.
[0034] According to one embodiment of the invention, only a single metal M1 or M2 is extracted from the catalyst, particularly when it contains only metal M1 or only metal M2. According to another embodiment, the depleted catalyst contains at least one metal M1 and at least one metal M2, and according to the invention, only the M1-type or M2-type metal is extracted, or both the M1-type and M2-type metals are extracted.
[0035] Therefore, this invention provides a novel method in which a metal derived from a source catalyst is dissolved and retained in solution until it is reused as a supplement to the impregnation solution for the production of a fresh / new catalyst. Unlike prior art, this invention does not seek to recover metal from the source catalyst in solid and single-metal form, thus saving many precipitation / filtration-type operations. Therefore, the method of this invention is more easily implemented on an industrial scale. This is further simplified when the extraction solution and the impregnation solution have a common solvent (or solvent mixture), especially when the solvents of the two solutions are the same (or similar, except for the solvent ratio, e.g., in the case of a solvent mixture).
[0036] Preferably, extraction is carried out using a solution containing a solvent, particularly an aqueous solvent, and at least one organic compound having coordination properties and optionally also acidic properties.
[0037] This is because it has been shown that adding organic compounds to a (typically aqueous) solution is very effective in extracting target metals that need to be recycled, by transferring the target metal to the liquid phase while the support of the source catalyst and other optional components of the degraded catalyst remain in the solid phase and are therefore easily removed.
[0038] It should be emphasized that the organic compounds that produce the most favorable results are those with acidic and coordinating properties. This is because organic acids enable the ionization of metal oxides, thereby limiting their interaction with the support and promoting their dissolution in the extraction solution. The coordinating agent itself allows for the formation of metal coordination compounds soluble in the extraction solution. Therefore, the combination of acidic and coordinating properties is particularly advantageous. Thus, the use of organic compounds possessing both of these properties, or combinations of acidic and coordinating organic compounds, is specifically recommended.
[0039] The organic compound, or at least one of them when several of them are present, may contain one or more chemical functional groups selected from carboxylic acids, phosphoric acids, sulfonic acids, alcohols, thiols, thioethers, sulfones, sulfoxides, ethers, aldehydes, ketones, esters, carbonates, amines, nitriles, imides, oximes, ureas, and amides, or a compound containing a furan ring or a sugar.
[0040] Organic compounds (or at least one of them, if present) may be selected from at least one of the following compounds: formic acid, acetic acid, oxalic acid, malonic acid, glutaric acid, glycolic acid, lactic acid, malonic acid, citric acid, tartaric acid, pyruvic acid, γ-ketovalerate, succinic acid, acetoacetic acid, gluconic acid, ascorbic acid, phthalic acid, salicylic acid, maleic acid, malic acid, fumaric acid, acrylic acid, thioglycolic acid, 2-hydroxy-4-methylthiobutyric acid, glutamic acid, N-acetylglutamic acid, alanine, glycine, cysteine, histidine, aspartic acid, N-acetylaspartic acid, 4-aminobutyric acid, 1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid (E DTA), N-dioxane (NTA), iminodiacetic acid (IDA), N-(2-hydroxyethyl)ethylenediamine-N,N′,N′-triacetic acid (HEDTA), diethylenetriaminepentaacetic acid (DTPA), N-dihydroxyethylglycine, tris(hydroxymethyl)methylglycine, 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP or etidronic acid), N-dioxanetri(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), 4-sulfophthalic acid, 3-(N-morpholino)-2-hydroxy-1-propanesulfonic acid (MOPSO), 2-(4-pyridyl)ethanesulfonic acid, phenol-4-sulfonic acid, thiodiacetic acid, and diethanolic acid.
[0041] This is because the group of compounds has acidic and coordination properties.
[0042] The organic compound (or at least one thereof) may be selected from at least one of the following compounds: dimethylglyoxime, methyl acetoacetate, ethyl acetoacetate, ethyl lactate, methyl glycolate, ethyl glycolate, dimethyl malate, diethyl malate, dimethyl tartrate, diethyl tartrate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, methyl 3-(methylthio)propionate, ethyl 3-(methylthio)propionate, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol (molecular weight 200-1500 g / mol), propylene glycol, glycerol, 2-butoxyethanol, 2-(2-butoxyethoxy)ethanol, 2-(2-methoxyethoxy)ethanol, Triethylene glycol dimethyl ether, crown ether, acetophenone, 2,4-pentanedione, pentanone, glucose, fructose, sucrose, sorbitol, xylitol, mannitol, γ-valerolactone, propylene carbonate, octylamine, N,N-diethylformamide, N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, propionamide, 1-methyl-2-pyrrolidone, tetramethylurea, N,N′-dimethylurea, acetonitrile, lactamide, furfuryl alcohol, 2-furfural, 5-hydroxymethylfurfural, ethyl 3-hydroxybutyrate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, N,N,N′,N′-tetramethyltartrate, 3-hydroxypropionitrile, and N,N′-bis(2-hydroxyethyl)ethylenediamine.
[0043] This is because the group of compounds exhibits coordination properties.
[0044] Advantageously, the extraction solution also contains at least one inorganic acid, particularly phosphoric acid, nitric acid, or boric acid. This combination of coordinating organic compounds and inorganic acids has proven to be highly effective, especially by creating a favorable, sufficiently acidic environment that enables the efficient extraction of the target metal, particularly when the impregnation of the support using this solution must be carried out in an acidic medium, and even more so when the final catalyst must contain phosphorus, and especially when phosphoric acid is chosen.
[0045] The concentration of each organic compound in the extraction solution is defined such that the concentration of one or more organic compounds in the extraction solution is defined such that for each organic compound or for each of one or more organic compounds (when there are several), the molar ratio of organic compound to one or more extracted metals is 0.2-25, preferably 0.2-11, preferably 0.2-5, preferably 0.4-2, preferably 0.4-1.2.
[0046] Advantageously, the recycling according to the invention may include at least one step of treating the source catalyst prior to extraction via a liquid route, selected from at least one of the following treatments: decoking, separation of contaminant / impurity type compounds, and mechanical grinding. The purpose of these pretreatments is to make extraction more efficient through mechanical, physical, or chemical processes: grinding reduces the particle size of the source catalyst and increases the contact surface area between the particles and the extraction solution. The removal or reduction of coke and other contaminants proceeds in the same direction by improving / increasing the contact between the extraction solution and the metal to be extracted contained in the source catalyst.
[0047] Advantageously, recycling may include at least one step of treating the extracted solution of one or more metals prior to impregnation, selected from at least one of the following processes: concentration, dilution, or alteration of the solution composition by completely or partially adding or removing at least one compound. According to one embodiment, this or these treatment steps are selected only from concentration, dilution, or alteration of the solution composition by completely or partially adding or removing at least one compound.
[0048] The purpose of these post-treatments is to bring the extract solution to the conditions required for use as an impregnation solution. Concentration, by thereby removing at least a portion of the solvent / non-metallic compound from the solution, will make it more efficient and closer to the concentration required for impregnation in conventional methods of impregnating fresh catalysts. This is also true, for example, by providing the solution with the constituent elements of the catalyst to be produced, particularly by providing at least one metal that is not present in the solution or is present in insufficient quantities.
[0049] Therefore, the impregnation of the support can begin with a solution of one or more extracted metals, with a supplement of at least one of metals M1 and M2, optionally with a supplement of phosphorus, and optionally with a supplement of one or more organic additives. This is because those skilled in the art recommend adding organic additives to the hydrotreating catalyst to improve its activity. The supplement can be added beforehand to the solution of one or more extracted metals for premixing, or added separately from the solution of one or more extracted metals to the apparatus for impregnating the support. The supplement can be in liquid or non-liquid form; if added separately, it will be in liquid form; if added to the solution of one or more extracted metals before impregnation, it can be in liquid or solid form.
[0050] Optionally, the method according to the invention may further include the step of sulfur impregnation of the substrate: when the catalyst to be produced must contain sulfur, it is known that sulfur is introduced, wholly or partially, at the end of the production process, either in situ on the catalyst production line or in situ on the hydrotreating unit in the hydrotreating reactor, particularly during the start-up phase of the unit.
[0051] The method according to the invention may also include one or more heat treatment steps of the carrier once impregnated. It typically includes at least one drying-type heat treatment. It may also include calcination.
[0052] Typically provided after impregnation, in a manner known in the manufacture of new catalysts:
[0053] -Optional ripening steps,
[0054] -Drying or calcining
[0055] -Optional addition of organic additives
[0056] - and, with the addition of organic additives, drying again,
[0057] - and finally, optional vulcanization.
[0058] These steps, particularly the post-impregnation of organic additives, can therefore be carried out in a manner similar to that of the recycling catalyst of the present invention.
[0059] According to the invention, at least a portion of the impregnation solution can be reused after impregnation of the carrier, particularly as a supplement to the extraction solution. This thus limits the consumption of solvents and (optionally) organic compounds in the method.
[0060] According to the invention, a solution of one or more metals can be concentrated to remove at least a portion of the solvent and optionally at least a portion of the optional organic compound it contains, and then the thus removed portion of the solvent / organic compound can be reused as a supplement to the extraction solution. This reuse allows for limiting the consumption of solvent / organic compounds in the method.
[0061] According to one embodiment, the method according to the invention includes the following (sequential but not necessarily continuous) steps:
[0062] - At least one step (a1, a2, a3) of treating the source catalyst,
[0063] - Extract one or more metals (b) from the source catalyst using an extraction solution to obtain a solution of the extracted one or more metals.
[0064] - At least one optional step (c) to purify the solution of one or more metals extracted in step (b) to remove all or some of the possible impurities.
[0065] -At least one optional step (d) of concentrating and extracting a solution of one or more metals.
[0066] - At least one optional step (e) to adjust the composition of the solution of one or more metals extracted by step (b), (c), or (d).
[0067] - The carrier is impregnated (f) by a liquid route using an impregnation solution obtained from a solution of the extracted one or more metals obtained in steps (b), (c), (d), or (e) to obtain an impregnated substrate. The impregnation solution is optionally supplemented with one or more metals, phosphorus, and one or more organic additives. The extracted one or more metals are maintained in the liquid phase from extraction to impregnation (depending on whether steps (c), (d), and (e) are performed and the order in which they are performed).
[0068] -Optional vulcanization (g) of the impregnated carrier obtained in step (f).
[0069] It should be noted that step (b) is performed before step (f), and vulcanization (g) is performed after step (f). Optional steps (c), (d), and (e) are preferably performed in the order described above, i.e., step (c), then (d), then (e), but they can also be performed in a different order (e.g., (d), (c), (e) or (c), (e), (d) or (e), (c), (d)).
[0070] As described above, the purpose of the method according to the invention is to produce, more specifically, hydrotreating or hydrocracking catalysts.
[0071] The depleted catalyst used in the recycling method according to the invention can be pre-regenerated or restored before being recycled via liquid extraction of metal.
[0072] The catalyst to be produced preferably contains Mo and / or W as metal M1, and Ni and / or Co as metal M2. Its support is preferably based on silica and / or alumina, and preferably contains phosphorus and optionally sulfur. The source catalyst is of the same type as the catalyst to be produced and contains at least the same metal M1 and / or the same metal M2.
[0073] In the method according to the invention, the support impregnated with an impregnation solution obtained from a solution of one or more extracted metals may be pre-impregnated with a (conventional) impregnation solution. After impregnation with the impregnation solution according to the invention, the support may also be post-impregnated with a conventional impregnation solution. The term "conventional" impregnation solution should be understood as a "fresh" solution containing precursors of the catalyst's active phase components, particularly metal components, in a known manner. The purpose of this pre-impregnation and / or post-impregnation of the support is, in particular, to adjust the amount of metal, if necessary, so that the catalyst ultimately has the desired composition.
[0074] In the context of this invention, the support may also be a metal-poor catalyst of the type of regenerated / restored spent catalyst.
[0075] The present invention also relates to catalysts produced according to the above method, which may therefore contain one or more recycled metals entirely, or contain one or more recycled metals and “fresh” metals in part.
[0076] The present invention also relates to any hydrotreating or hydrocracking catalyst comprising a mixture of fresh catalyst particles (which are not obtained by recycling according to the present invention) and catalyst particles obtained by the recycling method of the present invention. Attached Figure Description
[0077] Figure 1 A block diagram showing a first alternative form of an apparatus for implementing the method according to the invention.
[0078] Figure 2 A block diagram showing a second alternative form of an apparatus for implementing the method according to the invention.
[0079] The accompanying drawings are highly schematic and do not necessarily represent all operations that may be involved in the method according to the invention. The same reference numerals in the figures refer to the same operations / components / devices.
[0080] Description of the implementation plan
[0081] definition
[0082] Chemical elements are classified into groups according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, edited by DRLide, 81st edition, 2000-2001). For example, Group VIII according to the CAS classification corresponds to the metals in columns 8, 9, and 10 according to the new IUPAC classification.
[0083] Source catalyst
[0084] In the non-limiting examples and detailed description of the invention, it is understood that the specifications and formulation of catalysts produced by recycling correspond to the "source" catalyst (minus its contaminants, coke, etc., which will gradually deactivate the catalyst).
[0085] Naturally, the production of a recycled catalyst from a source catalyst remains within the scope of this invention, wherein the source catalyst comprises:
[0086] - At least one metal shared with the recycling catalyst, but possibly not all of the metals shared with it.
[0087] - and / or one or more common metals in varying amounts,
[0088] - or even one or more common metals and one or more additional metals, which will not form part of the composition of the produced recycling catalyst.
[0089] Therefore, a source catalyst that does not have the same function as the recycled catalyst to be produced can be used, as long as they have at least one common metal (hydrotreatment catalyst, hydrocracking catalyst, Fischer-Tropsch catalyst), or a source catalyst with the same function can be used (e.g., a hydrotreatment catalyst in both cases).
[0090] This is because, as can be seen from the above, the composition of the catalyst produced can be adjusted by optional adjustment steps according to the invention, and the extraction steps according to the invention can be selected to be selective, that is, to operate to extract only one or more metals common to the catalyst to be produced from the source catalyst.
[0091] The explanation is as follows:
[0092] The source catalyst of the method according to the invention is a catalyst comprising at least one oxide support and at least one metal, preferably several metals. The term "source" according to the invention has been defined above.
[0093] The source catalyst comprises at least one metal belonging to Group VIII and / or at least one metal belonging to Group VIB, an oxide support, and optionally phosphorus. It may also contain, but is not limited to, coke and / or sulfur as described below.
[0094] A deoiling step is preferably performed before removing the degraded catalyst from hydrotreating and / or hydrocracking processes. The deoiling step typically involves contacting at least partially degraded catalyst with an inert gas stream (i.e., substantially oxygen-free) at a temperature of 300-400°C, preferably 300-350°C, for example, in a nitrogen atmosphere. The inert gas flow rate is 5-150 sl.h per unit volume of catalyst. -1 The process takes 3-7 hours. In an alternative form, the deoiling step can be carried out with light hydrocarbons, by steam treatment, or any other similar method.
[0095] The oxide support for the source catalyst in the method according to the invention is typically selected from porous solids such as alumina, silica, silica-alumina, and titanium oxide or magnesium oxide, used alone or as a mixture with alumina or silica-alumina.
[0096] In another preferred embodiment, the oxide present in the support of the source catalyst according to the method of the invention is silica-alumina, containing at least 50% by weight of alumina relative to the total weight of the composite support. The silica content in the support is at most 50% by weight relative to the total weight of the support, typically less than or equal to 45% by weight, preferably less than or equal to 40% by weight.
[0097] According to a particularly preferred alternative, the support for the source catalyst is composed of alumina, silica, or silica-alumina.
[0098] The oxide support may also advantageously contain an additional 0.1-80% by weight, preferably 0.1-50% by weight, of zeolite relative to the total weight of the support. In this case, all known zeolite sources and all related preparation methods can be incorporated. Preferably, the zeolite is selected from FAU, BEA, ISV, IWR, IWW, MEI, UWY, and more preferably from FAU and BEA, such as zeolite Y and / or β-zeolite, and particularly preferably, for example, USY and / or β-zeolite.
[0099] The carrier is advantageously provided in the form of beads, extrusions, granules or irregular and non-spherical agglomerates, the specific shape of which can be produced by a crushing step.
[0100] The active phase of the source catalyst preferably comprises at least one Group VIB metal and at least one Group VIII metal. The Group VIB metal present in the active phase of the catalyst is preferably selected from molybdenum and tungsten, or a mixture of these two elements. The Group VIII metal present in the active phase of the catalyst is preferably selected from cobalt, nickel, or a mixture of these two elements. The active phase of the catalyst is preferably selected from elemental combinations of nickel-molybdenum, cobalt-molybdenum, nickel-cobalt-molybdenum, nickel-tungsten, nickel-molybdenum-tungsten, and nickel-cobalt-tungsten.
[0101] The content of Group VIII metals is 1-10% by weight, preferably 1.5-9% by weight, and more preferably 2-8% by weight of Group VIII metal oxides relative to the total weight of the dry catalyst. When the metal is cobalt or nickel, the metal content is expressed as CoO and NiO, respectively.
[0102] The content of Group VIB metals is 5-40% by weight, preferably 8-35% by weight, and most preferably 10-30% by weight of Group VIB metal oxides relative to the total weight of the dry catalyst. When the metal is molybdenum or tungsten, the metal content is expressed as MoO3 and WO3, respectively.
[0103] When the catalyst contains two types of metals, the molar ratio of Group VIII metal to Group VIB metal in the catalyst is preferably 0.1 to 0.8, more preferably 0.15 to 0.6, even more preferably 0.2 to 0.6, or 0.3 to 0.5.
[0104] The source catalyst of the method according to the invention may also contain phosphorus as a dopant. A dopant is an added element that does not exhibit any catalytic properties on its own, but increases the catalytic activity of the active phase.
[0105] The phosphorus content in the source catalyst is preferably from 0.1% to 20% by weight relative to the total weight of the dried catalyst, expressed as P2O5, more preferably from 0.2% to 15% by weight, expressed as P2O5, and very preferably from 0.3% to 8% by weight, expressed as P2O5.
[0106] The molar ratio of phosphorus to Group VIB elements in the catalyst is greater than or equal to 0.05, preferably greater than or equal to 0.07, more preferably 0.08-1, more preferably 0.01-0.9, and very preferably 0.15-0.6.
[0107] The source catalyst of the method according to the invention may contain sulfur. The sulfur content in the source catalyst is preferably 1% to 15% by weight, more preferably 2% to 12% by weight, and very preferably 4% to 10% by weight, expressed as an element relative to the total weight of the dried catalyst. The sulfur content is measured by elemental analysis according to ASTM D5373.
[0108] The source catalyst of the method according to the invention may contain coke, particularly when it has not yet been regenerated. It should be noted that the term "coke" in this patent application refers to a hydrocarbon-based substance that is deposited on the catalyst surface during catalyst use, is highly cyclized and fused, and has a graphite-like appearance.
[0109] The coke content, expressed as a percentage by weight of carbon, can be 5-20% by weight, preferably 6-16% by weight, and especially 7-14% by weight, relative to the total weight of the dried catalyst. The coke content is determined according to the ASTM D5373 method.
[0110] Optionally, the source catalyst may additionally exhibit low levels of contaminants, such as silicon, arsenic, iron, sodium or chlorine, or sulfur, generated from feedstocks treated by a fresh catalyst (which produces the source catalyst).
[0111] Preferably, the silicon content of the source catalyst (in addition to the silicon content that may be present on the fresh catalyst) is less than 2% by weight relative to the total weight of the source catalyst, and very preferably less than 2000 ppm by weight.
[0112] Preferably, the arsenic content is less than 2000 ppm by weight relative to the total weight of the source catalyst, and most preferably less than 500 ppm by weight.
[0113] Preferably, the chlorine content is less than 2000 ppm by weight relative to the total weight of the regenerated catalyst, and most preferably less than 500 ppm by weight.
[0114] Preferably, the sulfur content is less than 2% by weight relative to the total weight of the source catalyst, and most preferably less than 2000 ppm by weight.
[0115] Very preferably, when the source catalyst is a regenerated catalyst, it is not contaminated, that is, it contains less than 100 ppm by weight of silicon (in addition to the silicon that may be present on the fresh catalyst), 100 ppm by weight of sodium (in addition to the sodium that may be present on the fresh catalyst), 50 ppm by weight of arsenic, 50 ppm by weight of iron and 50 ppm by weight of chlorine.
[0116] According to one embodiment of the invention, the source catalyst of the method according to the invention may be contained in or consist of fine powder generated during the operation of discharging the spent catalyst in an industrial unit from which the spent catalyst is removed, or during the regeneration process.
[0117] According to another embodiment, the source catalyst of the method according to the invention comprises, or is composed of, fine powders and / or oversized products produced by various unit operations of a novel catalyst.
[0118] Steps of the method for manufacturing a catalyst based on recycled metals according to the present invention
[0119] - Step (a) (optional): One or more steps prior to extraction
[0120] When the source catalyst is a degraded catalyst, it is generated during the hydrotreatment of hydrocarbon fractions containing sulfur and other contaminants such as silicon, arsenic, chlorine, iron, sodium, or nitrogen, particularly in hydrodesulfurization or hydroconversion processes. The formation of coke and / or the deposition of contaminants converts fresh catalyst into at least partially degraded catalyst.
[0121] Optional step (a) includes, prior to step (b) of metal extraction, removing all or part of one or more impurities that may be contained in the source catalyst by any method known to those skilled in the art. Preferably, step (a) includes a regeneration step to remove all or part of the coke, sulfur and / or chlorine, as described in detail below, or a heat treatment step under a gaseous stream containing hydrogen sulfide, which is particularly carried out to remove arsenic.
[0122] Example of step (a1): Regeneration
[0123] A regeneration step is performed to remove coke and sulfur from a catalyst that has been at least partially degraded: this step allows for the removal of all or part of the coke, sulfur and / or chlorine that may have deposited on the catalyst.
[0124] Even if this is possible, regeneration is preferably not carried out by keeping the loaded catalyst in the hydrotreating reactor (in-situ regeneration). Preferably, at least partially depleted catalyst is therefore removed from the reactor and sent to a regeneration unit for regeneration (non-in-situ regeneration).
[0125] The regeneration step is typically carried out in an oxygen-containing gaseous stream, usually air. The water content in the gas is typically 0-50% by weight. The gas flow rate, expressed as the flow rate per unit volume of at least partially depleted catalyst, is preferably 20-2000 sl·h. -1 More preferably 30-1000Sl.h -1 Especially preferred is 40-500Sl.h -1 The regeneration duration is preferably 2 hours or longer, more preferably 2.5 hours or longer, and particularly preferably 3 hours or longer. The regeneration of at least partially depleted catalyst is generally carried out at a temperature of 320°C to 550°C, preferably 360°C to 500°C.
[0126] The regenerated source catalyst consists of an oxide support, an active phase formed of at least one Group VIB metal and at least one Group VIII metal, and optionally phosphorus from the source catalyst. This regenerated catalyst is characterized by a specific surface area of 20 to 300 m². 2 / g, preferably 30 to 280m 2 / g, preferably 40 to 260m 2 / g, with a highly preferred concentration of 80 to 250 mg 2 / g.
[0127] The pore volume of the source catalyst (here, the depleted and regenerated catalyst) is typically 0.1 cm³. 3 / g-1.3cm 3 / g, preferably 0.2cm 3 / g-1.1cm 3 / g.
[0128] The regenerated catalyst obtained in the regeneration step contains residual carbon, the content of which is less than 3% by weight relative to the total weight of the regenerated catalyst, preferably 0-2.9% by weight, more preferably 0-2.0% by weight, and particularly preferably 0-1.0% by weight. It should be noted that the term "residual carbon" in this patent application refers to carbon (coke) remaining in the regenerated catalyst after the regeneration of a failed hydrotreating catalyst. The residual carbon content in the regenerated hydrotreating catalyst is measured according to the ASTM D5373 method.
[0129] An example of step (a2): heat treatment in a gaseous stream containing hydrogen sulfide (optionally, a method that accumulates along with the regeneration in the previous step (a1)).
[0130] All or part of the elemental arsenic or arsenic compounds that may be present in the source catalyst can be removed by passing a stream of hydrogen sulfide and vapor or inert gas through a solid at a temperature of 300-750°C. During this process, the arsenic contained in the source catalyst forms arsenic sulfide (having the formula As₂S₃), which volatilizes from the solid. This reaction is preferably carried out by fluidizing the solid in a stream of hydrogen sulfide and vapor or inert gas. When using a mixture of hydrogen sulfide and inert gas, the inert gas is preferably nitrogen, carbon dioxide, or a combustion gas.
[0131] Example of step (a3): Optional pre-grinding
[0132] Prior to extraction, the source catalyst may advantageously undergo an optional grinding step to promote the kinetics of metal extraction during extraction step (b) of the method according to the invention. In this case, the step includes a first optional stage (a3) of conditioning the source catalyst with at least one grinding to obtain source catalyst particles with a size of at most 1 mm. Of course, several successive grinding steps can be performed to achieve the target particle size. Any method known to those skilled in the art can be used to perform this crushing or grinding step, for example, using a ball mill or a rotary cutting mill. Preferably, the size of the source catalyst used during extraction step (b) according to the invention is 1 to 1000 micrometers (1 mm), preferably 80 to 500 micrometers, and more preferably 100 to 400 micrometers. Most often, the ground source catalyst is transported to the extraction zone by any means known to those skilled in the art, particularly by a screw conveyor or by pneumatic conveying.
[0133] - Extraction step (b)
[0134] According to this step, the source catalyst is contacted with an extraction solution containing at least one organic compound, which preferably has coordination and optional acidic properties (e.g., at least one compound having both properties, or a combination of at least one acidic compound and at least one coordination compound, or only at least one coordination compound).
[0135] The extraction solution according to the invention can contain any polar protic solvent known to those skilled in the art. Polar protic solvents are preferred, for example, those selected from methanol, ethanol, and water, or water-ethanol or water-methanol mixtures. Very preferably, the solvent used in the impregnation solution is composed of water. In the case of an aqueous solution, the pH of the solution can be changed by optionally adding an acid or a base. The pH of the extraction solution is typically 0.1-8.5, preferably 0.5-6, and most preferably 1-4.
[0136] Typically, organic compounds are selected from compounds containing one or more chemical functional groups, said chemical functional groups being selected from carboxylic acids, phosphonic acids, sulfonic acids, alcohols, thiols, thioethers, sulfones, sulfoxides, ethers, aldehydes, ketones, esters, carbonates, amines, nitriles, imides, oximes, ureas, and amides, or from compounds containing a furan ring or sugars.
[0137] Examples of coordination organic compounds, as well as coordination and acidic organic compounds, have already been listed above; therefore, these lists will not be repeated here.
[0138] The concentration of each organic compound in the extraction solution is limited such that the molar ratio of organic compound to extracted metal is 0.2-25, preferably 0.2-11, preferably 0.2-5, preferably 0.4-2, and preferably 0.4-1.2.
[0139] When several organic compounds are present, various molar ratios apply to each organic compound present.
[0140] In one embodiment of the invention, the extraction solution may also contain phosphorus. The presence of phosphorus in the extraction solution promotes the extraction of metals, particularly molybdenum, due to the high stability of the heteropolyanion formed by the metal and phosphorus. Adding phosphorus in the form of phosphoric acid (H3PO4) also allows for a reduction in the pH of the solution, which generally also favors the extraction of metals contained in the source catalyst. Inorganic acids other than phosphoric acid, particularly nitric acid or boric acid, can also be used.
[0141] The preferred phosphorus precursor is phosphate (H3PO4), but its esters and salts, such as ammonium phosphate, are also suitable, as are polyphosphates. Without being bound by any theory, it seems that the combination of phosphate with an organic acid with an acidity constant pKa greater than 1.5—that is, a weak organic acid—allows for a synergistic effect to be observed at the metal extraction level, which is unpredictable when using phosphate or the organic acid alone. Extraction in the presence of two specific acids allows for very good dissolution of the metal phase.
[0142] In one embodiment of the invention, the extraction solution may further contain an oxidizing agent to promote metal extraction. Preferably, the oxidizing agent contained in the extraction solution is hydrogen peroxide. When an oxidizing agent is present, the concentration is typically 0.1-5.0 mol / L. -1 .
[0143] Typically, the operating conditions of step (b) are selected to maximize the extraction of the metal contained in the source catalyst, while minimizing the dissolution of one or more metals contained in the support of the source catalyst, and simultaneously limiting the amount of organic compound so that the amount of organic compound is not excessive relative to the optimal amount of organic compound required in the impregnation step, in order to obtain a high-performance catalyst. It is also sought to minimize the amount of extraction solution used so as to obtain the most concentrated metal solution possible at the end of the extraction: therefore, the need to concentrate the solution before using it in the impregnation solution or as an impregnation solution is limited.
[0144] Contact with the extraction solution should be performed under the following conditions:
[0145] -Temperature: 10-150℃, especially 15-95℃
[0146] - Pressure: Atmospheric pressure to 20 bar, especially atmospheric pressure or at most 10 bar.
[0147] - Duration: 1 minute to 20 hours, preferably 5 to 300 minutes, preferably 5 to 180 minutes.
[0148] Preferably, one or more devices performing the contact operation do not have heating equipment, and the temperature of the contact operation is regulated by the temperature of the extraction solution. The temperature of the extraction solution can be 15°C to 95°C, 20°C to 95°C, or 25°C to 95°C, and preferably 30°C to 90°C, and more preferably 50°C to 85°C. Thus, for this particular contact step, it can be at ambient temperature or it has been heated. It can also be at a given temperature, particularly above ambient temperature, because it is at least partially derived from the recycling of liquid effluent generated in the method according to the invention and already within that temperature range.
[0149] As described above, to achieve the desired effect, the amount of extraction solution used in this step is preferably as low as possible. Preferably, this step (b) is performed by contacting the source catalyst with a solution having a volume 1.5 to 60 times that of the source catalyst. Preferably, the volume of the solution is 2 to 30 times that of the source catalyst, more preferably 2 to 20 times that of the source catalyst.
[0150] For step (b) to be carried out in a continuous mode, all modes of contact, whether in a single step or in several steps, are possible, depending on whether the contact occurs in parallel, counter-current, or cross-current flow. Intermittent contact operation can also be provided. As an illustration, the contact operation can be carried out by impregnation or under the flow of the extraction solution, for example by distributing a trickle of the extraction solution onto a source catalyst that is optionally in motion.
[0151] At the end of step (b), the solution is separated from the solid residue to obtain, on the one hand, the leachable catalyst, and on the other hand, a metal solution to be used in steps (c), (d), (e), or (f). Preferably, the residual metal content of the leachable catalyst (the sum of the contents of the different metals contained in the leachable catalyst, expressed as oxides) is less than 10% by weight, preferably less than 5% by weight, and very preferably less than 2% by weight. Any liquid / solid separation method can be used, such as by filtration or by discharge, for example by gravity. Preferably, the separation step is carried out using a pressure filter.
[0152] - Step (c) (optional): Purification
[0153] The optional step (c) of the metal solution produced in purification step (b) serves to remove all or part of the impurities that may be contained in the metal solution, particularly those arising from impurities that may be present on the source catalyst or related to the partial dissolution of the catalyst support. Step (c) may be performed in a single step or in several consecutive steps.
[0154] If the metal solution contains suspended solids after the separation step, at the end of step (b), any known method for removing these suspended solids can be used during step (c). Preferably, this removal is carried out by filtration (e.g., microfiltration and ultrafiltration on a cross-flow filter). Other methods include centrifugation or coagulation.
[0155] For dissolved impurities, such as arsenates or arsenites, all known methods can be used during step (c), particularly and preferably adsorption, precipitation and extraction by solvent on a solid, while taking care not to remove the target metal that has already been extracted.
[0156] - Step (d) (optional): Concentration
[0157] Step (d) involves concentrating the metal solution obtained in step (b) or (c) by removing a portion of the solvent and all or part of the organic compounds contained in the metal solution. This step may be necessary if the metal concentration is too low relative to the concentration required for impregnation. Any known method for removing a portion of the solvent from the solution is conceivable. Step (d) may be performed in a single step or in several consecutive steps. All or part of the solvent (containing or not containing organic compounds) extracted from the metal solution in step (d) may be recycled to extraction step (b).
[0158] Preferably, and particularly when the metal solution is an aqueous solution, step (d) is carried out by evaporation and concentration. In this case, neutralization is preferably performed to bring the effluent into the evaporator at a pH range of 5-7. This pH adjustment allows for limiting co-distillation unless it is desired that the latter be used for the co-removal of the solvent and some organic compounds, and to avoid precipitation of metal oxides as much as possible. Preferably, all or part of the distillate is recycled to extraction step (b).
[0159] When only partial solvent removal is required, the preferred technology, in addition to evaporation and concentration, is membrane technology, with nanofiltration, reverse osmosis, total evaporation, solvent extraction, or low-temperature concentration being highly preferred.
[0160] When using solvents and one or more organic compounds, the preferred technique when it is necessary to remove them is evaporation and concentration.
[0161] - Step (e) for adjusting the composition of the metal solution (optional)
[0162] Step (e) involves altering the metal solution obtained from steps (b), (c), or (d) by adding and / or removing certain one or more components. Metal precursors and / or phosphorus precursors and / or organic additives may be added. If desired, all or part of the organic compound used for metal extraction may also be removed. The aim is to obtain a metal solution whose composition corresponds to the composition required in the impregnation step (f) for synthesizing the catalyst according to the invention.
[0163] The case of metals:
[0164] Even if it is desired that the catalyst according to the invention has the same formulation as the source catalyst, the ratio between the metals in the metal solution can be adjusted, on the one hand because the purification step (a) of the catalyst can change the initial content of the metals in the source catalyst, and on the other hand because the extraction step (b) can produce different extraction rates for each metal.
[0165] The ratio between the metals is adjusted by adding a supplementary solution containing one or more of the metals, or by directly dissolving one or more metal precursors in the metal solution obtained from steps (b), (c), or (d), with the latter being preferred. In the metal solution obtained from step (e) described above, the molar ratio of Group VIII metals to Group VIB metals is generally 0.1-0.8, preferably 0.15-0.6.
[0166] For example, in the molybdenum source, oxides and hydroxides, molybdic acid and its salts, especially ammonium salts, such as ammonium molybdate or ammonium heptamolybdate, phosphomolybdic acid (H3PMo) can be used. 12 O 40 ) and its salts, and optionally silicomolybdic acid (H4SiMo)12 O 40 Molybdenum source can also be any heteropoly compound of the Keggin, vacant Keggin, substituted Keggin, Dawson, Anderson, or Strandberg type, for example. Preferably, molybdenum trioxide and Keggin, vacant Keggin, substituted Keggin, and Strandberg type heteropoly compounds are used.
[0167] The tungsten precursors that can be used are also well known to those skilled in the art. For example, in the tungsten source, oxides and hydroxides, tungstic acid and its salts, especially ammonium salts, such as ammonium tungstate or ammonium metatungstate, phosphotungstic acid and its salts, and optionally silicotungstic acid (H4SiW) can be used. 12 O 40 ) and its salts. The tungsten source can also be any heteropoly compound of the Keggin, vacant Keggin, substituted Keggin, or Dawson type, for example. Oxides and ammonium salts, such as ammonium metatungstate, or heteropoly anions of the Keggin, vacant Keggin, or substituted Keggin type, are preferred.
[0168] Cobalt precursors that can be used are advantageously selected from, for example, oxides, hydroxides, basic carbonates, carbonates, and nitrates. Cobalt hydroxide and cobalt carbonate are preferred. Cobalt acetoacetate may also be considered.
[0169] Nickel precursors that can be used are advantageously selected from, for example, oxides, hydroxides, basic carbonates, carbonates, and nitrates. Nickel acetoacetate may also be considered.
[0170] Phosphorus:
[0171] A phosphorus precursor can be used in step (b). If the phosphorus / metal ratio of the metal solution obtained from steps (b), (c), or (d) is lower than the phosphorus / metal ratio required for the impregnation solution in step (f), a phosphorus precursor, the same or different from the phosphorus precursor optionally used in step (b), can be added to the metal solution during step (e). This is especially true when no phosphorus compound / precursor is added in step (b), or when it is at least partially consumed by the support (when the support contains alumina) to form aluminophosphate. In this case, the molar ratio of phosphorus to Group VIB metal is 0.1-2.5 mol / mol, preferably 0.1-2.0 mol / mol, more preferably 0.1-1.0 mol / mol, or 0.15-0.8 mol / mol, or 0.2-0.6 mol / mol.
[0172] The preferred phosphorus precursor is phosphate (H3PO4), but its esters and salts, such as ammonium phosphate, are also suitable, just like polyphosphates. Phosphorus can also be introduced simultaneously with one or more Group VIB elements in the form of Keggin, vacant Keggin, substituted Keggin, or Strandberg heteropolyanions.
[0173] Regarding organic additives:
[0174] Those skilled in the art have recommended the addition of organic additives to hydrotreating catalysts to improve their activity. These are known to improve metal dispersion on the support surface and / or play a beneficial role in the sulfidation process of the catalyst. Therefore, one or more organic additives known to those skilled in the art can be advantageously added at this step. Typically, the amount of each organic additive added is limited such that the additive / metal molar ratio in the impregnation solution is 0.1 to 1.
[0175] Patent FR3083134 describes examples of potentially suitable organic additives that can be used in aqueous form and therefore can be added to the impregnation solution (in step (e) or step (f)). Patent FR3083131 also describes examples of potentially suitable organic additives, but which will be added separately during the pre-impregnation or post-impregnation of the carrier.
[0176] Organic compounds used for metal extraction:
[0177] The metal solution obtained from steps (b), (c), or (d) may contain an excess of organic compound relative to the desired impregnation solution. The ratio of organic compound to metal can be adjusted in two ways. The first method involves adding a concentrated solution of the metal precursor or directly dissolving these metal precursors to achieve the desired ratio. In this case, the final catalyst obtained will contain a mixture of recycled and new metals.
[0178] If the organic compound is in excessive excess and the first approach cannot be used (i.e., the amount of recycled metal incorporated into the final catalyst is insignificant, for example, less than 5% of the total metal), then the second approach involves removing all or part of the excess organic compound from the metal solution. In this case, the organic compound can be recycled to step (b). For this purpose, any method known to those skilled in the art for separating organic molecules from the metal solution is envisioned.
[0179] - Step (f): Impregnation
[0180] According to step (f), the porous support or catalyst already containing one or more metals (as defined above for "support") is contacted with the solution obtained in steps (b), (c), (d), or (e). According to step (f), the contacting of the porous support or catalyst with the metal salt in the solution can be performed by any known method, such as ion exchange, dry impregnation, over-impregnation, vapor deposition, etc. The contacting operation can be performed in one step or in several consecutive steps.
[0181] According to a preferred method, step (f) of contacting the carrier with the metal solution is carried out by over-impregnation or by dry impregnation.
[0182] Balanced or over-impregnation involves immersing the support or catalyst in a solution with a volume larger than (typically significantly larger than) the pore volume of the support or catalyst. Dry impregnation itself involves introducing an impregnation solution with a volume equal to or slightly smaller than the pore volume of the support or catalyst. Dry impregnation allows all components of the impregnation solution to be deposited on a given support or catalyst.
[0183] Step (f) can advantageously be carried out by one or more over-immersions in the solution or preferably by one or more dry immersions, and for example by using a single over-immersion in the immersion solution.
[0184] Step (f) is carried out at a temperature typically between 10°C and 95°C, and at a pressure between atmospheric pressure and 20 bar, preferably at atmospheric pressure, and is preferably carried out for a period of 1 minute to 20 hours, preferably 1 to 300 minutes. Step (f) is preferably carried out at a temperature between 10°C and 60°C, preferably at ambient temperature.
[0185] Advantageously, after each impregnation step, the impregnated support or catalyst is aged. Aging allows the impregnation solution to be uniformly dispersed within the support or catalyst.
[0186] Any curing step described in this invention is advantageously carried out at atmospheric pressure, in a water-saturated atmosphere, and at a temperature of 17°C to 50°C, and preferably at ambient temperature. Typically, a curing time of ten minutes to forty-eight hours, and preferably thirty minutes to six hours, is sufficient.
[0187] Advantageously, step (f) is followed by a drying step at a temperature below 200°C, preferably 50-180°C, more preferably 70-150°C, and very preferably 75-130°C. The drying step preferably lasts from 10 minutes to 24 hours. Longer times are not excluded, but do not necessarily contribute to improvement. The drying step can be carried out by any known technique. It is advantageously carried out at atmospheric pressure or under reduced pressure. Preferably, the step is carried out at atmospheric pressure. It is advantageously carried out using hot air or any other hot gas. Preferably, the gas used is air or an inert gas, such as argon or nitrogen. Very preferably, drying is carried out in the presence of nitrogen and / or air, and advantageously in a crossflow bed.
[0188] According to one alternative approach, drying is advantageously performed to preferably retain at least 30% by weight of the organic additives introduced during step (e) and / or step (f). Preferably, this amount is greater than 50% by weight, more preferably greater than 70% by weight, based on the carbon remaining on the catalyst.
[0189] According to an alternative form, drying is advantageously carried out to preferably retain at least 30% by weight of the organic extractable compound introduced during step (f); preferably, this amount is greater than 50% by weight, more preferably greater than 70% by weight, based on the carbon remaining on the catalyst.
[0190] Optionally, a calcination step may follow drying. This may be the case, for example, if it is necessary to remove all or part of one or more organic extractable compounds. According to this alternative, at the end of the drying step, the calcination step is carried out at a temperature of 200°C to 600°C, preferably 250°C to 550°C, under an inert atmosphere (e.g., nitrogen) or an oxygen-containing atmosphere (e.g., air). The duration of this heat treatment is typically 0.5 hours to 16 hours, preferably 1 hour to 5 hours. After this treatment, the active phase is therefore typically present in oxide form; thus, the heteropolyanions are converted into oxides. Similarly, the catalyst no longer contains or contains very little of the organic extractable compounds and organic additives. However, the introduction of organic additives during its preparation allows for improved dispersion of the active phase, resulting in a more active catalyst.
[0191] Preferably, the catalyst is not calcined.
[0192] In embodiments in which step (f) is carried out by at least two impregnation cycles, drying and optional calcination are advantageously performed after each impregnation.
[0193] The oxide support used in step (f) of the method according to the invention is typically selected from the following porous solids: alumina, silica, silica-alumina, and titanium oxide or magnesium oxide used alone or as a mixture with alumina or silica-alumina.
[0194] The oxide support advantageously has a total pore volume of 0.1-1.5 ml / g, preferably 0.4-1.1 ml / g.
[0195] The specific surface area of the oxide support is advantageously 5-400 m². 2 .g -1 10-350m is preferred 2 .g -1 More preferably 40-350m 2 .g -1 In this invention, the specific surface area is determined by the BET method according to standard ASTM D3663.
[0196] The oxide support of the recycled catalyst according to the present invention can have the same properties as the support of the source catalyst, as described above.
[0197] Preferably, the oxide support is selected from silica, the transition alumina family, and silica-alumina. Very preferably, the oxide support is substantially composed of at least one transition alumina, that is, it contains at least 51% by weight, preferably at least 60% by weight, very preferably at least 80% by weight, or even at least 90% by weight of transition alumina. It is preferably composed only of transition alumina. Preferably, the oxide support of the catalyst according to the method of the invention is γ-phase alumina.
[0198] In another preferred embodiment, the oxide present in the support of the catalyst according to the method of the invention is silica-alumina, containing at least 50% by weight of alumina relative to the total weight of the composite support. The silica content in the support is at most 50% by weight relative to the total weight of the support, typically less than or equal to 45% by weight, preferably less than or equal to 40% by weight.
[0199] Silicon sources are well known. Examples include silicic acid, silicon dioxide in powder or colloidal form (silica sol), or tetraethyl orthosilicate Si(OEt)4.
[0200] When the catalyst is supported on silica, it contains more than 50% by weight of silica relative to the total weight of the support, and typically it contains only silica.
[0201] According to a particularly preferred alternative, the carrier consists of alumina, silicon dioxide, or a silicon dioxide-alumina mixture.
[0202] The oxide support may also advantageously contain an additional 0.1-80% by weight, preferably 0.1-50% by weight, of zeolite relative to the total weight of the support. In this case, any zeolite source and any associated preparation method known to those skilled in the art can be incorporated. Preferably, the zeolite is selected from FAU, BEA, ISV, IWR, IWW, MEI, UWY, and more preferably from FAU and BEA, such as zeolite Y and / or β-zeolite, and particularly preferably, for example, USY and / or β-zeolite.
[0203] In addition to those that may be introduced in steps (e) and / or (f), the support may also contain at least a portion of one or more Group VIB and Group VIII metals and / or at least a portion of phosphorus and / or at least a portion of sulfur and / or at least a portion of one or more organic additives. These are introduced, for example, during the preparation of the support. This is referred to as a “pre-impregnated” support.
[0204] One or more metals may also be added to a carrier that has already been impregnated with the impregnation solution according to the invention. This is referred to as a "post-impregnated" carrier.
[0205] In both cases, the purpose of the "pre-impregnated" or "post-impregnated" carrier is the same: the problem is to adjust the metal content of the final catalyst by adding a certain amount of one or more metals present in the impregnation solution according to the invention, or by adding one or more other metals in a separate step, particularly before and / or after the impregnation step (f) with the impregnation solution of the invention, with another impregnation solution.
[0206] The support can even be a catalyst, thus allowing it to be further "loaded" with metal. It can be a catalyst that is already metal-depleted, particularly the exhausted catalyst itself, optionally regenerated, and then optionally restored.
[0207] The carrier is advantageously provided in the form of beads, extrusions, granules or irregular and non-spherical agglomerates, the specific shape of which can be produced by a crushing step.
[0208] The active phase of the recycled catalyst, which is the target of the method according to the invention, is generally of the type already described above as a "depleted" catalyst. It is also possible to seek to produce a recycled catalyst according to the invention containing a lower metal loading than the depleted catalyst used, particularly if this allows the extract solution to be used without concentration prior to impregnation. The recycled catalyst can then be used differently from the depleted catalyst from which it is derived (for different hydrocarbon feedstocks) (e.g., a catalyst with 20 wt% Mo, expressed as MoO3, relative to the weight of the dry catalyst, can be used for the hydrotreating of distillate, while a catalyst containing a lower Mo loading of -10 wt% Mo, expressed as MoO3, can be used for the hydrotreating of naphtha).
[0209] The amount of recycled metal contained in the catalyst according to the invention is 1-100% by weight of the metal contained in the catalyst produced according to the invention, preferably 10-100% by weight, preferably 20-100% by weight, and more preferably 50-100% by weight of the metal contained in the catalyst according to the invention.
[0210] It should be emphasized that the catalyst produced according to the present invention can have a different formulation and different amounts of metal and different ratios between metals than the spent catalyst used for metal recovery: thus, as described above, according to the present invention, a spent catalyst containing a high metal loading can be used to produce a catalyst containing a lower metal loading (or vice versa). This allows the step of concentrating the solution after the extraction step (b) to be avoided, if appropriate, or at least its intensity / duration can be reduced.
[0211] It should also be noted that the catalyst produced according to the present invention may be an additive, that is, it may be impregnated with one or more organic additives before the final sulfidation in step (g), the function of which is to improve the catalytic activity relative to the catalyst without additives. It should be understood that, preferably, no calcination step is performed after its introduction.
[0212] - Step (g) (optional): Vulcanization
[0213] Before use, the catalyst produced by the method according to the invention may undergo an optional sulfidation step. Sulfidation is preferably carried out in a sulfur-reducing medium, that is, in the presence of H2S and hydrogen, to convert the metal oxide into sulfides, such as MoS2 and Co9S8. Sulfidation is carried out by injecting a stream containing H2S and hydrogen, or a sulfur compound that can decompose to yield H2S in the presence of a catalyst and hydrogen, onto the catalyst. Polysulfides, such as dimethyl disulfide (DMDS), are commonly used H2S precursors for sulfidation catalysts. Sulfur may also be derived from the feedstock. The temperature is adjusted to allow H2S to react with the metal oxide to form metal sulfides. This sulfidation can be carried out in situ or ex-situ (inside or outside the reactor) in a reactor of the hydrotreating or hydroconversion method according to the invention at a temperature of 200-600°C and more preferably 300-500°C.
[0214] Figure 1 The first alternative form of the method according to the invention is shown in the form of a block diagram:
[0215] The source catalyst is fed to purification unit 2 via line 1: optional step (a1). The effluent containing contaminants is removed via line 3, while the purified catalyst is taken out via line 4 and fed to mill 5: optional step (a3). The pulverized catalyst 6 is fed to extraction unit 9 to recover the metal-rich metal solution 11: this is the extraction step (b). For this purpose, an extraction solution 8 containing organic compounds is used. This extraction solution 8 can be a mixture of recirculated extraction solution 13 and supplementary extraction solution 7, which allows for adjustment of the composition of the catalyst to be produced, particularly the ratio and amount of metals. Extraction unit 9 operates in a temperature range of 10 to 150°C, particularly 10 to 95°C, and a pressure range of 1 to 20 bar.
[0216] Unit 9 also produces effluent 10, which contains, in particular, the source / depleted catalyst support and residual metal. The metal solution 11 is fed to concentration unit 12; this is an optional concentration step (d), which allows for the preparation of a solution 14 with a higher metal loading. Concentration unit 12 also allows for the recovery of the lean metal portion recirculated through line 13 (e.g., by condensation of the evaporation portion in the case of concentration by evaporation) to form part of the extract solution 8. A supplementary solution 16, which may contain metals, phosphorus, and organic additives, is added to solution 14 to adjust the composition of the metal solution: this is the conditioning step (e). The mixture constituting the impregnation solution and the catalyst support 15 are then used in impregnation unit 17 to deposit the metal onto the catalyst support: this is the impregnation step (f). Following optional aging, heat treatment, and optional post-addition steps known to those skilled in the art, the impregnated catalyst 18 can finally be fed to the sulfidation unit 19, whereby the metal oxides can be converted into their sulfide forms: this is the sulfidation step (g), which is optional (it can also be carried out in situ subsequently in a hydrotreating / hydroconversion reactor). Catalyst 20 is thus obtained.
[0217] Figure 2 A second alternative form of the method according to the invention is shown in block diagram form. It is close to the first alternative form; only two differences from the first alternative form are shown below:
[0218] - Step (d) to remove the concentrated metal extract solution
[0219] The outlet solution of the impregnation unit 17 is reused to form part of the extraction solution 8, particularly the main part or the majority of it.
[0220] Example 1
[0221] The starting material was a degraded "CoMoP" catalyst (used in hydrotreating processes) containing molybdenum, cobalt, and phosphorus (deposited on an alumina support). It was pre-regenerated at 450°C under a dry air stream for 4 hours.
[0222] The regenerated catalyst contains molybdenum, phosphorus, and cobalt. The composition of the catalyst is expressed in the form of oxides and is relative to the weight of the dry catalyst: 21.6 wt% MoO3 (14.4 wt% molybdenum), 3.7 wt% CoO (2.9 wt% cobalt, i.e., Co / Mo molar ratio equal to 0.33), and 3.2 wt% P2O5 (1.4 wt% phosphorus, i.e., P / Mo molar ratio equal to 0.3).
[0223] The extraction of molybdenum and cobalt from the regenerated catalyst was carried out on a laboratory scale: 40 g of the regenerated catalyst (referred to as the source catalyst), pre-ground to a particle size of 100–300 micrometers, and 200 g of the extraction solution were introduced into a round-bottom flask. The extraction solution was an aqueous solution containing 4 wt% glutaric acid. The pH of the mixture was adjusted to 2.0 by adding phosphoric acid. The amounts of organic acid (glutaric acid) and inorganic acid (phosphoric acid) were chosen so that they would not need to be removed / reduced subsequently in the extraction solution used as an impregnation solution. The round-bottom flask, equipped with a reflux condenser to limit evaporative water loss, was then placed in a water bath heated to 85°C, and the mixture was stirred at 200 rpm for 6 hours with a magnetic rod. The mixture was then filtered through sintered glass with a porosity of 5 to recover both the multimetallic solution and the solid residue. Solution analysis showed that it contained 25.9 g / L molybdenum and 4.6 g / L cobalt. Therefore, the calculated extraction rates of Mo and Co were 90% and 80%, respectively.
[0224] Adjust the glutaric acid / Mo and Co / Mo ratios of the multimetallic solution to obtain a solution suitable for impregnating the new carrier.
[0225] To this end, the polymetallic solution was first concentrated by evaporation. This removed 80% of the solvent (water) to obtain 40 ml of a solution containing 13.0% by weight of molybdenum. The concentrated solution had a glutaric acid / Mo molar ratio of 1.1, compatible with the impregnation solution. The Co / Mo molar ratio was 0.3. Therefore, a sufficient amount of the cobalt precursor Co(OH)₂, i.e., 180 mg, was added to adjust this ratio to 0.4.
[0226] Finally, 40 ml of the resulting impregnation solution (pH 1.3) was used to impregnate 10 g of alumina support for three hours at ambient temperature using an excess impregnation method. After aging in a humid atmosphere at ambient temperature for 16 hours and drying at 120 °C for 2 hours, the resulting recycled catalyst had a formulation of 21.1 wt% MoO3, 3.6 wt% CoO, and 3.3 wt% P2O5, and contained 100% recycled Mo.
[0227] Thus, catalysts produced from recycled metals exhibit performance levels that are essentially equivalent to those of fresh catalysts without recycled metals.
Claims
1. A method for producing a recycling catalyst, said recycling catalyst comprising at least one metal M1 from Group VIB and / or at least one metal M2 from Group VIII, optionally phosphorus and / or sulfur, and a support based on one or more oxides, characterized in that... The method includes at least a portion of one or more metals of a recycled source catalyst, the source catalyst comprising metal M1 and / or metal M2 common to the recycled catalyst to be produced, the method comprising: - Extract metal M1 and / or metal M2 from the source catalyst by extraction solution to obtain a solution of one or more extracted metals, then - impregnate a support with an impregnation solution obtained from the solution of the one or more extracted metals to obtain an impregnated substrate, wherein the one or more extracted metals remain in the liquid phase from extraction to impregnation. Extraction is performed using a solution containing a solvent, at least one organic compound with coordination properties, and phosphoric acid.
2. The method as described in claim 1, characterized in that... The extraction solution and the impregnation solution share at least one common solvent.
3. The method as described in claim 1 or 2, characterized in that... The extraction and impregnation solutions are acidic media.
4. The method as described in claim 3, characterized in that... Extraction is performed using a solution containing an aqueous solvent and at least one organic compound with coordination and acidic properties.
5. The method as described in claim 1 or 2, characterized in that... The organic compound comprises one or more chemical functional groups selected from the group consisting of carboxylic acids, phosphonic acids, sulfonic acids, alcohols, thiols, thioethers, sulfones, sulfoxides, ethers, aldehydes, ketones, esters, amines, nitriles, imides, oximes, ureas, and amides, or a compound containing a furan ring or a sugar.
6. The method as described in claim 4, characterized in that... The organic compound is selected from at least one of the following compounds: formic acid, acetic acid, oxalic acid, malonic acid, glutaric acid, glycolic acid, lactic acid, malonic acid, citric acid, tartaric acid, pyruvic acid, γ-ketovalerate, succinic acid, acetoacetic acid, gluconic acid, ascorbic acid, phthalic acid, salicylic acid, maleic acid, malic acid, fumaric acid, acrylic acid, mercaptoacetic acid, 2-hydroxy-4-methylthiobutyric acid, glutamic acid, N-acetylglutamic acid, alanine, glycine, cysteine, histidine, aspartic acid, N-acetylaspartic acid, 4-aminobutyric acid, 1,2-cyclohexanediaminetetraacetic acid, ethylenediaminetetraacetic acid, hypozoxytriacetic acid, iminodiacetic acid, N-(2-hydroxyethyl)ethylenediamine-N,N',N' - Triacetic acid, diethylenetriaminepentaacetic acid, N-dihydroxyethylglycine, tris(hydroxymethyl)methylglycine, 1-hydroxyethide-1,1-diphosphonic acid, nitrotri(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), 4-sulfophthalic acid, 3-(N-morpholino)-2-hydroxy-1-propanesulfonic acid, 2-(4-pyridyl)ethanesulfonic acid, phenol-4-sulfonic acid, thiodiacetic acid, and diethanolic acid.
7. The method as described in claim 1, characterized in that... The organic compound is selected from at least one of the following compounds: dimethyl oxime, methyl acetoacetate, ethyl acetoacetate, ethyl lactate, methyl glycolate, ethyl glycolate, dimethyl malate, diethyl malate, dimethyl tartrate, diethyl tartrate, ethyl 3-hydroxybutyrate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, methyl 3-(methylthio)propionate, ethyl 3-(methylthio)propionate, ethylene glycol, diethylene glycol, triethylene glycol, and polyethylene glycol with a molecular weight of 200-1500 g / mol. Propylene glycol, glycerol, 2-butoxyethanol, 2-(2-butoxyethoxy)ethanol, 2-(2-methoxyethoxy)ethanol, triethylene glycol dimethyl ether, crown ether, acetophenone, 2,4-pentanedione, pentanone, glucose, fructose, sucrose, sorbitol, xylitol, mannitol, γ-valerolactone, propylene carbonate, octylamine, N,N-diethylformamide, N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, propionamide, 1-methyl-2-pyrrolidone, tetramethylurea, N,N'-dimethylurea, acetonitrile, lactamide, furfuryl alcohol, 2-furfural, 5-hydroxymethylfurfural, ethyl 3-hydroxybutyrate, 2-hydroxyethyl acrylate, 1-vinyl-2-pyrrolidone, N,N,N',N'-tetramethyltartrate, 3-hydroxypropionitrile, and N,N'-bis(2-hydroxyethyl)ethylenediamine.
8. The method as described in claim 4, characterized in that The concentration of one or more organic compounds in the extraction solution is limited such that, for each organic compound or for each of the one or more organic compounds, the molar ratio of the organic compound to the extracted one or more metals is 0.2-25.
9. The method as described in claim 4, characterized in that... The concentration of one or more organic compounds in the extraction solution is limited such that, for each organic compound or for each of the one or more organic compounds, the molar ratio of the organic compound to the extracted one or more metals is 0.4-1.
2.
10. The method as described in claim 1 or 2, characterized in that... Recycling includes at least one step of treating the source catalyst prior to extraction via a liquid route, selected from at least one of the following treatments: decoking, separation of contaminant / impurity type compounds, and mechanical grinding.
11. The method as described in claim 1 or 2, characterized in that... Recycling includes at least one step of treating a solution of one or more metals extracted prior to impregnation, selected from at least one of the following processes: concentration, dilution, or alteration of the composition of the solution by completely or partially adding or removing at least one compound.
12. The method as described in claim 1 or 2, characterized in that... The impregnation of the carrier begins with a solution of one or more extracted metals, with the addition of at least one of metals M1 and M2, optionally with the addition of phosphorus, and / or with the addition of one or more organic additives.
13. The method as described in claim 1 or 2, characterized in that... The method includes: - Sulfurized impregnated substrate.
14. The method as described in claim 1 or 2, characterized in that... After impregnating the carrier, at least a portion of the impregnation solution is used as a supplement to the extraction solution.
15. The method as described in claim 1 or 2, characterized in that... A solution of one or more metals is concentrated to remove at least a portion of the solvent and optionally at least a portion of the optional one or more organic compounds contained therein, and the solvent / one or more organic compounds thus removed are reused as a supplement to the extraction solution.
16. The method as described in claim 1 or 2, characterized in that... The method includes the following steps: - At least one step (a1, a2, a3) of treating the source catalyst, wherein step (a1) is regeneration, step (a2) is heat treatment under a gaseous stream containing hydrogen sulfide, and step (a3) is pre-grinding. - Extract one or more metals (b) from the source catalyst using an extraction solution to obtain a solution of the extracted one or more metals. - At least one optional step (c) to purify the solution of one or more metals extracted in step (b) to remove all or some of the possible impurities. -At least one optional step (d) of concentrating and extracting a solution of one or more metals. - At least one optional step (e) to adjust the composition of the solution of one or more metals extracted by step (b), (c), or (d). - An impregnating substrate is obtained by impregnating a carrier (f) via a liquid route with an impregnation solution obtained from a solution of the extracted one or more metals obtained in steps (b), (c), (d), or (e), wherein the impregnation solution is optionally supplemented with one or more metals, phosphorus, and one or more organic additives, wherein the extracted one or more metals are maintained in the liquid phase from extraction to impregnation. -Optional vulcanization (g) of the impregnated carrier obtained in step (f).
17. The method as described in claim 1 or 2, characterized in that... The source catalyst is a pre-regenerated or restored spent catalyst.
18. The method as described in claim 1 or 2, characterized in that... The support on which the impregnation is performed by an impregnation solution produced from a solution of one or more extracted metals is a depleted metal catalyst of the type of spent catalyst that is pre-impregnated or post-impregnated with the impregnation solution or optionally regenerated / restored.
Citation Information
Patent Citations
Process for recovering group vi-b metals from spent catalysts
EP2064358A1
CATALYST BASED ON IMIDAZOLIDINONES, IMIDAZOLIDINEDIONES, PYRIMIDINONES AND / OR PYRIMIDINETRIONES AND ITS USE IN A HYDROCRACKING AND / OR HYDROTREATMENT PROCESS
FR3083131A1
Method for recovering molybdenum and method for preparing catalyst
US20070167321A1
Method for hydrotreating a diesel fuel in reactors in parallel with hydrogen recycling
WO2015078675A1
Process for recovering group vi-b metals from spent catalysts
CN101517104A