Isolation film, method for manufacturing the same, and secondary battery and electric device including the same
By coating the separator with pressure-sensitive adhesive and organic particles, the misalignment problem between the electrode and the separator during the transfer process is solved, achieving efficient bonding and stability of the battery cell, improving the dynamics and safety performance of the battery cell, and simplifying the production process.
Patent Information
- Application Number
- CN202180096158.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2041-12-30
AI Technical Summary
In the manufacturing process of electrochemical device cells, the electrodes and separators are prone to misalignment during transfer, resulting in poor adhesion, which affects the dynamic performance and safety performance of the cell. Furthermore, the softening point of existing adhesive coatings is too low, which makes the interlayer adhesion of the separator unfavorable for high-speed composite.
The pressure-sensitive separator is coated with 40-90wt% of primary organic particles and 10-20wt% of pressure-sensitive adhesive polymer and plasticizer to ensure that it does not stick under low pressure, effectively bonds the electrode sheets under high pressure, avoids misalignment, and achieves tight bonding at room temperature.
It improves the structural stability and dynamic performance of battery cells, simplifies the production process, saves space and time, reduces energy consumption, increases production capacity, and at the same time ensures the safety performance and shaping effect of battery cells.
Smart Images

Figure HPA0000345676290000011 
Figure HPA0000345676290000012 
Figure HPA0000345676290000013
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a separator membrane, a method for preparing the same, and a secondary battery and an electrical device comprising the separator membrane. Background Technology
[0002] During the manufacturing process of electrochemical device cells, misalignment inevitably occurs between the electrodes and the separator during transfer. This can range from minor issues like electrodes coming into contact and rendering the cell unusable, to more serious problems like wrinkling of the electrodes after full charging, severely impacting kinetic performance and reducing cell safety. Therefore, an adhesive coating is currently applied to the separator, and in the first bonding process between the electrodes and separator, pre-pressing is typically performed under appropriate pressure to ensure a certain level of adhesion between the electrodes and separator before proceeding to the next process. However, due to production efficiency requirements, the pressure and duration at this stage are often insufficient to achieve adequate adhesion between the electrodes and separator.
[0003] To address the aforementioned issues, when using adhesive materials with very low DSC melting points for the adhesive coating on the separator, the following challenges need to be considered: The separator is a soft material. To facilitate the efficient use and transportation of electrochemical devices, the separator is typically carried on a cylindrical roll, which is wound into a roll under a certain force. At this time, the separator layers are in close contact with each other and there is a certain pressure. If the DSC melting point on the separator is too low, it often leads to the separator layers sticking together, which is not conducive to the high-speed bonding of the subsequent electrode and the separator. Summary of the Invention
[0004] This application was made in view of the aforementioned problems, and its object is to provide a pressure-sensitive separator and a method for preparing the same, as well as a secondary battery comprising the pressure-sensitive separator. Furthermore, this application also aims to provide an electrical device comprising the secondary battery.
[0005] To achieve the above objectives, a first aspect of this application provides a pressure-sensitive separator, which may include: a porous separator substrate and a pressure-sensitive coating applied to at least one surface of the separator substrate, comprising 40-90 wt% of first organic particles and 10-20 wt% of a pressure-sensitive adhesive polymer, and optionally 0-50 wt% of second organic particles; wherein the pressure-sensitive adhesive polymer may include an adhesive polymer and a plasticizer. This separator exhibits excellent pressure-sensitive properties, with an adhesion strength below 0.23 N / m under ≤1 MPa pressure, particularly below 0.1 N / m, thus preventing layer-to-layer adhesion during winding and storage. Under ≥2 MPa pressure, it can achieve significant adhesion to the electrode sheet. Therefore, when using this separator to prepare battery cells, the electrode sheet and separator can be tightly bonded under appropriate pressure at room temperature.
[0006] In some embodiments, the mass ratio of the adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer can be (4-19):1, or optionally (4-11):1. When the relative content of the plasticizer in the pressure-sensitive adhesive polymer is within the above range, it ensures that the electrode and the separator achieve a large adhesion force under certain pressure, without causing an increase in the resistance of the separator or a decrease in the cycle performance of the secondary battery.
[0007] In some embodiments, the pressure-sensitive adhesive polymer may have a core-shell structure, wherein both the core and the shell of the core-shell structure may include the adhesive polymer and a plasticizer. In the core structure, the mass ratio of the adhesive polymer to the plasticizer may be (2-5):1, optionally (3-4):1, and in the shell structure, the mass ratio may be (6-10):1, optionally (7-9):1. Since both the core and shell of the core-shell structure are primarily composed of the adhesive polymer and the plasticizer, the pressure-sensitive performance of the pressure-sensitive adhesive polymer can be further improved, thereby further enhancing the kinetic performance of the separator.
[0008] In some embodiments, a portion of the plasticizer is grafted onto the binder polymer. Optionally, at least 5 wt% of the plasticizer is grafted onto the binder polymer. When a portion of the plasticizer is grafted onto the binder polymer, it can prevent the plasticizer from migrating excessively into the electrolyte during cycling, thus preventing the consumption of various functional additives in the electrolyte, increasing the separator resistance, and affecting the cell's dynamic performance.
[0009] In some embodiments, the average particle size of the pressure-sensitive adhesive polymer can be 0.5-3.0 μm, optionally 0.8-2.0 μm. A pressure-sensitive adhesive polymer with a suitable particle size facilitates its uniform distribution on the first organic particles or both the first and second organic particles, contributing to the adhesion of its core and shell to the electrode under certain pressure, and effectively improving the resistance of the separator.
[0010] In some embodiments, the DSC melting point of the pressure-sensitive adhesive polymer can be -50℃ to 100℃, or optionally -45℃ to 60℃. When the DSC melting point of the pressure-sensitive adhesive polymer is within the above range, it can ensure the bonding strength at room temperature and avoid excessive bonding strength at 1MPa, which would cause the separator to roll up and stick. At the same time, it avoids insufficient bonding strength at 2MPa at room temperature, which would result in weak adhesion between the separator and the electrode, and would be detrimental to cell shaping.
[0011] In some embodiments, the adhesive polymer may comprise a copolymer formed by copolymerization of a mixture of reactive monomers comprising at least one of a first monomer, at least one of a second monomer, at least one of a third monomer, and at least one of a reactive dispersant:
[0012] The first monomer: its melting point is generally above 80℃, and may include acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, hydroxymethylacrylamide, acrylamide, styrene, and acrylonitrile;
[0013] The second monomer: its melting point generally does not exceed 80℃, and may include C4-C22 alkyl acrylates, isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate (isooctyl acrylate), cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylurea methacrylate, dicyclopentene ethoxylate methacrylate, tetrahydrofuran methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, ethylurea methacrylate, propylene methacrylate, dicyclopentene ethoxylate methacrylate, tetrahydrofuran methacrylate, and trifluoroethyl methacrylate.
[0014] The third monomer is a crosslinking monomer containing at least one of hydroxyl, amino, or double bond, and may include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, γ-methacryloyloxypropyltrimethoxysilane, N-hydroxymethylacrylamide, N-butoxymethyl (meth)acrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, epoxy resins with an epoxy value of 0.35-0.50, and divinylbenzene;
[0015] Reactive dispersants may include polyvinyl alcohol, polyacryl alcohol, ethylene glycol, polyethylene glycol, and polyvinyl alcohol. Optionally, these reactive dispersants have a degree of alcoholysis ≥85% and an average degree of polymerization of 400-2000; preferably, a degree of alcoholysis ≥88% and an average degree of polymerization of 500-1600.
[0016] When the adhesive polymer comprises a copolymer formed by copolymerization of a mixture of reactive monomers including at least one of the first monomers, at least one of the second monomers, at least one of the third monomers and at least one of the reactive dispersants, it can ensure that the adhesive polymer has suitable swelling and adhesion, ensure that the pressure-sensitive adhesive polymer has suitable swelling, pressure sensitivity and adhesion properties, and at the same time has a suitable elastic modulus, ensuring the shaping effect, dynamic performance and safety performance of the battery cell.
[0017] In some embodiments, the plasticizer may be selected from one or more of the following: glycerol C4-C10 alkyl diether or monoether, glycerol C4-C10 carboxylic acid monoester or diester, propylene glycol C4-C10 alkyl monoether, and glycerol.
[0018] In some embodiments, the average thickness of the pressure-sensitive coating may be 2-20 μm, and optionally 2-15 μm.
[0019] In some embodiments, the average particle size of the first organic particles can be 5-30 μm, optionally 5-20 μm. This results in a larger average particle size for the first organic particles, which on the one hand increases the effective contact area between the electrode and the separator, thereby significantly improving their adhesion; on the other hand, it prevents these organic particles from penetrating into the pores formed in the separator substrate. Furthermore, the larger particle size and relatively larger voids also solve the problem of poor air permeability of the separator and reduce the possibility of small particles clogging the separator pores, thus avoiding the risk of increased internal resistance. In addition, because the first organic particles have a larger average particle size, they possess a certain compressibility, effectively providing stress relief space at the corners of the battery cell when present there.
[0020] In some embodiments, the DSC melting point of the first organic particles can be -50℃ to 200℃, or optionally -40℃ to 160℃. When the DSC melting point of the first organic particles is within this range, it can withstand electrolyte swelling. On the one hand, it will not consume excessive electrolyte, and residual monomers are less likely to be soaked out by the electrolyte and block the separator, thus affecting the dynamic performance of the battery cell. On the other hand, it will not cause a significant decrease in the adhesion between the separator and the electrode, and the electrode is less likely to be damaged by the first organic particles, leading to a decrease in safety performance.
[0021] In some embodiments, the weight-average molecular weight of the first organic particle may be 300 × 10⁻⁶. 3 g / mol - 800 × 10 3 g / mol, can be selected as 400×10 3 g / mol - 650 × 10 3 g / mol. The weight-average molecular weight of the first organic particles is within the above range, which ensures that the first organic particles have suitable swelling and suitable adhesion to the electrode. In some embodiments, the first organic particles may be one or more polymers containing one or more groups selected from the following: halogen, phenyl, epoxy, cyano, ester, and amide.
[0022] In some embodiments, the first organic particle may be a homopolymer or copolymer of fluorinated alkenyl monomer units, a homopolymer or copolymer of olefinic monomer units, a homopolymer or copolymer of unsaturated nitrile monomer units, a homopolymer or copolymer of epoxide monomer units, a dimer, homopolymer or copolymer of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers.
[0023] In some embodiments, the fluorinated alkenyl monomer unit may be selected from one or more of difluoroethylene, vinylidene fluoride, trifluoroethylene, trifluorochloroethylene, tetrafluoroethylene, hexafluoropropylene, or derivatives thereof.
[0024] In some embodiments, the olefin-based monomer unit may be selected from one or more of ethylene, propylene, butadiene, isoprene, styrene, or derivatives thereof.
[0025] In some embodiments, the unsaturated nitrile monomer unit may be selected from one or more of acrylonitrile, methacrylonitrile, or their derivatives.
[0026] In some embodiments, the alkyl oxide monomer unit may be selected from one or more of ethylene oxide, propylene oxide, or their derivatives.
[0027] In some embodiments, the monosaccharide monomer unit may be selected from glucose or a derivative thereof.
[0028] In some embodiments, the first organic particle may be selected from at least one of the following: perfluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose.
[0029] In some embodiments, the first organic particle may be selected from at least one of the following: polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, perfluorinated polyvinyl chloride, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.
[0030] When the first organic particle is selected from the above-mentioned substances, it exhibits suitable swelling and appropriate adhesion to the electrode. This enables appropriate bonding force with the pressure-sensitive binder polymer, while ensuring uniform dispersion of the pressure-sensitive binder polymer on it, thus guaranteeing adhesion and kinetic properties.
[0031] In some embodiments, the mass ratio of the first organic particles to the second organic particles can be (1-4):1, or optionally (1.5-2.5):1. When the mass ratio of the first organic particles to the second organic particles is within the above range, the wettability and distribution uniformity of the electrolyte can be effectively improved, further enhancing the high-temperature storage performance of the battery. The first organic particles have a relatively large average particle size and are typically designed as secondary particles, while the second organic particles have a relatively small average particle size and are typically designed as primary particles. The combined action of the first and second organic particles enhances the adhesion between the separator and the electrode plates while effectively ensuring that the separator has a moderately non-uniform pore structure.
[0032] In some embodiments, the average particle size of the second organic particles may be 0.5-10 μm, and optionally 2-8 μm.
[0033] In some embodiments, the DSC melting point of the second organic particles can be -30 to 100°C, or optionally -30 to 70°C. When the DSC melting point of the second organic particles is within this range, it can withstand electrolyte swelling. On the one hand, it will not consume excessive electrolyte, and residual monomers are less likely to be soaked out by the electrolyte and block the separator, thus affecting the dynamic performance of the battery cell. On the other hand, it will not cause a significant decrease in the adhesion between the separator and the electrode, and the electrode is less likely to be damaged by the second organic particles, leading to a decrease in safety performance.
[0034] In some embodiments, the weight-average molecular weight of the second organic particle may be 10 × 10⁻⁶. 3 g / mol-100×10 3 g / mol, which can be selected as 20×10 3 g / mol - 80 × 10 3 g / mol. The weight-average molecular weight of the second organic particles is within the above range, which ensures that the second organic particles have suitable swelling and suitable adhesion to the electrode.
[0035] In some embodiments, the second organic particle is a polymer comprising one or more groups selected from the following: phenyl, epoxy, cyano, ester, hydroxy, carboxyl, sulfonyl ester, and pyrrolidone.
[0036] In some embodiments, the second organic particle may be selected from at least one of the following: homopolymers or copolymers of acrylate monomer units, homopolymers or copolymers of acrylic monomer units, homopolymers or copolymers of unsaturated nitrile monomer units, homopolymers or copolymers of olefin monomer units, homopolymers or copolymers of styrene monomer units, homopolymers or copolymers of epoxy monomer units, polyurethane compounds, rubber compounds, dimers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers.
[0037] In some embodiments, the acrylate monomer unit may be selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, methyl methacrylate, butyl methacrylate, isooctyl methacrylate, or derivatives thereof.
[0038] In some embodiments, the acrylic monomer unit may be selected from one or more of acrylic acid, methacrylic acid, or derivatives thereof.
[0039] In some embodiments, the unsaturated nitrile monomer unit may be selected from one or more of acrylonitrile, methacrylonitrile, or their derivatives.
[0040] In some embodiments, the olefinic monomer unit may be selected from one or more of ethylene, vinyl acetate, butadiene, or derivatives thereof.
[0041] In some embodiments, the styrene monomer unit may be selected from one or more of styrene, methylstyrene, or their derivatives.
[0042] In some embodiments, the epoxy monomer unit may be selected from one or more of ethylene oxide, propylene oxide, or their derivatives.
[0043] In some embodiments, the monosaccharide monomer unit may be selected from glucose or a derivative thereof.
[0044] In some embodiments, the second organic particle is selected from at least one of the following: polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer, styrene-butyl acrylate-isooctyl acrylate copolymer, and polyimide.
[0045] When the second organic particle is selected from the above-mentioned substances, it exhibits suitable swelling and appropriate adhesion to the electrode. This allows for suitable bonding with the pressure-sensitive binder polymer, while simultaneously ensuring uniform dispersion of the pressure-sensitive binder polymer on it, thus guaranteeing both adhesion and kinetic properties.
[0046] In some embodiments, the porosity of the separator substrate can be 10-95%, the pore size can be 20-60 nm, and the thickness can be 3-12 μm, optionally 5-9 μm. When the porosity of the separator substrate is within the above range, a balance between the kinetics and safety performance of the secondary battery can be achieved; when the thickness of the separator substrate is within the above range, a balance between the energy density and safety performance of the secondary battery can be achieved.
[0047] In some embodiments, the separator substrate comprises a membrane or nonwoven fabric selected from one or more of the following: polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymer, polyphenylene sulfide, and polyvinyl naphthalene.
[0048] The second aspect of this application provides a method for preparing the separator membrane of the first aspect of this application, which includes the following steps:
[0049] S1) The first organic particles and dispersant are added to the solvent to form a first polymer solution;
[0050] S2) Add the pressure-sensitive adhesive polymer to the first polymer solution obtained in step S1) and mix to form a second polymer solution;
[0051] S3) Optionally, the second organic particles are added to the second polymer solution obtained in step S2), and mixed to form a third polymer solution; and
[0052] S4) The second polymer solution obtained in step S2) or the third polymer solution obtained in step S3) is coated onto at least one surface of the porous separator substrate, and the separator is obtained after drying.
[0053] The isolation membrane includes a pressure-sensitive coating formed on at least one surface of the isolation membrane substrate, comprising 40-90 wt% of first organic particles and 10-20 wt% of a pressure-sensitive adhesive polymer, and optionally 0-50 wt% of second organic particles; wherein the pressure-sensitive adhesive polymer comprises an adhesive polymer and a plasticizer.
[0054] A third aspect of this application provides a secondary battery comprising a positive electrode, a negative electrode, a separator spaced between the positive electrode and the negative electrode, and an electrolyte, wherein the separator is the separator provided in the first aspect of this application or a separator prepared by the method provided in the second aspect of this application.
[0055] A fourth aspect of this application provides an electrical device comprising a secondary battery selected from the third aspect of this application.
[0056] Beneficial effects
[0057] The pressure-sensitive separator provided in this application comprises a porous separator substrate and a pressure-sensitive coating applied to at least one surface of the separator substrate. The coating comprises 40-90 wt% of first organic particles and 10-20 wt% of pressure-sensitive adhesive polymer, and optionally 0-50 wt% of second organic particles. The pressure-sensitive adhesive polymer may include an adhesive polymer and a plasticizer, enabling the separator to have good ion conduction and adhesion properties at room temperature. Its resistance at room temperature is below 1.32 Ω, especially below 1.1 Ω, and it does not adhere under pressure ≤1 MPa, but can adhere significantly to the electrode under pressure ≥2 MPa. Therefore, on the one hand, the electrodes and separators of electrochemical devices can be tightly bonded at room temperature, preventing misalignment during production and transfer, thus ensuring the structural stability of the electrochemical device. This also guarantees the cell's group margin and casing quality, improving cell shaping performance, safety performance, and kinetic performance. Furthermore, it eliminates the need for a tunnel furnace and a second composite process in traditional cell manufacturing, saving production space and time, reducing energy consumption, and increasing production capacity. On the other hand, the separator provided by this invention does not stick together during winding and storage, facilitating its use in subsequent cell manufacturing. Attached Figure Description
[0058] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0059] Figure 1 This is a schematic diagram of a secondary battery provided in an embodiment of this application.
[0060] Figure 2 This is a schematic diagram of a battery module provided in an embodiment of this application.
[0061] Figure 3 This is a schematic diagram of a battery pack provided in an embodiment of this application.
[0062] Figure 4 yes Figure 3 The exploded diagram.
[0063] Figure 5 This is a schematic diagram of an electrical device provided in an embodiment of this application.
[0064] Figure 6 A photograph of the morphology of the pressure-sensitive coating of the isolation membrane prepared in Example 13 of this application is shown.
[0065] The reference numerals in the attached figures are explained as follows:
[0066] 1. Battery pack;
[0067] 2. Upper box;
[0068] 3. Lower box;
[0069] 4. Battery module;
[0070] 5. Secondary battery. Detailed Implementation
[0071] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the separator, its preparation method, secondary battery, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0072] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0073] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0074] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0075] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0076] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0077] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0078] In the description of this article, it should be noted that, unless otherwise stated, "above" and "below" include the number itself, and "several" in "one or several" means two or more.
[0079] Rechargeable batteries
[0080] Rechargeable batteries have become a preferred power source for electrical devices due to their advantages such as high energy density, portability, lack of memory effect, and environmental friendliness. The separator in a rechargeable battery is a crucial component for ensuring battery safety. However, during the manufacturing process of electrochemical cells, misalignment between the electrodes and the separator is inevitable. This can range from minor issues like electrodes coming into contact and rendering the cell unusable, to more serious issues like the electrodes wrinkling after a full charge, severely impacting kinetic performance and reducing cell safety. Therefore, currently, an adhesive coating is applied to the separator, and in the first bonding process between the electrode and the separator of the electrochemical device, pre-pressing is usually performed under appropriate pressure to ensure a certain degree of adhesion between the electrode and the separator before entering the next process. However, due to production efficiency requirements and considering that high pressure can degrade the structure of the main material, the pressure and time at this stage are insufficient to achieve a proper bonding effect between the electrode and the separator. Furthermore, to ensure cell mass margin and casing quality, the electrode and separator of the electrochemical device often need to be baked in a tunnel oven at 80-100℃ for ≥700s before applying pressure to ensure a tight bond between the electrode and the separator. This process requires a large amount of production space and time, making it difficult to increase production capacity. On the other hand, in order to solve the above problems, the adhesive coating on the separator uses an adhesive material with a very low softening point. The following challenges need to be considered: The separator is a soft material. In order to facilitate the high-efficiency use and transportation of electrochemical devices, the separator is usually carried by a cylindrical roll. Under a certain force, the separator is wound into a roll. At this time, the separator layers are in close contact with each other and there is a certain pressure. If the softening point of the adhesive material on the separator is too low, it will often cause the separator layers to stick together, which is not conducive to the high-speed composite of the electrode and the separator.
[0081] This application provides a secondary battery with good safety and kinetic performance.
[0082] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.
[0083] [Positive electrode plate]
[0084] The positive electrode includes a positive current collector and a positive electrode film disposed on at least one surface of the positive current collector and comprising a positive active material. As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0085] The positive current collector can be made of a material with good conductivity and mechanical strength. In some embodiments, the positive current collector can be aluminum foil.
[0086] This application does not impose specific restrictions on the type of positive electrode active material. Materials known in the art that can be used as positive electrodes for secondary batteries can be used, and those skilled in the art can select them according to actual needs.
[0087] In some embodiments, the secondary battery provided by the present invention can be a lithium-ion secondary battery. The positive electrode active material may comprise positive electrode active materials known in the art for use in batteries. For example, the positive electrode active material may comprise at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.15 Al 0.05 At least one of O2 and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0088] In some embodiments, the positive electrode membrane may optionally include an adhesive. There is no specific limitation on the type of adhesive, and those skilled in the art can select one according to actual needs. As an example, the adhesive used for the positive electrode membrane may include one or more of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).
[0089] In some embodiments, the positive electrode membrane may optionally include a conductive agent. There is no specific limitation on the type of conductive agent, and those skilled in the art can select it according to actual needs. As an example, the conductive agent used for the positive electrode membrane may include one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0090] In some embodiments, the step of preparing a positive electrode sheet using a positive active material may include: dispersing the positive active material, a binder, and an optional conductive agent in a solvent, which may be N-methylpyrrolidone, and stirring evenly under the action of a vacuum stirrer to obtain a positive slurry; uniformly coating the positive slurry onto a positive current collector aluminum foil, drying it at room temperature, transferring it to an oven for drying, and then cold pressing and slitting to obtain a positive electrode sheet.
[0091] [Negative electrode plate]
[0092] The negative electrode includes a negative current collector and a negative electrode film disposed on at least one surface of the negative current collector. As an example, the negative current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative current collector.
[0093] The negative electrode current collector can be made of a material with good conductivity and mechanical strength, serving both as a conductor and a current collector. In some embodiments, the negative electrode current collector can be made of copper foil.
[0094] The negative electrode film includes a negative electrode active material. The steps for preparing a negative electrode sheet using the negative electrode active material may include: dispersing the negative electrode active material, binder, and optional thickener and conductive agent in a solvent, which may be deionized water, to form a uniform negative electrode slurry; coating the negative electrode slurry onto a negative electrode current collector, and obtaining the negative electrode sheet after processes such as drying and cold pressing.
[0095] In some embodiments, this application does not specifically limit the type of negative electrode active material, and the negative electrode sheet may optionally include negative electrode active materials that can be used as negative electrodes in secondary batteries. The negative electrode active material may be one or more of graphite materials (such as artificial graphite and natural graphite), mesophase microcarbon spheres (MCMB), hard carbon, soft carbon, silicon-based materials, and tin-based materials.
[0096] In some embodiments, the adhesive may be selected from one or more of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0097] In some embodiments, the thickener may be sodium carboxymethyl cellulose (CMC-Na).
[0098] In some embodiments, the conductive agent used for the negative electrode sheet may be selected from one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0099] [Electrolytes]
[0100] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0101] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0102] In some embodiments, the electrolyte salt may be selected from one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalate borate), LiBOB (lithium dioxalate borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorodioxalate phosphate), and LiTFOP (lithium tetrafluorooxalate phosphate).
[0103] In some embodiments, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0104] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, additives that improve battery low-temperature performance, etc.
[0105] [Isolation membrane]
[0106] Secondary batteries using electrolytes, as well as some secondary batteries using semi-solid electrolytes, also include a separator. The separator is placed between the positive and negative electrodes to provide isolation.
[0107] In the secondary battery provided in this application, the separator can be a pressure-sensitive separator provided in this application. This separator has good ion conduction and adhesion properties under room temperature conditions. Its resistance under room temperature conditions is below 1.32Ω, especially below 1.1Ω; its adhesion force under ≤1MPa is below 0.23N / m, especially below 0.1N / m; and its adhesion force to the electrode under ≥2MPa is above 0.34N / m, especially above 0.50N / m, and even more especially above 0.60N / m. The separator and its preparation method will be described in detail below.
[0108] Separating membrane
[0109] The isolation membrane provided in this application may include: a porous isolation membrane substrate and a pressure-sensitive coating applied to at least one surface of the isolation membrane substrate, comprising 40-90 wt% of first organic particles and 10-20 wt% of a pressure-sensitive adhesive polymer, and optionally 0-50 wt% of second organic particles; wherein the pressure-sensitive adhesive polymer may include an adhesive polymer and a plasticizer.
[0110] Through extensive research, the inventors have observed that when a pressure-sensitive coating comprising 40-90 wt% first organic particles, 10-20 wt% pressure-sensitive adhesive polymer, and optionally 0-50 wt% second organic particles is coated onto at least one surface of a porous separator substrate to prepare the separator, a pressure-sensitive separator exhibiting good ion-conducting ability and adhesive properties at room temperature can be obtained. The pressure-sensitive adhesive polymer may include an adhesive polymer and a plasticizer; their combined action gives the pressure-sensitive adhesive polymer excellent pressure-sensitive properties, further enhancing the pressure-sensitive properties of the separator, resulting in an adhesive force below 0.23 N / m under ≤1 MPa, particularly below 0.1 N / m. Therefore, it can prevent the separator from being blocked. The separator film achieves layer-to-layer adhesion during winding and storage, and enables it to bond significantly with the electrode under pressure ≥2MPa. Therefore, when using this separator film to manufacture battery cells, the electrode and separator film can be tightly bonded under normal temperature and appropriate pressure. This avoids misalignment between the electrode and separator film, which could lead to battery cell scrap, affect battery cell performance, and create safety risks. Furthermore, it eliminates the need for tunnel furnaces and second composite processes in traditional battery cell manufacturing, thereby saving production space and time, reducing energy consumption, and significantly increasing battery cell production capacity. It also improves the shaping performance, safety performance, and kinetic performance of the battery cell, thereby enhancing the safety and kinetic performance of the secondary battery containing the battery cell and the electrical device containing the secondary battery.
[0111] In some embodiments, the mass ratio of the adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer may be (4-19):1, or optionally (4-11):1. When the relative content of the plasticizer in the pressure-sensitive adhesive polymer is within the above range, it ensures a strong adhesion between the electrode and the separator without increasing the resistance of the separator or reducing the cycle performance of the secondary battery.
[0112] The plasticizer content can be determined using a Shimadzu STA449F3 thermogravimetric analyzer. As a specific example, the test method is as follows: Take approximately 10 mg of pressure-sensitive adhesive polymer solid, record the initial mass as M0, heat to 200℃, record the mass as M1, the plasticizer content is M1-M0, and the adhesive polymer content is M0-(M1-M0). Test conditions are set as follows: temperature range -100-400℃, nitrogen atmosphere, 10℃ / min.
[0113] In some embodiments, the pressure-sensitive adhesive polymer may have a core-shell structure, in which both the core and shell may contain an adhesive polymer and a plasticizer. The mass ratio of the adhesive polymer to the plasticizer in the core structure may be (2-5):1, optionally (3-4):1, and the mass ratio in the shell structure may be (6-10):1, optionally (7-9):1. The core and shell of the core-shell structure are both composed of an adhesive polymer and a plasticizer, which can further improve the pressure-sensitive performance of the pressure-sensitive adhesive polymer, thereby further enhancing the kinetic performance of the separator. On the other hand, the inclusion of a plasticizer in the pressure-sensitive adhesive polymer allows for rapid migration between the adhesive polymer and the main material of the separator under certain pressure (e.g., 1-2 MPa), plasticizing the adhesive polymer, causing its molecular chains to extend, and enabling intermolecular hydrogen bonding with adhesives such as SBR in the negative electrode, thickeners such as CMC, and adhesives such as PVDF in the positive electrode, thus improving interfacial wetting and enhancing the bonding effect between the two interfaces. Under pressure of ≥2MPa, the core structure is crushed, and the plasticizer in the core is released, which can further enhance the above effects.
[0114] In some embodiments, a portion of the plasticizer is grafted onto the adhesive polymer. Optionally, at least 5 wt% of the plasticizer is grafted onto the adhesive polymer, based on its weight. When a portion of the plasticizer is grafted onto the adhesive polymer, it prevents the plasticizer from migrating excessively into the electrolyte during cycling, consuming various functional additives in the electrolyte, increasing the separator resistance, and affecting the cell's dynamic performance. When at least 5 wt% of the plasticizer is grafted onto the adhesive polymer backbone, the separator and electrode can form a "broken-and-connected" relationship, thereby improving the durability of room-temperature adhesion, reducing rebound, and further ensuring that no excessive plasticizer migrates into the electrolyte during cycling, affecting cell performance. The grafting rate can be detected by infrared testing, specifically by obtaining the Fourier transform infrared spectra of the adhesive polymer, plasticizer, and pressure-sensitive adhesive polymer, with the Fourier transform infrared spectra obtained at 1500-1700 cm⁻¹ for the pressure-sensitive adhesive polymer. -1 A peak appears at the position that is distinct from the adhesive polymer and the individual plasticizer. This peak represents the grafted plasticizer, and the area under the peak represents the amount of grafted plasticizer. The grafting rate of the plasticizer can be calculated from this.
[0115] In some embodiments, the average particle size of the pressure-sensitive adhesive polymer may be 0.5-3.0 μm, optionally 0.8-2.0 μm. A pressure-sensitive adhesive polymer with a suitable average particle size facilitates its uniform distribution on the first or second organic particles, contributing to the adhesion of its core and shell to the electrode under certain pressure, and effectively improving the resistance of the separator.
[0116] The average particle size of pressure-sensitive adhesive polymers can be determined using a laser particle size analyzer (such as Malvern Master Size 3000) in accordance with standard GB / T 19077.1-2016.
[0117] In some embodiments, the DSC melting point of the pressure-sensitive adhesive polymer can be -50℃ to 100℃, and can be selected as -45℃ to 60℃. When the DSC melting point of the pressure-sensitive adhesive polymer is within the above range, it can ensure the bonding strength at room temperature and avoid excessive bonding strength at 1MPa, which would cause the separator to roll up and stick. At the same time, it avoids the bonding strength at 2MPa at room temperature being too small, which would cause the separator to stick weakly and be detrimental to cell shaping.
[0118] In some embodiments, the adhesive polymer comprises a copolymer formed by copolymerization of a mixture of reactive monomers comprising at least one of a first monomer, at least one of a second monomer, at least one of a third monomer, and at least one of a reactive dispersant:
[0119] The first monomer: its melting point is generally above 80℃, and may include acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, hydroxymethylacrylamide, acrylamide, styrene, and acrylonitrile;
[0120] The second monomer: its melting point generally does not exceed 80℃, and may include C4-C22 alkyl acrylates, isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate (isooctyl acrylate), cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylurea methacrylate, dicyclopentene ethoxylate methacrylate, tetrahydrofuran methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, ethylurea methacrylate, propylene methacrylate, dicyclopentene ethoxylate methacrylate, tetrahydrofuran methacrylate, and trifluoroethyl methacrylate.
[0121] The third monomer is a crosslinking monomer containing at least one of hydroxyl, amino, or double bond, and may include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, γ-methacryloyloxypropyltrimethoxysilane, N-hydroxymethylacrylamide, N-butoxymethyl (meth)acrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, epoxy resins with an epoxy value of 0.35-0.50, and divinylbenzene;
[0122] Reactive dispersants: These dispersants, during the synthesis of pressure-sensitive adhesive polymers, act as both copolymerizers and dispersants with the aforementioned first, second, and third monomers. They may include polyvinyl alcohol, polyacryl alcohol, ethylene glycol, polyethylene glycol, and polyvinyl alcohol. Optionally, these reactive dispersants have a degree of alcoholysis ≥85% and an average degree of polymerization of 400-2000; preferably, a degree of alcoholysis ≥88% and an average degree of polymerization of 500-1600.
[0123] When the adhesive polymer comprises a copolymer formed by copolymerization of a mixture of reactive monomers including at least one of the first monomers, at least one of the second monomers, at least one of the third monomers and at least one of the reactive dispersants, it can ensure that the adhesive polymer has suitable swelling and adhesion, ensure that the pressure-sensitive adhesive polymer has suitable swelling, pressure sensitivity and adhesion properties, and at the same time has a suitable elastic modulus, ensuring the shaping effect, dynamic performance and safety performance of the battery cell.
[0124] In some embodiments, the plasticizer may be selected from one or more of the following: glycerol C4-C10 alkyl diether or monoether, glycerol C4-C10 carboxylic acid monoester or diester, propylene glycol C4-C10 alkyl monoether, and glycerol.
[0125] In some embodiments, the pressure-sensitive adhesive polymer can be synthesized according to the following synthesis method, including the following steps:
[0126] The first step involves adding 0.1-1% by mass (relative to the total weight of the mixture of reactive monomers (including the first monomer, second monomer, third monomer, and reactive dispersant), auxiliaries (including emulsifiers, stabilizers, and aqueous initiators), and plasticizers added during the synthesis of pressure-sensitive adhesive polymers) and 2-3% by mass of an oligomer (e.g., octadecyl methacrylate) with a number average molecular weight ≤1000 and a melting point of 0-30°C. The homogenizer speed is controlled at 8000-12000 r / min, such as 10000 r / min, for dispersion. The dispersion time can be 20-60 min, such as 50 min, and the dispersion reaction temperature is 20-40°C, such as 25°C, to a solvent (e.g., deionized water) to obtain the first mixture.
[0127] The second step involves adding 1-4% by mass of a stabilizer to the first mixture, such as at least one of the following: polyethylene oxide, allyl polyether sulfate, methylene succinic acid (itaconic acid), styrene sulfonic acid, sodium vinyl sulfonate, or sodium nanocellulose; the homogenizer speed is controlled at 6000-8000 r / min, for example, 6500 r / min, for 20-60 min, for example, 30 min, and the mixing reaction temperature is 20-60℃, for example, 45℃, to obtain the second mixture.
[0128] The third step involves adding 0.05-0.5% by mass of an aqueous initiator to the second mixture, such as at least one selected from the following: sodium bicarbonate, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, tert-butyl peroxide, tert-butyl valerate peroxide, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl percarbonate, dicyclohexyl percarbonate, potassium persulfate, sodium persulfate, ammonium persulfate, azobisisobutyronitrile, and azobisisoheptanenitrile. The homogenizer speed is controlled at 8000-12000 r / min, for example, 8000 r / min for mixing, for 20-60 min, such as 30 min. The reaction temperature is 60-80℃, such as 72℃, to obtain the third mixture.
[0129] The fourth step involves gradually and uniformly adding (controlling the addition to be completed within 60 minutes) 35%-45% mass fraction of the reaction monomer mixture to the third mixture at a homogenizer speed of 100-1000 r / min, such as 400 r / min, for a reaction time of 80-100 minutes, such as 80 minutes, to obtain the fourth mixture.
[0130] The fifth step involves continuing the reaction of the fourth mixture at a reaction temperature of 80-90℃ (e.g., 84℃) and a homogenizer speed of 12000-18000 r / min (e.g., 15000 r / min) for 120-240 min (e.g., 180 min) to obtain the fifth mixture.
[0131] Step 6: Add 10-20% by mass of plasticizer, such as glycerin, to the fifth mixture. Control the reaction temperature at 80-90℃, such as 84℃; control the homogenizer speed at 12000-18000 r / min, such as 15000 r / min; and control the reaction time at 120-240 min, such as 180 min, to obtain the sixth mixture.
[0132] Step 7: Add 0.05-0.5% by mass of an aqueous initiator, such as ammonium persulfate-sodium bicarbonate, to the mixture from step 6. Control the homogenizer speed to 8000-12000 r / min, e.g., 8000 r / min, for 20-60 minutes, e.g., 30 minutes. Maintain the reaction temperature at 60-80℃, e.g., 72℃, to obtain the mixture from step 7.
[0133] Step 8: Under the condition that the homogenizer speed is 100-1000 r / min, such as 400 r / min, gradually and evenly add 30%-40% mass fraction of the reaction monomer mixture to the seventh mixture (controlling the addition to be completed in 60 min), and the reaction time is 100-160 min, such as 120 min, to obtain the eighth mixture.
[0134] Step 9: Add 5-20% by mass of plasticizer, such as glycerin, to the mixture from step 8. Control the reaction temperature at 80-90℃, such as 84℃; the homogenizer speed at 12000-18000 r / min, such as 15000 r / min; and the reaction time at 120-240 min, such as 180 min, to obtain the mixture from step 9.
[0135] Step 10: Cool the mixture from step 9 to below 50°C, filter the mixture, and obtain the core-shell structured pressure-sensitive adhesive polymer. Those skilled in the art can also synthesize non-core-shell structured pressure-sensitive adhesive polymers by referring to the above method (omitting steps 7 to 9 and correspondingly changing the mass fraction of the added plasticizer and reactive monomer mixture).
[0136] In some embodiments, the average thickness of the pressure-sensitive coating may be 2-20 μm, and optionally 2-15 μm.
[0137] In some embodiments, the average particle size of the first organic particles can be 5-30 μm, optionally 5-20 μm. The average particle size of the first organic particles can be determined using a laser particle size analyzer (such as a Malvern Master Size 3000) in accordance with standard GB / T 19077.1-2016. When the average particle size of the first organic particles is controlled at 5-30 μm, the first organic particles have a larger average particle size. On the one hand, this increases the effective contact area between the electrode and the separator, thereby significantly improving the adhesion between the electrode and the separator. On the other hand, it prevents these organic particles from penetrating into the pores formed in the separator substrate. Furthermore, the larger size results in relatively larger voids, thus solving the problem of poor air permeability of the separator and reducing the possibility of small particles clogging the separator pores, avoiding the risk of increased internal resistance. Furthermore, because the corners are not laminated during cell manufacturing (especially for prismatic batteries), the separator and electrode are not bonded at these points. The separator cannot effectively transfer and release the accumulated stress from the electrode. Moreover, the inherent structure of the prismatic battery cell module causes the corners to be blocked, making it difficult to release the stress generated by electrode expansion. Therefore, if there is insufficient space at the battery corners, when cycling reaches a certain point—that is, when the stress exceeds the elongation of the copper-aluminum foil—the electrode will break, potentially puncturing the separator and posing a serious safety risk. In this invention, the first organic particles, with their large average particle size and compressibility, effectively provide stress release space at the cell corners when present there.
[0138] In some embodiments, the DSC melting point of the first organic particles can be -50℃ to 200℃, or optionally -40℃ to 160℃. When the DSC melting point of the first organic particles is within this range, it can withstand electrolyte swelling. On the one hand, it will not consume excessive electrolyte, and residual monomers are less likely to be soaked out by the electrolyte and block the separator, thus affecting the dynamic performance of the battery cell. On the other hand, it will not cause a significant decrease in the adhesion between the separator and the electrode, and the electrode is less likely to be damaged by the first organic particles, leading to a decrease in safety performance.
[0139] In some embodiments, the weight-average molecular weight of the first organic particles may be 300 × 10⁻⁶. 3 g / mol - 800 × 10 3 g / mol, can be selected as 400×10 3 g / mol - 650 × 10 3 g / mol.
[0140] The weight-average molecular weight of the first organic particles is within the aforementioned range, ensuring suitable swelling and adhesion to the electrode. For the same type of first organic particles, an excessively high weight-average molecular weight results in insufficient swelling, hindering electrolyte replenishment during later stages of cell cycling and affecting cell performance. Conversely, an excessively high weight-average molecular weight leads to excessively high modulus, directly damaging the electrode and impacting cell safety. Conversely, an excessively low weight-average molecular weight results in excessive swelling, causing a large amount of residual monomers to dissolve under the influence of the electrolyte, increasing the resistance of the separator and deteriorating the electrolyte, thus affecting the cell's dynamic performance.
[0141] The weight-average molecular weight (Mw) was measured using a Tosoh HLC-8320 GPC gel permeation chromatography system (SuperMultipore HZ series semi-micro SEC column, polystyrene as standard). The test method was as follows: 2 mg of the polymer powder to be tested was dissolved in 2 mL of GPC-specific DMF solvent, and then 2.5 μL was injected for testing. The parameters were set as follows: pump flow rate: 5 mL / min; injection volume: 100 μL; temperature control range: 60℃; data acquisition frequency: 100 Hz.
[0142] In some embodiments, the first organic particle may be a polymer comprising one or more groups selected from the following: halogen, phenyl, epoxy, cyano, ester, and amide.
[0143] In some embodiments, the first organic particle may be a homopolymer or copolymer of fluorinated alkenyl monomer units, a homopolymer or copolymer of olefinic monomer units, a homopolymer or copolymer of unsaturated nitrile monomer units, a homopolymer or copolymer of epoxide monomer units, a dimer, homopolymer or copolymer of monosaccharide monomer units, and a modified compound of each of the above homopolymers or copolymers.
[0144] In some embodiments, the fluorinated alkenyl monomer unit may be selected from one or more of difluoroethylene, vinylidene fluoride, trifluoroethylene, trifluorochloroethylene, tetrafluoroethylene, hexafluoropropylene, or derivatives thereof.
[0145] In some embodiments, the olefin-based monomer unit may be selected from one or more of ethylene, propylene, butadiene, isoprene, styrene, or derivatives thereof.
[0146] In some embodiments, the unsaturated nitrile monomer unit may be selected from one or more of acrylonitrile, methacrylonitrile, or their derivatives.
[0147] In some embodiments, the epoxide monomer unit may be selected from one or more of ethylene oxide, propylene oxide, or their derivatives.
[0148] In some embodiments, the monosaccharide monomer unit may be selected from glucose or a derivative thereof.
[0149] In some embodiments, the first organic particle may be selected from at least one of the following: perfluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose.
[0150] In some embodiments, the first organic particle may be selected from at least one of the following: polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, perfluorinated polyvinyl chloride, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.
[0151] When the first organic particle is selected from the above-mentioned substances, it exhibits suitable swelling and appropriate adhesion to the electrode. This enables the achievement of suitable bonding force with the pressure-sensitive adhesive polymer, while simultaneously ensuring uniform dispersion of the pressure-sensitive adhesive polymer on it, thus guaranteeing both adhesion and kinetic properties.
[0152] In some embodiments, the mass ratio of the first organic particles to the second organic particles can be (1-4):1, or optionally (1.5-2.5):1. When the mass ratio of the first organic particles to the second organic particles is within the above range, the wettability and distribution uniformity of the electrolyte can be effectively improved, further enhancing the high-temperature storage performance of the battery. In particular, if a foreign object is inserted into the battery during use, the second organic particles can instantly wrap the foreign object and the exposed copper or aluminum foil, forming a first polymer insulating layer, effectively reducing the probability of short circuits between the positive and negative electrodes and improving the battery's safety performance. As the temperature around the foreign object increases, the first organic particles will form a more robust second polymer insulating layer around the first polymer insulating layer, thereby further improving the battery's safety performance.
[0153] In some embodiments, the average particle size of the second organic particles can be 0.5-10 μm, optionally 2-8 μm. The average particle size of the second organic particles can be determined using a laser particle size analyzer (such as a Malvern Master Size 3000) in accordance with standard GB / T 19077.1-2016. Using second organic particles within the above particle size range allows for the formation of sufficient and unevenly distributed voids between the first and second organic particles during normal operation of the secondary battery, ensuring unobstructed ion transport channels and thus further enhancing the battery's cycle performance. Simultaneously, when the secondary battery operates at high temperatures (e.g., due to cell failure and high temperatures), the first and second organic particles can form a large-area gel film structure, reducing or blocking ion transport channels, preventing further contact between the positive and negative electrodes, delaying thermal runaway, and further improving the battery's safety performance. The first organic particles have a relatively large average particle size and are typically designed as secondary particles, while the second organic particles have a relatively small average particle size and are typically designed as primary particles. The combined effect of the first and second organic particles enhances the adhesion between the separator and the electrode plates while effectively ensuring that the separator has a moderately non-uniform porosity. Furthermore, during battery cell fabrication, the secondary organic particles help form a uniform coating interface, effectively improving the problem of electrode misalignment. The primary organic particles, being primary particles, are less prone to forming large-area adhesive film structures between particles, thus preventing pore blockage and further improving the battery's rate performance and safety performance.
[0154] In some embodiments, the DSC melting point of the second organic particles can be -30 to 100°C, preferably -30 to 70°C. When the DSC melting point of the second organic particles is within the above range, it can withstand electrolyte swelling. On the one hand, it will not consume too much electrolyte, and residual monomers will not be easily soaked out by the electrolyte and block the separator, thereby affecting the dynamic performance of the cell. On the other hand, it will not cause a significant decrease in the adhesion between the separator and the electrode, and the electrode will not be easily damaged by the second organic particles, resulting in a decrease in safety performance.
[0155] The DSC melting point is a term known in the art and can be determined using instruments and methods known in the art, such as the DSC 200F3 DSC melting point analyzer from NETZSC GmbH, Germany. As a specific example, the test method is as follows: Approximately 10 mg of sample is taken for testing. Test conditions are set as follows: temperature range: -100-200℃, nitrogen atmosphere, 10℃ / min. The temperature corresponding to the absorption peak during the first heating is selected as the DSC melting point.
[0156] In some embodiments, the weight-average molecular weight of the second organic particles may be 10 × 10⁻⁶. 3 g / mol-100×10 3 g / mol, which can be selected as 20×10 3 g / mol - 80 × 10 3 g / mol.
[0157] The weight-average molecular weight of the second organic particles is within the aforementioned range, ensuring suitable swelling and adhesion to the electrode. For the same type of second organic particles, an excessively high weight-average molecular weight results in insufficient swelling, hindering electrolyte replenishment during later stages of cell cycling and affecting cell performance. Conversely, an excessively high weight-average molecular weight leads to excessively high modulus, directly damaging the electrode and impacting cell safety. Conversely, an excessively low weight-average molecular weight results in excessive swelling, causing a large amount of residual monomers to dissolve under electrolyte conditions, increasing the separator resistance and deteriorating the electrolyte, thus affecting cell kinetics. The testing method for the weight-average molecular weight of the second organic particles is the same as that for the first organic particles.
[0158] In some embodiments, the second organic particle is a polymer comprising one or more groups selected from the following: phenyl, epoxy, cyano, ester, hydroxy, carboxyl, sulfonyl ester, and pyrrolidone.
[0159] In some embodiments, the second organic particle may be a homopolymer or copolymer of acrylate monomer units, a homopolymer or copolymer of acrylic monomer units, a homopolymer or copolymer of unsaturated nitrile monomer units, a homopolymer or copolymer of olefin monomer units, a homopolymer or copolymer of styrene monomer units, a homopolymer or copolymer of epoxy monomer units, a polyurethane compound, a rubber compound, a dimer, homopolymer or copolymer of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers.
[0160] In some embodiments, the acrylate monomer unit may be selected from one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, methyl methacrylate, butyl methacrylate, isooctyl methacrylate, or derivatives thereof.
[0161] In some embodiments, the acrylic monomer unit may be selected from one or more of acrylic acid, methacrylic acid, or derivatives thereof.
[0162] In some embodiments, the unsaturated nitrile monomer unit may be selected from one or more of acrylonitrile, methacrylonitrile, or their derivatives.
[0163] In some embodiments, the olefinic monomer unit may be selected from one or more of ethylene, vinyl acetate, butadiene, or their derivatives.
[0164] In some embodiments, the styrene monomer unit may be selected from one or more of styrene, methylstyrene, or their derivatives.
[0165] In some embodiments, the epoxy monomer unit may be selected from one or more of ethylene oxide, propylene oxide, or their derivatives.
[0166] In some embodiments, the monosaccharide monomer unit may be selected from glucose or a derivative thereof.
[0167] In some embodiments, the second organic particle is selected from at least one of the following: polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer, styrene-butyl acrylate-isooctyl acrylate copolymer, and polyimide.
[0168] When the second organic particle is selected from the above-mentioned substances, it exhibits suitable swelling and appropriate adhesion to the electrode. This allows for suitable bonding with the pressure-sensitive adhesive polymer while ensuring uniform dispersion of the polymer, thus guaranteeing both adhesion and kinetic properties.
[0169] In some embodiments, the porosity of the separator substrate can be 10-95%, the pore size can be 20-60 nm, and the thickness can be 3-12 μm, optionally 5-9 μm. When the porosity of the separator substrate is within the above range, a balance between the kinetics and safety performance of the secondary battery can be achieved; when the thickness of the separator substrate is within the above range, a balance between the energy density and safety performance of the secondary battery can be achieved.
[0170] In some embodiments, the separator substrate may include a membrane or nonwoven fabric selected from one or more of the following: polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymer, polyphenylene sulfide, and polyvinyl naphthalene.
[0171] Preparation method of the separator
[0172] This application also provides a method for preparing a separating membrane, which includes the following steps:
[0173] S1) The first organic particles and dispersant are added to the solvent to form a first polymer solution;
[0174] S2) Add the pressure-sensitive adhesive polymer to the first polymer solution obtained in step S1) and mix to form a second polymer solution;
[0175] S3) Optionally, the second organic particles are added to the second polymer solution obtained in step S2), and mixed to form a third polymer solution; and
[0176] S4) The second polymer solution obtained in step S2) or the third polymer solution obtained in step S3) is coated onto at least one surface of the porous separator substrate, and the separator is obtained after drying.
[0177] The isolation membrane includes a pressure-sensitive coating formed on at least one surface of the isolation membrane substrate, comprising 40-90 wt% of first organic particles and 10-20 wt% of a pressure-sensitive adhesive polymer, and optionally 0-50 wt% of second organic particles; wherein the pressure-sensitive adhesive polymer comprises an adhesive polymer and a plasticizer.
[0178] In some embodiments, non-limiting examples of the dispersant used in step S1) may include acrylates (such as BYK brand 22136), branched alcohol polyethers (such as Dow brand TMN-6), and polyethylene glycol trimethyl nonyl ether. Non-limiting examples of the solvent used in step S1) may include acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane, water, or mixtures thereof.
[0179] In some embodiments, non-limiting examples of the coating method used in step S4) may include dip coating, mold coating, roller coating, comma coating, spin coating, or combinations thereof. The weight of the single-sided coating after drying may be 0.42-0.52 g / m². 2 .
[0180] [Outer Packaging]
[0181] In some embodiments, the secondary battery may include an outer packaging for encapsulating a positive electrode, a negative electrode, a separator, and an electrolyte. As an example, the positive electrode, negative electrode, and separator may be stacked or wound to form a stacked or wound battery cell, with the cell encapsulated within the outer packaging; the electrolyte may be a liquid electrolyte that wets the cell. The number of cells in the secondary battery may be one or more, adjustable as needed.
[0182] In some embodiments, the outer packaging of the secondary battery can be a soft pack, such as a pouch. The soft pack can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS). The outer packaging of the secondary battery can also be a hard shell, such as an aluminum shell.
[0183] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly by a winding process or a stacking process.
[0184] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. Figure 1 This is an example of a square-structured secondary battery 5.
[0185] The secondary batteries provided by this invention can be assembled into battery modules. The number of secondary batteries contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.
[0186] Figure 2 This is battery module 4, used as an example. (See reference...) Figure 2 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0187] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0188] In this invention, battery modules assembled from secondary batteries can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack.
[0189] Figure 3 and Figure 4 This is battery pack 1 as an example. (See reference...) Figure 3 and Figure 4 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0190] Electrical appliances
[0191] This application also provides an electrical device, which includes a secondary battery provided by this application, the secondary battery providing power to the electrical device. The electrical device may be, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0192] The electrical device can be equipped with a secondary battery, battery module, or battery pack according to its usage requirements.
[0193] Figure 5 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0194] Another example of an electrical device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use rechargeable batteries as their power source.
[0195] Example
[0196] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0197] Example 1
[0198] Preparation of the separating membrane
[0199] 1) A polyethylene microporous membrane with a thickness of approximately 9 μm, a pore size of approximately 50 nm, and a porosity of approximately 38% was selected as the substrate for the isolation membrane;
[0200] 2) The first organic particles (polyvinylidene fluoride-co-hexafluoropropylene (of which, based on the weight of vinylidene fluoride (VDF) monomer and hexafluoropropylene (HFP) monomer, HFP monomer accounts for approximately 9%), have a weight-average molecular weight of approximately 600 × 10⁻⁶. 3 g / mol, with an average particle size of about 7 μm and a DSC melting point of about 150 °C) and dispersant (BYK-22136) are added to water to form a first polymer solution;
[0201] 3) A pressure-sensitive adhesive polymer (with a glass transition temperature of approximately 10°C and an average particle size of approximately 1.1 μm, comprising an adhesive polymer and a plasticizer in a mass ratio of 5:1 (wherein approximately 8 wt% of the plasticizer is grafted onto the adhesive polymer relative to its weight) and a certain amount of deionized water, wherein the adhesive polymer is a copolymer of 30% isobutyl acrylate + 25% isooctyl acrylate + 5% 2-hydroxypropyl methacrylate + 15% styrene + 22% acrylonitrile + 3% polyvinyl alcohol, and the plasticizer is glycerol) is added to the first polymer solution obtained in step 2) and mixed to form a second polymer solution with a solid content of 12 wt%, wherein the mass ratio of the first organic particles to the pressure-sensitive adhesive polymer is 85:15;
[0202] 4) The second polymer solution with a solid content of 12 wt% obtained in step 3) is used as an aqueous coating slurry and coated onto one surface of the separator substrate by spin-jet coating. After drying, the separator is obtained. The prepared separator includes a separator substrate and a pressure-sensitive coating coated on one surface of the separator substrate. The pressure-sensitive coating has a thickness of about 3 μm and includes first organic particles and a pressure-sensitive adhesive polymer in a mass ratio of 85:15. The pressure-sensitive adhesive polymer includes an adhesive polymer and a plasticizer in a mass ratio of 5:1 (wherein about 8 wt% of the plasticizer is grafted onto the adhesive polymer relative to the weight of the plasticizer).
[0203] Preparation of secondary batteries
[0204] Active material LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were thoroughly mixed in a solvent N-methylpyrrolidone at a weight ratio of 94:3:3 to obtain a positive electrode slurry. This slurry was then coated onto an Al foil, dried, and cold-pressed to obtain the positive electrode sheet. The loading of the positive electrode active material on the positive electrode sheet was 0.32 g / 1540.25 mm². 2 Its density is 3.45 g / cm³. 3 .
[0205] Artificial graphite (active material), acetylene black (conductive agent), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (CMC) (thickener) were thoroughly mixed in deionized water at a weight ratio of 95:2:2:1 to obtain a negative electrode slurry. This slurry was then coated onto a Cu foil, dried, and cold-pressed to obtain the negative electrode sheet. The graphite loading on the negative electrode sheet was 0.18 g / 1540.25 mm. 2 Its density is 1.65 g / cm³. 3 .
[0206] Ethyl carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 3:5:2. LiPF6 was then uniformly dissolved in this solution to obtain the electrolyte. The concentration of LiPF6 in the electrolyte was 1 mol / L.
[0207] The separators prepared according to the various embodiments or comparative examples are used as separators for battery cells.
[0208] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. This is then wound to obtain a bare cell. The bare cell is placed in outer packaging, electrolyte is injected, and it is then sealed to obtain a secondary battery. It should be noted that if the separator coating is single-sided, the coated side should face the cathode (i.e., the positive electrode).
[0209] Evaluation of the adhesive properties of the release liner
[0210] The testing process is as follows:
[0211] 1. Select a separator membrane with a length of 300 mm and a width of 100 mm, and the above-prepared positive and negative electrode sheets.
[0212] 2. Wrap the release liner with paper on both sides and use a die and a punch to cut it into samples of 54.2mm*72.5mm.
[0213] 3. Neatly stack the cut separator sample with the positive or negative electrode sheet, making sure the separator is facing upwards. Place 130mm*130mm Teflon pads on top and bottom, place the stacked sample in the middle of a cardboard, and cover it with a 150mm*160mm cardboard.
[0214] 4. Place the stacked samples into the flatbed press and adjust the pressure. Adjust the air pressure to 350KG±10KG (equivalent to about 0.87MPa) or 850Kg±10KG (equivalent to about 2.24MPa). Set T=25℃ and time to 15s for hot pressing.
[0215] 5. Cut the hot-pressed sample into strips of 72.5mm*15mm using a die and a punch.
[0216] 6. Secure one side of the electrode to the steel plate using double-sided tape, and attach the separator to the other side. Use double-sided tape to attach a 15mm wide strip of A4 paper to the separator, completing the test sample preparation. During testing, fix the steel plate holding the electrode in place, and use a tensile testing machine to pull the A4 paper strip upwards, separating the separator from the electrode.
[0217] 7. Turn on the high-speed rail tensile testing machine and set it in sequence as follows: adhesion force test, speed 50mm / min, and initial clamp spacing 40mm.
[0218] 8. Place the test sample between the clamps, fix the end of the steel plate to the lower clamp, and fix the A4 paper to the upper clamp. Clamp the upper and lower clamps with the fixtures respectively.
[0219] 9. Click on the stretching operation interface on the computer desktop, clear the force and displacement to zero, and then click "Start" to perform a pre-stretch of about 5mm; after the pre-stretch, clear the force and displacement to zero again, start the test, and after the test is completed, export and save the complete data.
[0220] 10. For each group, at least 5 test samples must be measured, and if the adhesion test curves of the 5 test samples show good repeatability, then proceed to the next group of tests. Otherwise, the tests need to be repeated until the repeatability of the 5 test samples is good.
[0221] 11. After the test is completed, plot the bond strength (N / m)-displacement curve and calculate the bond force.
[0222] Evaluation of the resistivity of the separator
[0223] The testing process is as follows:
[0224] (1) Preparation of isolation membrane: Cut each isolation membrane to be tested into samples of the same size (45.3mm*33.7mm), and bake the samples at 60℃ for at least 4 hours, and then quickly transfer them into a 25℃ Class 100 clean glove box for later use.
[0225] (2) Preparation of Symmetrical Battery Confinement Pocket Bag (Symmetrical Battery Confinement Aluminum-Plastic Bag (Aluminum-Plastic Bag is a common commodity of polypropylene and aluminum foil composite for soft-pack batteries)): Blank symmetric batteries are assembled using Cu Foil to Cu Foil (copper foil to copper foil) as current collectors. The confinement of the Pocket Bag is achieved by punching a hole in the center of the green adhesive. Before use, the Pocket Bag should be baked at 60°C for at least 4 hours, and then quickly transferred to a 25°C Class 100 clean glove box as described in (1) above for later use;
[0226] (3) Assembly of symmetrical cells: Using the anode as the electrode, five groups of symmetrical cell samples with different numbers of separator layers (1, 2, 3, 4, 5 layers) were assembled in situ in the glove box as described in (1) above. Each group of samples had five parallel samples. The Pocket bag was side-sealed with a simple packaging machine, liquid was injected (300 μL) with a pipette, and the bottom was sealed.
[0227] (4) Apply clamps to the assembled symmetrical battery: Place the assembled symmetrical battery in the glove box as described in (1) above overnight so that the electrolyte can fully wet the separator; the next day, apply metal clamps, and control the pressure of the clamps at 0.7 MPa;
[0228] (5) Measurement of electrochemical impedance spectroscopy (EIS):
[0229] Before measurement, symmetrical cells with different numbers of separator layers are placed in a high and low temperature chamber at 25°C for half an hour and the EIS is measured at the set temperature (25°C). (If it is a low temperature (e.g. -25°C to 0°C), the constant temperature time can be extended accordingly, such as about two hours).
[0230] (6) A French Bio-Logic VMP3 electrochemical workstation was used, with a voltage of <5V, a current of <400mA, and a current accuracy of 0.1%*100μA. During the measurement, the EIS measurement conditions were set to a voltage frequency of 1MHz-1kHz, a disturbance voltage of 5MV, and a clamp pressure of 0.7MPa.
[0231] (7) Plot a scatter plot of the real part of the EIS data against the negative imaginary part. At the same time, plot the data of parallel samples with different numbers of layers and the same number of layers on one plot. The resulting EIS plot can be used as a comparison of the original EIS data.
[0232] (8) Remove the points in the EIS image obtained in (7) that are not in the first quadrant to obtain a new EIS image. Perform linear fitting on the scatter points in the first quadrant of the new EIS image to obtain the correlation. Let y = 0 to obtain the x value, which is the required resistance value of the electrolyte in the separator. By analogy, the resistance values between parallel samples with different numbers of layers can be obtained by performing linear fitting on the measured EIS data.
[0233] Performance evaluation of secondary batteries
[0234] Cyclic performance test:
[0235] Five batteries were taken from each of the prepared secondary batteries, and the secondary batteries were repeatedly charged and discharged through the following steps. The cycle capacity retention rate of the secondary batteries under the conditions of 25℃ or 45℃ was calculated.
[0236] In an environment of 25℃, the first charge and discharge cycle was performed. Constant current and constant voltage charging was conducted at a charging current of 0.7C (the current value required to completely discharge the theoretical capacity within 2 hours) until the upper limit voltage reached 4.4V. Then, constant current discharging was performed at a discharging current of 0.5C until the final voltage reached 3V. The discharge capacity of the first cycle was recorded. Subsequently, 1000 charge and discharge cycles were performed, and the discharge capacity of the 1000th cycle was recorded. Cycle capacity retention rate = (Discharge capacity of the 1000th cycle / Discharge capacity of the first cycle) × 100%.
[0237] The first charge and discharge cycle was performed at 45℃. Constant current and constant voltage charging was conducted at a charging current of 0.7C (the current required to completely discharge the theoretical capacity within 2 hours) until the upper limit voltage reached 4.4V. Then, constant current discharging was performed at a discharging current of 0.5C until the final voltage reached 3V. The discharge capacity of the first cycle was recorded. Subsequently, 1000 charge and discharge cycles were performed, and the discharge capacity of the 1000th cycle was recorded. Cycle capacity retention rate = (Discharge capacity of the 1000th cycle / Discharge capacity of the first cycle) × 100%.
[0238] Example 2-3
[0239] Except for the different mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating, everything else is the same as in Example 1. Specifically:
[0240] In Example 2, the mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating of the isolation membrane was 90:10.
[0241] In Example 3, the mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating of the isolation membrane was 80:20.
[0242] Examples 4-9
[0243] Except for the different adhesive polymer or plasticizer used in the pressure-sensitive adhesive polymer, everything else is the same as in Example 1. Specifically:
[0244] The pressure-sensitive adhesive polymer used in Example 4 is a copolymer of 30% isobutyl acrylate, 25% isooctyl acrylate, 5% 2-hydroxypropyl acrylate, 15% styrene, 22% acrylamide, and 3% polyethylene glycol, with glycerol as the plasticizer.
[0245] The pressure-sensitive adhesive polymer used in Example 5 consists of a copolymer of 30% cyclohexyl acrylate, 25% tetrahydrofuran methacrylate, 5% 2-hydroxypropyl methacrylate, 15% styrene, 22% acrylonitrile, and 3% polyethylene glycol, with glycerol as the plasticizer.
[0246] The pressure-sensitive adhesive polymer used in Example 6 is a copolymer of 30% cyclohexyl acrylate, 25% tetrahydrofuran methacrylate, 5% divinylbenzene, 15% styrene, 22% acrylonitrile, and 3% polyethylene glycol, with glycerol as the plasticizer.
[0247] The pressure-sensitive adhesive polymer used in Example 7 is a copolymer of 30% isobutyl acrylate, 25% isooctyl acrylate, 5% divinylbenzene, 15% styrene, 22% acrylonitrile, and 3% polyvinyl alcohol, and the plasticizer is glycerol.
[0248] The pressure-sensitive adhesive polymer used in Example 8 is a copolymer of 30% isobutyl acrylate, 25% isooctyl acrylate, 5% 2-hydroxypropyl methacrylate, 15% styrene, 22% acrylonitrile, and 3% polyvinyl alcohol, and the plasticizer is glycerol C4-C10 alkyl diether.
[0249] The pressure-sensitive adhesive polymer used in Example 9 is a copolymer of 30% isobutyl acrylate, 25% isooctyl acrylate, 5% 2-hydroxypropyl methacrylate, 15% styrene, 22% acrylonitrile, and 3% polyvinyl alcohol, and the plasticizer is propylene glycol C4-C10 alkyl monoether.
[0250] Examples 10-12
[0251] Except for the different grafting rate of the plasticizer in the pressure-sensitive adhesive polymer used, everything else is the same as in Example 1. Specifically:
[0252] The plasticizer grafting in the pressure-sensitive adhesive polymer used in Example 10 was 5 wt%.
[0253] The plasticizer grafting in the pressure-sensitive adhesive polymer used in Example 11 was 3 wt%.
[0254] The plasticizer grafting in the pressure-sensitive adhesive polymer used in Example 12 was 0 wt%, meaning the plasticizer was ungrafted.
[0255] Example 13
[0256] Preparation of the separating membrane
[0257] 1) A polyethylene microporous membrane with a thickness of approximately 9 μm, a pore size of approximately 50 nm, and a porosity of approximately 38% was selected as the substrate for the isolation membrane;
[0258] 2) The first organic particles (polyvinylidene fluoride-co-hexafluoropropylene (of which, based on the weight of vinylidene fluoride (VDF) monomer and hexafluoropropylene (HFP) monomer, HFP monomer accounts for approximately 9%), have a weight-average molecular weight of approximately 600 × 10⁻⁶. 3 g / mol, with an average particle size of about 7 μm and a DSC melting point of about 150 °C) and dispersant (BYK-22136) are added to water to form a first polymer solution;
[0259] 3) A pressure-sensitive adhesive polymer (with a DSC melting point of approximately 10°C and an average particle size of approximately 1.1 μm, comprising an adhesive polymer and a plasticizer in a mass ratio of 5:1 (where approximately 8 wt% of the plasticizer is grafted onto the adhesive polymer relative to its weight) and a certain amount of deionized water, wherein the adhesive polymer is a copolymer of 30% isobutyl acrylate + 25% isooctyl acrylate + 5% 2-hydroxypropyl methacrylate + 15% styrene + 22% acrylonitrile + 3% polyvinyl alcohol, and the plasticizer is glycerol) is added to the first polymer solution obtained in step 2) and mixed to form a second polymer solution with a solid content of 12 wt%.
[0260] 4) Add the second organic particles (30% styrene-50% butyl acrylate-20% isooctyl acrylate, average particle size of 4 μm, DSC melting point of about 55°C) to the second polymer solution obtained in step 3), so that the mass ratio of the first organic particles to the second organic particles is 65:20, and mix to form a third polymer solution with a solid content of 12%, wherein the mass ratio of the organic particles (including the first organic particles and the second organic particles with a mass ratio of 65:20) to the pressure-sensitive adhesive polymer is 85:15;
[0261] 5) The third polymer solution with a solid content of 12 wt% obtained in step 4) is used as an aqueous coating slurry and coated onto one surface of the separator substrate by spin-jet coating. After drying, the separator is obtained. The prepared separator includes a separator substrate and a pressure-sensitive coating coated on one surface of the separator substrate. The pressure-sensitive coating has a thickness of about 3 μm and includes organic particles (including first and second organic particles with a mass ratio of 65:20) and a pressure-sensitive adhesive polymer in a mass ratio of 85:15. The pressure-sensitive adhesive polymer includes an adhesive polymer and a plasticizer in a mass ratio of 5:1 (wherein about 8 wt% of the plasticizer is grafted onto the adhesive polymer relative to its weight). Figure 6 As shown, the morphology of the pressure-sensitive coating of the diaphragm prepared in this embodiment is illustrated.
[0262] Examples 14-15
[0263] Except for the different mass ratio of organic particles to pressure-sensitive adhesive polymer in the pressure-sensitive coating, it is the same as in Example 13. Specifically:
[0264] In Example 14, the pressure-sensitive coating of the isolation membrane has a mass ratio of organic particles to pressure-sensitive adhesive polymer of 85:15, wherein the mass ratio of the first organic particles to the second organic particles is 75:10.
[0265] In Example 15, the pressure-sensitive coating of the isolation membrane has a mass ratio of organic particles to pressure-sensitive adhesive polymer of 90:10, wherein the mass ratio of the first organic particles to the second organic particles is 65:25.
[0266] Comparative Examples 1-2
[0267] Except for the different mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating, everything else is the same as in Example 1. Specifically:
[0268] In Comparative Example 1, the mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating of the separator was 91:9.
[0269] In Comparative Example 2, the mass ratio of the first organic particles to the pressure-sensitive adhesive polymer in the pressure-sensitive coating of the isolation membrane was 74:26.
[0270] Comparative Examples 3-4
[0271] Except for not using the pressure-sensitive adhesive polymer described in Example 1, everything else is the same as in Example 1. Specifically:
[0272] The separator prepared in Comparative Example 3 uses only the adhesive polymer and contains no plasticizer. In the pressure-sensitive coating of the prepared separator, the mass ratio of the first organic particles to the adhesive polymer is 85:15.
[0273] The separator prepared in Comparative Example 4 uses only plasticizer and does not contain adhesive polymer. In the pressure-sensitive coating of the prepared separator, the mass ratio of the first organic particles to the plasticizer is 85:15.
[0274] The adhesive properties, resistance, and cycle performance of the separators prepared in Examples 1-15 and Comparative Examples 1-4 were evaluated, and the results are shown in Table 1 below.
[0275] Table 1: Performance of the separators prepared in Examples 1-15 and Comparative Examples 1-4, and cycle performance test results of the secondary batteries prepared from these separators.
[0276]
[0277]
[0278] As shown in Table 1 above, the use of a pressure-sensitive adhesive polymer prepared from an adhesive polymer and a plasticizer, combined with organic particles, effectively endows the separator with high adhesion and ion conduction capabilities at room temperature. Under room temperature conditions, the resistance of the prepared separator is below 1.32Ω. Under ≥2MPa, the adhesion force with the cathode electrode is above 0.70N / m, even above 1.00N / m, and the adhesion force with the anode electrode is above 0.50N / m. Under ≤1MPa, the adhesion force with the electrode is below 0.1N / m. Therefore, the prepared separator can avoid layer-to-layer adhesion during winding and storage. Furthermore, when using this separator to prepare battery cells, the electrode and separator can be tightly bonded at room temperature. This avoids misalignment between the electrode and separator, preventing cell scrap, performance degradation, and safety risks. It also eliminates the need for a tunnel furnace and a second composite process in traditional battery cell manufacturing, saving production space and time, reducing energy consumption, and significantly increasing battery cell production capacity. Simultaneously, it improves cell shaping performance, safety performance, and kinetic performance. The results of Examples 10-12 show that grafting plasticizers into the pressure-sensitive adhesive polymer helps reduce the separator's resistance and improves the cycle performance of secondary batteries prepared from the separator. This is especially true when the plasticizer grafting rate in the pressure-sensitive adhesive polymer is above 5 wt%, which further facilitates obtaining a separator with lower resistance and a secondary battery with superior cycle performance. The results of Comparative Examples 1-2 show that both excessive and insufficient use of pressure-sensitive adhesive polymers lead to a significant increase in the resistance of the separator and a substantial deterioration in the cycle performance of the secondary battery. The results of Comparative Examples 3-4 show that using only one type of pressure-sensitive adhesive polymer—either an adhesive polymer or a plasticizer—leads to a deterioration in the adhesive properties of the separator and a deterioration in the cycle performance of the secondary battery. Furthermore, when the pressure-sensitive adhesive polymer consists entirely of plasticizers, the resistance of the separator increases significantly, and the cycle performance of the secondary battery deteriorates even further.
[0279] Examples 16-20
[0280] Except for the different particle size of the first organic particles and the different thickness of the pressure-sensitive coating, everything else is the same as in Example 1. Specifically:
[0281] The first organic particles used in Example 16 have a particle size of about 3 μm and a pressure-sensitive coating thickness of about 0.8 μm.
[0282] The first organic particles used in Example 17 have a particle size of about 5 μm and a pressure-sensitive coating thickness of about 2 μm.
[0283] The first organic particles used in Example 18 have a particle size of approximately 20 μm, and the pressure-sensitive coating has a thickness of approximately 15 μm.
[0284] The first organic particles used in Example 19 have a particle size of about 30 μm and a pressure-sensitive coating thickness of about 20 μm.
[0285] The first organic particles used in Example 20 have a particle size of approximately 36 μm, and the pressure-sensitive coating has a thickness of approximately 22 μm.
[0286] Examples 21-27
[0287] Except for the different particle size of the pressure-sensitive adhesive polymer, everything else is the same as in Example 1. Specifically:
[0288] The pressure-sensitive adhesive polymer used in Example 21 has a particle size of approximately 0.3 μm.
[0289] The pressure-sensitive adhesive polymer used in Example 22 has a particle size of approximately 0.5 μm.
[0290] The pressure-sensitive adhesive polymer used in Example 23 has a particle size of approximately 0.8 μm.
[0291] The pressure-sensitive adhesive polymer used in Example 24 has a particle size of approximately 1.0 μm.
[0292] The pressure-sensitive adhesive polymer used in Example 25 has a particle size of approximately 2.0 μm.
[0293] The pressure-sensitive adhesive polymer used in Example 26 has a particle size of approximately 3.0 μm.
[0294] The pressure-sensitive adhesive polymer used in Example 27 has a particle size of approximately 3.5 μm.
[0295] Examples 28-32
[0296] Except for the different mass ratio of adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer used, everything else is the same as in Example 1. Specifically:
[0297] The pressure-sensitive adhesive polymer used in Example 28 comprises an adhesive polymer and a plasticizer in a mass ratio of approximately 3:1.
[0298] The pressure-sensitive adhesive polymer used in Example 29 comprises an adhesive polymer and a plasticizer in a mass ratio of approximately 4:1.
[0299] The pressure-sensitive adhesive polymer used in Example 30 comprises an adhesive polymer and a plasticizer in a mass ratio of approximately 11:1.
[0300] The pressure-sensitive adhesive polymer used in Example 31 comprises an adhesive polymer and a plasticizer in a mass ratio of approximately 19:1.
[0301] The pressure-sensitive adhesive polymer used in Example 32 comprises an adhesive polymer and a plasticizer in a mass ratio of approximately 21:1.
[0302] Examples 33-38
[0303] Except for the different particle size of the second organic particles used and the different thickness of the prepared pressure-sensitive coating, it is the same as in Example 14. Specifically:
[0304] The second organic particles used in Example 33 have a particle size of approximately 0.3 μm, and the thickness of the pressure-sensitive coating is approximately 3 μm.
[0305] The second organic particles used in Example 34 have a particle size of approximately 0.5 μm, and the thickness of the pressure-sensitive coating is approximately 3 μm.
[0306] The second organic particles used in Example 35 have a particle size of approximately 2 μm, and the thickness of the pressure-sensitive coating is approximately 3 μm.
[0307] The second organic particles used in Example 36 have a particle size of approximately 8 μm, and the thickness of the pressure-sensitive coating is approximately 4 μm.
[0308] The second organic particles used in Example 37 have a particle size of approximately 10 μm and a pressure-sensitive coating thickness of approximately 6 μm.
[0309] The second organic particles used in Example 38 have a particle size of approximately 12 μm, and the thickness of the pressure-sensitive coating is approximately 10 μm.
[0310] The adhesive properties, resistance, and cycle performance of the separators prepared in Examples 16-38 were evaluated, and the results are shown in Table 2 below.
[0311] Table 2: Performance of the separators prepared in Examples 16-38 and cycle performance test results of the secondary batteries prepared from these separators.
[0312]
[0313]
[0314] As shown in Table 2, the separators prepared in Examples 16-20 by changing the particle size of the first organic particles, Examples 21-27 by changing the particle size of the pressure-sensitive adhesive polymer, Examples 28-32 by changing the mass ratio of the adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer, and Examples 33-38 by changing the particle size of the second organic particles all exhibit good high adhesion performance and ion conduction capability at room temperature. Under room temperature conditions, their resistance is all below 1.3Ω, and their adhesion force to the cathode electrode is above 0.56N / m under ≥2MPa, while their adhesion force to the electrode is below 0.23N / m under ≤1MPa. The secondary batteries prepared using the separators prepared in each example also exhibit good cycle performance, with capacity retention rates above 70% under 25℃ and 45℃ conditions. Especially when the particle size of the first organic particles used is in the range of 5-30 μm, and / or the particle size of the pressure-sensitive adhesive polymer is in the range of 0.5-3 μm, and / or the mass ratio of the adhesive polymer and plasticizer included in the pressure-sensitive adhesive polymer is in the range of (4-19):1, and / or the particle size of the second organic particles is in the range of 0.5-10 μm, the separator can be more effectively endowed with good high adhesion performance and ion conduction capability at room temperature. Under room temperature conditions, its resistance is below 1.1 Ω, and the adhesion force with the cathode electrode is above 0.80 N / m under ≥2 MPa, while the adhesion force with the electrode is below 0.1 N / m under ≤1 MPa. The secondary batteries prepared using these separators also have better cycle performance, and their capacity retention rate is above 80% under 25℃ and 45℃ conditions.
[0315] Examples 39-47
[0316] Except that the pressure-sensitive adhesive polymer used is a core-shell structured pressure-sensitive adhesive polymer, the rest is the same as in Example 1. Both the core and shell of the core-shell structured pressure-sensitive adhesive polymer contain adhesive polymer and plasticizer. The specific mass ratios of adhesive polymer and plasticizer in the core and shell of the pressure-sensitive adhesive polymers used in Examples 39-47 are shown in Table 3 below.
[0317] The adhesive properties, resistance, and cycle performance of the separators prepared in Examples 39-47 above were evaluated, and the results are shown in Table 4 below.
[0318] Table 3: Mass ratio of adhesive polymer and plasticizer in the core and shell of the pressure-sensitive adhesive polymers used in Examples 39-47
[0319]
[0320] Table 4: Performance of the separators prepared in Examples 39-47 and cycle performance test results of the secondary batteries prepared from these separators.
[0321]
[0322]
[0323] As shown in Table 4 above, when a pressure-sensitive adhesive polymer with a core-shell structure, prepared from an adhesive polymer and a plasticizer, is used in the preparation of the separator, it can effectively impart high adhesion performance and ion conduction capability at room temperature. The resulting separators have low resistance, all below 0.9Ω. Under ≥2MPa, the adhesion force with the cathode electrode is above 1.21N / m, and the adhesion force with the anode electrode is above 0.85N / m. Under ≤1MPa, the adhesion force with the electrode is below 0.1N / m. Furthermore, the prepared secondary batteries all exhibit good cycle performance, with capacity retention rates above 89% under 25℃ and 45℃ conditions. Especially when the mass ratio of adhesive polymer to plasticizer in the core structure of the pressure-sensitive adhesive polymer in the core-shell structure is (3-4):1, and the mass ratio of adhesive polymer to plasticizer in the shell structure is (7-9):1, the separator can be further effectively endowed with high adhesion performance and ion conduction capability at room temperature. The resulting separator has lower resistance, all below 0.8Ω, and the adhesion force with the cathode electrode is above 1.23N / m under ≥2MPa and above 1.1N / m with the anode electrode, while the adhesion force with the electrode is below 0.1N / m under ≤1MPa. The secondary battery prepared from these separators also has better cycle performance, with a capacity retention rate of over 91% under 25℃ and 45℃ conditions.
[0324] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A separating membrane, characterized in that, include: Porous membrane substrate; and A pressure-sensitive coating applied to at least one surface of the separator substrate comprises 40-90 wt% of first organic particles, 10-20 wt% of pressure-sensitive adhesive polymer, and 0-50 wt% of second organic particles; The pressure-sensitive adhesive polymer comprises an adhesive polymer and a plasticizer, wherein a portion of the plasticizer is grafted onto the adhesive polymer; The pressure-sensitive coating satisfies the following condition: under an application pressure of ≤1 MPa, the adhesive force of the separator is below 0.23 N / m. Under pressure of ≥2MPa, the adhesive force of the separator is greater than 0.23 N / m; The average particle size of the first organic particle is 5-30 μm, and the first organic particle is a polymer containing halogen atoms and / or one or more groups selected from the following: phenyl, epoxy, cyano, ester and amide. The second organic particle has an average particle size of 0.5-10 μm and is a polymer containing one or more groups selected from the following: phenyl, epoxy, cyano, ester, hydroxy, carboxyl, sulfonyl ester and pyrrolidone.
2. The separator membrane according to claim 1, characterized in that, The mass ratio of the adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer is (4-19):
1.
3. The separator membrane according to claim 1, characterized in that, The mass ratio of the adhesive polymer and plasticizer in the pressure-sensitive adhesive polymer is (4-11):
1.
4. The separator according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive polymer has a core-shell structure, wherein both the core and the shell of the core-shell structure include an adhesive polymer and a plasticizer, wherein the mass ratio of the adhesive polymer to the plasticizer in the core structure is (2-5):1, and the mass ratio of the adhesive polymer to the plasticizer in the shell structure is (6-10):
1.
5. The separator according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive polymer has a core-shell structure, wherein both the core and the shell of the core-shell structure include an adhesive polymer and a plasticizer, wherein the mass ratio of the adhesive polymer to the plasticizer in the core structure is (3-4):1, and the mass ratio of the adhesive polymer to the plasticizer in the shell structure is (7-9):
1.
6. The separator according to claim 1 or 2, characterized in that, Based on the weight of the plasticizer, at least 5 wt% of the plasticizer is grafted onto the adhesive polymer.
7. The separator according to claim 1 or 2, characterized in that, Meet at least one of the following: The pressure-sensitive adhesive polymer has an average particle size of 0.5-3.0 μm; The DSC melting point of the pressure-sensitive adhesive polymer is -50℃ to 100℃.
8. The separator according to claim 1 or 2, characterized in that, Meet at least one of the following: The average particle size of the pressure-sensitive adhesive polymer is 0.8-2.0 μm; The DSC melting point of the pressure-sensitive adhesive polymer is -45℃ to 60℃.
9. The separator according to claim 1 or 2, characterized in that, The adhesive polymer comprises a copolymer formed by copolymerization of a mixture of reactive monomers comprising at least one of the following: a first monomer, at least one of the following: a second monomer, at least one of the following: a third monomer, and at least one of the following: a reactive dispersant. The first monomer includes acrylic acid, methacrylic acid, methyl methacrylate, tert-butyl methacrylate, isobornyl methacrylate, hydroxymethylacrylamide, acrylamide, styrene, and acrylonitrile; The second monomer includes C4-C22 alkyl acrylates, isobutyl acrylate, isooctyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, ethyl methacrylate, isobutyl methacrylate, 2-ethylhexyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, ethylurea methacrylate, dicyclopentene ethoxylate methacrylate, tetrahydrofuran methacrylate, trifluoroethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, and propylene methacrylate. The third monomer includes 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, γ-methacryloyloxypropyltrimethoxysilane, N-hydroxymethylacrylamide, N-butoxymethyl (meth)acrylamide, diacetone acrylamide (DAAM), ethyl acetoacetate methacrylate (AAEM), divinylbenzene, and epoxy resins with an epoxy value of 0.35-0.50; Reactive dispersants: including polyvinyl alcohol and polyethylene glycol.
10. The separator according to claim 1 or 2, characterized in that, The plasticizer is selected from one or more of the following: glycerol C4-C10 alkyl diether or monoether, glycerol C4-C10 carboxylic acid monoester or diester, propylene glycol C4-C10 alkyl monoether, and glycerol.
11. The separator according to claim 1 or 2, characterized in that, The average thickness of the pressure-sensitive coating is 2-20 μm.
12. The separator according to claim 1 or 2, characterized in that, The average thickness of the pressure-sensitive coating is 2-15 μm.
13. The separator according to claim 1 or 2, characterized in that, The average particle size of the first organic particle is 5-20 μm.
14. The separator according to claim 11, characterized in that, The average particle size of the first organic particle is 5-20 μm.
15. The separator according to claim 1 or 2, characterized in that, The first organic particle satisfies at least one of the following: The DSC melting point of the first organic particle is -50℃ to 200℃; The weight-average molecular weight of the first organic particle is 300 × 10⁻⁶. 3 g / mol - 800 × 10 3 g / mol.
16. The separator according to claim 1 or 2, characterized in that, The DSC melting point of the first organic particle is -40℃ to 160℃; The weight-average molecular weight of the first organic particle is 400 × 10⁻⁶. 3 g / mol - 650 × 10 3 g / mol.
17. The separator according to claim 1 or 2, characterized in that, The first organic particle satisfies at least one of the following: The first organic particle is selected from at least one of the following: homopolymers or copolymers of fluorinated alkenyl monomer units, homopolymers or copolymers of olefinic monomer units, homopolymers or copolymers of unsaturated nitrile monomer units, homopolymers or copolymers of epoxide monomer units, dimers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers. The first organic particle is selected from at least one of the following: polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyethylene-co-vinyl acetate, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose; The first organic particle is selected from at least one of the following: polyvinylidene fluoride-co-hexafluoropropylene, polystyrene-co-butyl acrylate, perfluorinated polyvinyl chloride, polyvinylidene fluoride, and polyvinylidene fluoride-co-trichloroethylene.
18. The separator according to claim 1 or 2, characterized in that, The mass ratio of the first organic particle to the second organic particle is (1-4):
1.
19. The separator according to claim 1 or 2, characterized in that, The mass ratio of the first organic particle to the second organic particle is (1.5-2.5):
1.
20. The separator according to claim 1 or 2, characterized in that, The average particle size of the second organic particle is 2-8 μm.
21. The separator according to claim 20, characterized in that, The average thickness of the pressure-sensitive coating is 2-20 μm.
22. The separator according to claim 1 or 2, characterized in that, The second organic particle satisfies at least one of the following: The DSC melting point of the second organic particle is -30 to 100°C; The weight-average molecular weight of the second organic particle is 10 × 10⁻⁶. 3 g / mol-100×10 3 g / mol.
23. The separator according to claim 1 or 2, characterized in that, The second organic particle satisfies at least one of the following: The DSC melting point of the second organic particle is -30 to 70°C; The weight-average molecular weight of the second organic particle is 20 × 10⁻⁶. 3 g / mol - 80 × 10 3 g / mol.
24. The separator according to claim 1 or 2, characterized in that, The second organic particle satisfies at least one of the following: The second organic particle is selected from at least one of the following: homopolymers or copolymers of acrylate monomer units, homopolymers or copolymers of acrylic monomer units, homopolymers or copolymers of unsaturated nitrile monomer units, homopolymers or copolymers of olefin monomer units, homopolymers or copolymers of styrene monomer units, homopolymers or copolymers of epoxy monomer units, polyurethane compounds, rubber compounds, dimers, homopolymers or copolymers of monosaccharide monomer units, and modified compounds of the above homopolymers or copolymers; The second organic particle is selected from at least one of the following: polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polystyrene-co-methyl methacrylate, polystyrene-co-butyl acrylate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer, styrene-butyl acrylate-isooctyl acrylate copolymer, and polyimide.
25. The separator according to claim 1 or 2, characterized in that, The porosity of the isolation membrane substrate is 10-95%, the pore size is 20-60 nm, and the thickness is 3-12 μm.
26. The separator according to claim 1 or 2, characterized in that, The thickness of the isolation membrane substrate is 5-9 μm.
27. The separator according to claim 1 or 2, characterized in that, The separator substrate comprises a membrane or nonwoven material selected from one or more of the following: polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymer, polyphenylene sulfide, and polyvinyl naphthalene.
28. The method for preparing the separator membrane according to any one of claims 1-27, characterized in that, Includes the following steps: S1) The first organic particles and dispersant are added to a solvent to form a first polymer solution; S2) Add the pressure-sensitive adhesive polymer to the first polymer solution obtained in step S1) and mix to form a second polymer solution; S3) Optionally, the second organic particles are added to the second polymer solution obtained in step S2), and mixed to form a third polymer solution; and S4) The second polymer solution obtained in step S2) or the third polymer solution obtained in step S3) is coated onto at least one surface of the porous separator substrate, and the separator is obtained after drying. The isolation membrane includes a pressure-sensitive coating formed on at least one surface of the isolation membrane substrate, comprising 40-90 wt% of first organic particles and 10-20 wt% of pressure-sensitive adhesive polymer, and 0-50 wt% of second organic particles; wherein the pressure-sensitive adhesive polymer comprises an adhesive polymer and a plasticizer.
29. A secondary battery, characterized in that, The invention includes a positive electrode, a negative electrode, a separator membrane spaced between the positive and negative electrode, and an electrolyte, wherein the separator membrane is the separator membrane according to any one of claims 1-27 or the separator membrane obtained by the preparation method according to claim 28.
30. An electrical device, characterized in that, Includes the secondary battery as described in claim 29.
Citation Information
Patent Citations
Organic / inorganic composite porous isolating membrane, preparation method thereof and electrochemical device
CN103441230A
Separator for electrochemical device
US20160149185A1