A polytetrafluoroethylene microporous membrane, a method for preparing the same, and an application thereof

By doping nano-titanium dioxide and metal oxide composites into polytetrafluoroethylene (PTFE) microporous membranes, the problems of poor wettability of PTFE membranes and easy loss of quenching agents were solved, thus achieving high performance and long lifespan of proton exchange membranes.

CN117065583BActive Publication Date: 2026-11-20STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311181767.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2026-11-20
Estimated Expiration
2043-09-13

AI Technical Summary

Technical Problem

Existing polytetrafluoroethylene (ePTFE) membranes have poor wettability and the quenching agent is easily lost, resulting in uneven performance and short service life of proton exchange membranes.

Method used

A composite of nano-titanium dioxide and metal oxides is doped into a polytetrafluoroethylene microporous membrane to enhance its hydrophilicity and free radical quenching ability. The composite is prepared by co-precipitation reaction and mixed with polytetrafluoroethylene resin to form a calendered film, which is then stretched and sintered for shaping.

Benefits of technology

It improves the hydrophilicity and wettability of polytetrafluoroethylene microporous membranes, extends the service life of proton exchange membranes, and enhances their performance stability and durability in proton exchange membranes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117065583B_ABST
    Figure CN117065583B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of membrane materials, and particularly relates to a polytetrafluoroethylene microporous membrane, a preparation method and application thereof. The polytetrafluoroethylene microporous membrane disclosed in the embodiment of the application comprises a composite of nanometer titanium dioxide and metal oxide, and the composite of nanometer titanium dioxide and metal oxide is doped in the polytetrafluoroethylene microporous membrane. In the polytetrafluoroethylene microporous membrane, the composite of nanometer titanium dioxide and metal oxide has a certain hydrophilic capacity, and the infiltration between ePTFE and ion exchange resin is enhanced; meanwhile, the metal oxide with a free radical quenching capacity is doped into ePTFE, so that the loss in the use process can be reduced by utilizing the complexity of the porous structure of the ePTFE membrane, and the service life of the proton exchange membrane is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of membrane material technology, specifically relating to a polytetrafluoroethylene microporous membrane, its preparation method, and its application. Background Technology

[0002] With rapid economic development and increasing energy consumption, the development of clean and renewable energy technologies has become a global focus. Hydrogen fuel cells, due to their extremely high energy conversion efficiency and non-toxic byproducts, are of great significance in addressing energy shortages and environmental pollution. As a core component of hydrogen fuel cells, the proton exchange membrane (PEM) needs to possess excellent properties such as high proton conductivity, good gas barrier properties, good chemical and thermal stability, and good mechanical and dimensional stability. Therefore, the stringent requirements for PEMs have become a research hotspot and a major challenge.

[0003] In the early 1960s, Grubb and Niedrach of General Electric in the United States successfully developed polybenzaldehyde sulfonic acid membranes, which were the earliest proton exchange membranes. Later, DuPont developed the Nafion series of products, which have excellent chemical stability and a service life of over 57,000 hours, leading to significant progress in fuel cell technology. Although homogeneous proton exchange membrane materials can largely meet the requirements of fuel cells, they still suffer from poor dimensional stability, high cost, and high fuel permeation. Porous polytetrafluoroethylene (ePTFE) membranes possess excellent chemical stability and good mechanical strength, making them the most commonly used reinforced porous support material. When perfluorinated microporous media are combined with perfluorinated ion exchange resins, the perfluorinated ion exchange resins form proton transport channels in the micropores, maintaining the membrane's proton conductivity while also improving the membrane's mechanical strength and dimensional stability.

[0004] Therefore, combining proton exchange membrane polymers with porous polytetrafluoroethylene (ePTFE) membranes has become an important solution for proton exchange membrane modification. Summary of the Invention

[0005] This invention is based on the inventor's discoveries and understanding of the following facts and problems:

[0006] Because ePTFE is a hydrophobic material and the membrane has small pores and pore sizes, the perfluorinated ion exchange resin exhibits poor wetting of the PTFE membrane, making it impossible to form a proton exchange membrane with uniform performance, good strength, and high proton conductivity. Furthermore, the presence of quenchers effectively protects the proton exchange membrane polymer material from free radical corrosion, thereby extending the membrane's lifespan. Currently, most metal oxides used for free radical quenching are directly incorporated into perfluorinated ion exchange resins. However, since quenchers are mostly inorganic phases, they cannot form strong interactions with the resin and are therefore easily lost during use.

[0007] Therefore, solving the problems of poor wettability of ePTFE membranes and easy loss of quenching agents is crucial for the preparation of high-performance proton exchange membranes.

[0008] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention propose a polytetrafluoroethylene (ePTFE) microporous membrane. The composite of nano-titanium dioxide and metal oxides possesses a certain degree of hydrophilicity, enhancing the wetting between ePTFE and perfluorinated ion exchange resins. Simultaneously, the doping of ePTFE with free radical quenching capabilities with metal oxides utilizes the complexity of the ePTFE membrane's porous structure to reduce losses during use and increase the proton exchange membrane's lifetime.

[0009] The polytetrafluoroethylene microporous membrane of this invention comprises a composite of nano-titanium dioxide and metal oxide, wherein the composite of nano-titanium dioxide and metal oxide is doped into the polytetrafluoroethylene microporous membrane.

[0010] The advantages and technical effects of the polytetrafluoroethylene (PTFE) microporous membrane in this invention are as follows: 1. In this invention, nano-titanium dioxide and metal oxides are doped into the PTFE microporous membrane in the form of a composite. This composite has the characteristics of small size and large specific surface area, resulting in a large interfacial area and interaction with PTFE. It can adhere well to PTFE, reducing the density formed by the vertical stacking of PTFE resin particles, i.e., the tightness and filling effect between PTFE resin particles, and increasing the pore size and porosity of the PTFE microporous membrane; 2. In this invention, the composite has a certain hydrophilicity, which can improve the hydrophilicity of the PTFE microporous membrane. When used to prepare proton exchange membranes, it can enhance the wetting performance between the PTFE microporous membrane and the ion exchange resin; 3. In this invention, the composite has free radical quenching ability. At the same time, since the composite is attached to the PTFE microporous membrane, it is not easily lost and can remain effective for a long time, thereby extending the life of the proton exchange membrane.

[0011] In some embodiments, the molar ratio of nano-titanium dioxide to metal oxide in the composite of nano-titanium dioxide and metal oxide is 1:3 to 1:10.

[0012] In some embodiments, the content of the composite of nano-titanium dioxide and metal oxide in the polytetrafluoroethylene microporous membrane is 0.99 to 9.09 wt%; and / or, the metal oxide includes at least one of cerium oxide, cobalt oxide, nickel oxide, and manganese oxide.

[0013] This invention also provides a method for preparing a polytetrafluoroethylene microporous membrane, comprising the following steps:

[0014] (1) Add the metal oxide precursor to the aqueous solution and the nano titanium dioxide precursor to the ethanol solution. Adjust the pH of the two and mix them. Add a coprecipitant to cause a coprecipitation reaction. Calcine the precipitate to obtain a composite of metal oxide and nano titanium dioxide.

[0015] (2) The composite obtained in step (1) is dispersed in lubricating oil and then mixed evenly with polytetrafluoroethylene resin. After standing and aging, it is pre-pressed to form a preform.

[0016] (3) The preforms obtained in step (2) are subjected to extrusion, calendering and high-temperature degreasing treatment in sequence to obtain calendered film;

[0017] (4) The calendered film obtained in step (3) is subjected to longitudinal stretching, transverse stretching and sintering in sequence to obtain the polytetrafluoroethylene microporous film.

[0018] The advantages and technical effects of the polytetrafluoroethylene (PTFE) microporous membrane preparation method of this invention are as follows: 1. The method of this invention incorporates metal oxides and nano-titanium dioxide into PTFE resin in the form of a composite, giving the resulting PTFE microporous membrane excellent hydrophilicity and long-lasting free radical quenching ability. When used to prepare proton exchange membranes, it can improve the wettability between the PTFE microporous membrane and the ion exchange resin, as well as the service life of the proton exchange membrane; 2. The PTFE microporous membrane prepared by the method of this invention has good comprehensive performance, is suitable for preparing proton exchange membranes, and is simple, efficient, and easy to promote and apply in industrial production.

[0019] In some embodiments, in step (1), the pH is adjusted to 8-10; and / or, the amount of coprecipitant added is such that the pH of the system is adjusted to 10-13; the temperature of the coprecipitation reaction is 60-100°C, and the reaction time is 0.5-1h.

[0020] In some embodiments, in step (1), the metal oxide precursor includes at least one of cerium chloride, cerium nitrate, cerium acetate, cobalt chloride, cobalt nitrate, cobalt acetate, nickel chloride, nickel nitrate, nickel acetate, manganese chloride, manganese nitrate, and manganese acetate; the nano-titanium dioxide precursor includes at least one of tetrabutyl titanate, isopropyl titanate, and ethyl titanate; and the coprecipitant includes at least one of sodium hydroxide, ammonia, and sodium carbonate.

[0021] In some embodiments, in step (2), the amount of lubricating oil used is 18-25 wt% of the polytetrafluoroethylene resin, and the amount of the composite used is 1-10 wt% of the polytetrafluoroethylene resin.

[0022] In some embodiments, in step (2), the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil, and liquid paraffin, and the polytetrafluoroethylene resin has a particle size of 400-500 nm.

[0023] In some embodiments, in step (2), the temperature of the static curing is 30-60°C and the time of static curing is 24-48h; the pressure of the pre-compression treatment is 2-10MPa and the time of pre-compression treatment is 20-40min.

[0024] In some embodiments, in step (3), the extrusion temperature is 30-100°C, the extrusion speed is 10-60 mm / min, the degreasing temperature is 150-200°C, and / or the thickness of the calendered film is 100-300 μm.

[0025] In some embodiments, in step (4), the longitudinal stretching temperature is 180-250°C, and the longitudinal stretching ratio is 6-9 times; the transverse stretching temperature is 120-150°C, and the transverse stretching ratio is 6-10 times; the sintering and shaping temperature is 330-360°C.

[0026] This invention also provides a proton exchange membrane, comprising the above-described polytetrafluoroethylene microporous membrane or the polytetrafluoroethylene microporous membrane prepared by the above-described preparation method. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the structure of the polytetrafluoroethylene microporous membrane prepared in Example 1;

[0028] Figure 2 This is a schematic diagram of the water contact angle of the polytetrafluoroethylene microporous membranes prepared in Examples 1-4 and Comparative Examples 1-2. Detailed Implementation

[0029] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0030] The polytetrafluoroethylene microporous membrane of this invention comprises a composite of nano-titanium dioxide and metal oxide, wherein the composite of nano-titanium dioxide and metal oxide is doped into the polytetrafluoroethylene microporous membrane.

[0031] The polytetrafluoroethylene (PTFE) microporous membrane of this invention incorporates nano-titanium dioxide and metal oxides in the form of a composite. This composite is characterized by its small size and large specific surface area, resulting in a large interfacial area and interaction with PTFE. This allows for excellent adhesion to PTFE, reducing the density of PTFE resin particles in the vertical direction (i.e., the tightness and filling effect between PTFE resin particles), and increasing the pore size and porosity of the PTFE microporous membrane. Furthermore, the composite possesses a certain degree of hydrophilicity, enhancing the hydrophilicity of the PTFE microporous membrane. When used in the preparation of proton exchange membranes, it strengthens the wetting properties between the PTFE microporous membrane and the ion exchange resin. The composite also exhibits free radical quenching ability. Moreover, because the composite is adhered within the PTFE microporous membrane, it is not easily lost and can remain effective for a long time, thereby extending the lifespan of the proton exchange membrane.

[0032] In some embodiments, preferably, the molar ratio of nano-titanium dioxide to metal oxide in the composite of nano-titanium dioxide and metal oxide is 1:3 to 1:10. More preferably, the content of the composite of nano-titanium dioxide and metal oxide in the polytetrafluoroethylene microporous membrane is 0.99 to 9.09 wt%; and / or, the metal oxide includes at least one of cerium oxide, cobalt oxide, nickel oxide, and manganese oxide.

[0033] In this embodiment of the invention, the preferred ratio of nano-titanium dioxide and metal oxide in the composite and the preferred amount of the composite are to ensure that it can better improve the hydrophilicity and free radical quenching performance of the polytetrafluoroethylene microporous membrane. If the amount of the composite is too small, the performance improvement of the polytetrafluoroethylene microporous membrane will be very limited. If the amount of the composite is too large, it will aggregate in the polytetrafluoroethylene microporous membrane, which is not conducive to the improvement of the performance of the polytetrafluoroethylene microporous membrane.

[0034] This invention also provides a method for preparing a polytetrafluoroethylene microporous membrane, comprising the following steps:

[0035] (1) Add the metal oxide precursor to the aqueous solution and the nano titanium dioxide precursor to the ethanol solution. Adjust the pH of the two and mix them. Add a coprecipitant to cause a coprecipitation reaction. Calcine the precipitate to obtain a composite of metal oxide and nano titanium dioxide.

[0036] (2) The composite obtained in step (1) is dispersed in lubricating oil and then mixed evenly with polytetrafluoroethylene resin. After standing and aging, it is pre-pressed to form a preform.

[0037] (3) The preforms obtained in step (2) are subjected to extrusion, calendering and high-temperature degreasing treatment in sequence to obtain calendered film;

[0038] (4) The calendered film obtained in step (3) is subjected to longitudinal stretching, transverse stretching and sintering in sequence to obtain the polytetrafluoroethylene microporous film.

[0039] The method for preparing polytetrafluoroethylene (PTFE) microporous membranes according to embodiments of the present invention involves doping PTFE resin with metal oxides and nano-titanium dioxide in the form of a composite. This results in PTFE microporous membranes with excellent hydrophilicity and long-lasting free radical quenching ability. When used to prepare proton exchange membranes, this method improves the wettability between the PTFE microporous membrane and the ion exchange resin, as well as the service life of the proton exchange membrane. The PTFE microporous membranes prepared by this method have good comprehensive performance, are suitable for the preparation of proton exchange membranes, and are simple, efficient, and easy to promote and apply in industrial production.

[0040] In some embodiments, preferably, in step (1), the pH is adjusted to 8-10; and / or, the amount of coprecipitant added is such that the pH of the system is adjusted to 10-13; the temperature of the coprecipitation reaction is 60-100°C, and the reaction time is 0.5-1 h. More preferably, in step (1), the metal oxide precursor includes at least one of cerium chloride, cerium nitrate, cerium acetate, cobalt chloride, cobalt nitrate, cobalt acetate, nickel chloride, nickel nitrate, nickel acetate, manganese chloride, manganese nitrate, and manganese acetate; the nano-titanium dioxide precursor includes at least one of tetrabutyl titanate, isopropyl titanate, and ethyl titanate; and the coprecipitant includes at least one of sodium hydroxide, ammonia, and sodium carbonate.

[0041] In this embodiment of the invention, the conditions for the coprecipitation reaction are preferred, which enable the coprecipitation reaction to proceed rapidly and fully without the formation of by-products. If the reaction temperature of the coprecipitant is too low or the pH value is too high, the solubility of the reactants decreases, the precipitation rate slows down, and the formation of precipitate may also be insufficient. If the reaction temperature of the coprecipitation reaction is too high or the pH value is too low, the solubility of the reactants increases, the reaction rate is accelerated, but this may also lead to problems such as excessive formation of precipitate, uneven particle size distribution, and the formation of by-products.

[0042] In some embodiments, preferably, in step (1), the calcination temperature is 400–600°C, and the calcination time is 2–5 hours. More preferably, before the calcination, the obtained precipitate is washed and dried sequentially.

[0043] In some embodiments, preferably, in step (2), the amount of lubricating oil is 18-25 wt% of the polytetrafluoroethylene resin, and the amount of the composite is 1-10 wt% of the polytetrafluoroethylene resin. More preferably, in step (2), the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil, and liquid paraffin, and the polytetrafluoroethylene resin has a particle size of 400-500 nm. More preferably, the composite is dispersed in the lubricating oil and then subjected to ultrasonic treatment at a frequency of 50-100 Hz for a duration of 0.5-1 h.

[0044] In this embodiment of the invention, the amount of lubricating oil is optimized and ultrasonic treatment is performed to enable the composite to be uniformly dispersed in the lubricating oil, while the lubricating oil can be uniformly filled in the polytetrafluoroethylene resin, reducing the fibrillation of the resin in the early stage.

[0045] In some embodiments, preferably, in step (2), the temperature of the static curing is 30–60°C, and the static curing time is 24–48 h; the pressure of the pre-compression treatment is 2–10 MPa, and the pre-compression treatment time is 20–40 min. More preferably, in step (2), the pre-compression treatment is completed in a preforming device.

[0046] In some embodiments, preferably, in step (3), the extrusion temperature is 30-100°C, the extrusion speed is 10-60 mm / min, the degreasing temperature is 150-200°C; and / or, the thickness of the calendered film is 100-300 μm.

[0047] In some embodiments, preferably, in step (4), the longitudinal stretching temperature is 180-250°C and the longitudinal stretching ratio is 6-9 times; the transverse stretching temperature is 120-150°C and the transverse stretching ratio is 6-10 times; the sintering and shaping temperature is 330-360°C.

[0048] This invention also provides a proton exchange membrane, comprising the above-described polytetrafluoroethylene microporous membrane or the polytetrafluoroethylene microporous membrane prepared by the above-described preparation method.

[0049] Example 1

[0050] (1) 1.5 mol of nickel chloride was added to an aqueous solution, and 0.5 mol of tetrabutyl titanate was added to an ethanol solution. The pH of the solution was adjusted to 9 and the temperature was 80℃. The two were thoroughly mixed under stirring. 0.5 mol / L sodium hydroxide solution was added to adjust the pH to 13 and the reaction was continued for 1 h. The precipitate was washed three times with deionized water and dried in a 100℃ oven for 2 h. Then it was transferred to a muffle furnace and calcined at 500℃ for 3 h to obtain a composite of nickel oxide and nano titanium dioxide.

[0051] (2) Add 2wt% of the composite (relative to PTFE resin content) to 25wt% of isoparaffinic lubricating oil (relative to PTFE resin content), treat it with an ultrasonic processor at 100Hz for 1h, add the mixture of composite and lubricating oil to PTFE resin powder and mix evenly, let it stand and mature at 60℃ for 24h to form a paste, and pre-press the matured PTFE paste through a pre-forming device to form a preform. The pre-forming pressure is 10MPa and the pre-forming time is 30min.

[0052] (3) The preform is extruded at 60℃ and 10mm / min to obtain rod-shaped material, and then the rod-shaped material is calendered into a thin sheet by a calender. After degreasing and removing the lubricating oil at 200℃, a calendered film with a thickness of 200μm is obtained.

[0053] (4) The calendered film is fed into the stretching unit and stretched longitudinally by 6 times at 230°C, and then stretched transversely by 9 times at 150°C. Finally, it is sintered and shaped at 340°C to obtain a polytetrafluoroethylene microporous membrane.

[0054] A schematic diagram of the structure of the polytetrafluoroethylene microporous membrane prepared in this embodiment is shown below. Figure 1 As shown, the composite of metal oxide and nano-titanium dioxide is uniformly dispersed in a polytetrafluoroethylene microporous membrane.

[0055] Example 2

[0056] (1) Add 1.5 mol of nickel nitrate to an aqueous solution and 0.5 mol of isopropyl titanate to an ethanol solution. Adjust the pH of the solution to 9 and the temperature to 80℃. Mix the two thoroughly under stirring. Add 0.5 mol / L sodium hydroxide solution to adjust the pH to 13 and continue the reaction for 1 h. Wash the precipitate three times with deionized water and dry it in a 100℃ oven for 2 h. Then transfer it to a muffle furnace and calcine it at 500℃ for 3 h to obtain a composite of nickel oxide and nano titanium dioxide.

[0057] (2) Add 5 wt% of the composite (relative to PTFE resin content) to 25 wt% of isoparaffinic lubricating oil (relative to PTFE resin content), treat it with an ultrasonic processor at 100 Hz for 1 h, add the mixture of composite and lubricating oil to PTFE resin powder and mix evenly, let it stand and mature at 60 ℃ for 24 h to form a paste, and pre-press the matured PTFE paste through a pre-forming device to form a preform. The pre-forming pressure is 10 MPa and the pre-forming time is 30 min.

[0058] (3) The preform is extruded at 60℃ and 10mm / min to obtain rod-shaped material, and then the rod-shaped material is calendered into a thin sheet by a calender. After degreasing and removing the lubricating oil at 200℃, a calendered film with a thickness of 200μm is obtained.

[0059] (4) The calendered film is fed into the stretching unit and stretched longitudinally by 6 times at 230°C, and then stretched transversely by 9 times at 150°C. Finally, it is sintered and shaped at 340°C to obtain a polytetrafluoroethylene microporous membrane.

[0060] Example 3

[0061] (1) Add 1.5 mol nickel acetate to an aqueous solution and 0.5 mol ethyl titanate to an ethanol solution. Adjust the pH of the solution to 9 and the temperature to 80℃. Mix the two thoroughly under stirring. Add 0.5 mol / L sodium hydroxide solution to adjust the pH to 13 and continue the reaction for 1 h. Wash the precipitate three times with deionized water and dry it in a 100℃ oven for 2 h. Then transfer it to a muffle furnace and calcine it at 500℃ for 3 h to obtain a composite of nickel oxide and nano titanium dioxide.

[0062] (2) Add 8 wt% of the composite (relative to PTFE resin content) to 25 wt% of isoparaffinic lubricating oil (relative to PTFE resin content), treat it with an ultrasonic processor at 100 Hz for 1 h, add the mixture of composite and lubricating oil to PTFE resin powder and mix evenly, let it stand and mature at 60 ℃ for 24 h to form a paste, and pre-press the matured PTFE paste through a pre-forming device to form a preform. The pre-forming pressure is 10 MPa and the pre-forming time is 30 min.

[0063] (3) The preform is extruded at 60℃ and 10mm / min to obtain rod-shaped material, and then the rod-shaped material is calendered into a thin sheet by a calender. After degreasing and removing the lubricating oil at 200℃, a calendered film with a thickness of 200μm is obtained.

[0064] (4) The calendered film is fed into the stretching unit and stretched longitudinally by 6 times at 230°C, and then stretched transversely by 9 times at 150°C. Finally, it is sintered and shaped at 340°C to obtain a polytetrafluoroethylene microporous membrane.

[0065] Example 4

[0066] (1) Add 1.5 mol of nickel chloride to an aqueous solution and 0.5 mol of isopropyl titanate to an ethanol solution. Adjust the pH of the solution to 9 and the temperature to 80℃. Mix the two thoroughly under stirring. Add 0.5 mol / L sodium hydroxide solution to adjust the pH to 13 and continue the reaction for 1 h. Wash the precipitate three times with deionized water and dry it in a 100℃ oven for 2 h. Then transfer it to a muffle furnace and calcine it at 500℃ for 3 h to obtain a composite of nickel oxide and nano titanium dioxide.

[0067] (2) Add 5 wt% of the composite (relative to PTFE resin content) to 25 wt% of isoparaffinic lubricating oil (relative to PTFE resin content), treat it with an ultrasonic processor at 100 Hz for 1 h, add the mixture of composite and lubricating oil to PTFE resin powder and mix evenly, let it stand and mature at 60 ℃ for 24 h to form a paste, and pre-press the matured PTFE paste through a pre-forming device to form a preform. The pre-forming pressure is 10 MPa and the pre-forming time is 30 min.

[0068] (3) The preform is extruded at 60℃ and 10mm / min to obtain rod-shaped material, and then the rod-shaped material is calendered into a thin sheet by a calender. After degreasing and removing the lubricating oil at 200℃, a calendered film with a thickness of 200μm is obtained.

[0069] (4) The calendered film is fed into the stretching unit and stretched longitudinally by 8 times at 230°C, and then stretched transversely by 10 times at 150°C. Finally, it is sintered and shaped at 340°C to obtain a polytetrafluoroethylene microporous membrane.

[0070] Comparative Example 1

[0071] The preparation method of this comparative example is the same as that of Example 1, except that the amount of nickel oxide and nano titanium dioxide composite added is 0%.

[0072] Comparative Example 2

[0073] The preparation method of this comparative example is the same as that of Example 1, except that step (1) is omitted, and nickel oxide and nano titanium dioxide are simply mixed and added to the isoparaffinic lubricating oil.

[0074] Performance testing

[0075] (1) The thickness, porosity, average pore size and tensile strength of the polytetrafluoroethylene microporous membranes prepared in Examples 1-4 and Comparative Examples 1-2 were tested, and the results are shown in Table 1:

[0076] Table 1. Thickness, porosity, average pore size, and tensile strength of polytetrafluoroethylene microporous membranes

[0077] Test Project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Thickness (μm) 12.7 12.1 12.9 11.5 12.5 12.5 Average pore size (nm) 201 242 271 237 170 181 Porosity (%) 65 69 75 70 59 61 Tensile strength (MPa) 50 54 62 61 45 46

[0078] Note: The tensile strength test equipment is a universal testing machine. The sample is cut along the TD and MD directions using a punch press. The sample width is 6 mm, the tensile rate is 50 mm / min, and the tensile strength is calculated according to GB / T13022-1991.

[0079] As can be seen from the data in Table 1, the polytetrafluoroethylene microporous membrane prepared in Comparative Example 1 has a lower average pore size and porosity compared to Example 1 because it does not contain nano-titanium dioxide and metal oxides. Compared to Example 1, the polytetrafluoroethylene microporous membrane prepared in Comparative Example 2 only involves a simple mixing of nickel oxide and nano-titanium dioxide. The specific surface area of ​​these two substances is much smaller than that of the composite. Therefore, they cannot effectively reduce the compactness and filling effect between PTFE resin particles in PTFE resin, and the improvement effect on the polytetrafluoroethylene microporous membrane is not as good as that of Example 1.

[0080] (2) The hydrophilicity of the polytetrafluoroethylene microporous membranes prepared in Examples 1-4 and Comparative Examples 1-2 was tested, and the results are as follows: Figure 2 As shown:

[0081] The polytetrafluoroethylene (PTFE) microporous membranes prepared in Examples 1-4 had contact angles with water ranging from 80° to 120°, exhibiting relatively good hydrophilicity. The PTFE microporous membrane prepared in Comparative Example 1, compared to Example 1, lacked the addition of nano-titanium dioxide and metal oxides, resulting in a contact angle of 146° with water and poor hydrophilicity. This makes it unfavorable for wetting with resins when used in the preparation of proton exchange membranes. The PTFE microporous membrane prepared in Comparative Example 2 showed decreased hydrophilicity compared to Example 1. This is because the simple mixing of nickel oxide and nano-titanium dioxide easily leads to agglomeration, significantly reducing its hydrophilic effect and consequently lowering the hydrophilicity of the microporous membrane.

[0082] (3) Proton exchange membranes were prepared using the polytetrafluoroethylene microporous membranes obtained in Examples 1-4 and Comparative Examples 1-2, and the conductivity of the proton exchange membranes was tested. The results are shown in Table 2.

[0083] The preparation method of the proton exchange membrane is as follows: First, a layer of perfluorosulfonic acid resin solution with a wet thickness of 120 μm is coated on a coating machine. Then, the prepared polytetrafluoroethylene microporous membrane is cut and covered on the perfluorosulfonic acid resin solution. After waiting for 2 minutes, another layer of perfluorosulfonic acid resin solution with a wet thickness of 80 μm is coated. After waiting for 2 minutes, the wet membrane is placed in an oven at 160℃ and dried for 10 minutes to obtain the proton exchange membrane.

[0084] The conductivity test method is as follows: the proton exchange membrane is cut into 10cm×10cm samples and placed in a constant temperature and humidity chamber. The constant temperature and humidity test is carried out at 80℃ and RH80% for 4h, 8h and 12h respectively.

[0085] Table 2. Conductivity (S / cm) of proton exchange membranes after different hygrothermal treatments

[0086] Processing time (h) Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 0 0.121 0.125 0.131 0.119 0.103 0.113 4 0.113 0.120 0.128 0.107 0.087 0.102 8 0.095 0.109 0.117 0.095 0.073 0.089 12 0.083 0.093 0.107 0.089 0.065 0.074

[0087] As can be seen from the data in Table 2, the proton exchange membranes prepared using the polytetrafluoroethylene (PTFE) microporous membranes of Examples 1-4 have relatively high conductivity. After 12 hours of treatment, the conductivity retention rates of the proton exchange membranes prepared using the PTFE microporous membranes of Examples 1-4 are 68.6%, 74.4%, 81.7%, and 74.8%, respectively, indicating good durability. The proton exchange membrane prepared using the PTFE microporous membrane of Comparative Example 1, due to the absence of the composite of metal oxide and nano-titanium dioxide, has a conductivity retention rate of only 63.1% after 12 hours of treatment, indicating poor durability. Compared to Example 1, the proton exchange membrane prepared using the PTFE microporous membrane of Comparative Example 2 only undergoes a simple mixing treatment of metal oxide and nano-titanium dioxide. During use, the metal oxide is easily depleted, resulting in a conductivity retention rate of only 65.5% after 12 hours of treatment, also indicating poor durability.

[0088] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0089] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.

Claims

1. A polytetrafluoroethylene microporous membrane, characterized in that, A composite comprising nano-titanium dioxide and metal oxide, wherein the composite of nano-titanium dioxide and metal oxide is doped in a polytetrafluoroethylene microporous membrane; The method for preparing the polytetrafluoroethylene microporous membrane includes the following steps: (1) The metal oxide precursor is added to an aqueous solution, and the nano-titanium dioxide precursor is added to an ethanol solution. The pH of the two is adjusted and they are mixed. A coprecipitant is added to cause a coprecipitation reaction. The precipitate is calcined to obtain a composite of metal oxide and nano-titanium dioxide. The metal oxide precursor includes at least one of cerium chloride, cerium nitrate, cerium acetate, cobalt chloride, cobalt nitrate, cobalt acetate, nickel chloride, nickel nitrate, nickel acetate, manganese chloride, manganese nitrate, and manganese acetate. The nano-titanium dioxide precursor includes at least one of tetrabutyl titanate, isopropyl titanate, and ethyl titanate. The coprecipitant includes at least one of sodium hydroxide, ammonia, and sodium carbonate. (2) The composite obtained in step (1) is dispersed in lubricating oil and then mixed evenly with polytetrafluoroethylene resin. After standing and aging, it is pre-pressed to form a preform. (3) The preforms obtained in step (2) are subjected to extrusion, calendering and degreasing processes in sequence to obtain a calendered film; (4) The calendered film obtained in step (3) is subjected to longitudinal stretching, transverse stretching and sintering in sequence to obtain the polytetrafluoroethylene microporous film.

2. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, The molar ratio of nano-titanium dioxide to metal oxide in the composite of nano-titanium dioxide and metal oxide is 1:3 to 1:

10.

3. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (1), the pH is adjusted to 8-10; and / or the amount of coprecipitant added is such that the pH of the system is adjusted to 10-13; the temperature of the coprecipitation reaction is 60-100℃ and the reaction time is 0.5-1h.

4. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (2), the amount of lubricating oil is 18-25 wt% of the polytetrafluoroethylene resin, and the amount of the composite is 1-10 wt% of the polytetrafluoroethylene resin.

5. The polytetrafluoroethylene microporous membrane according to claim 1 or 4, characterized in that, In step (2), the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil, and liquid paraffin, and the polytetrafluoroethylene resin has a particle size of 400~500nm.

6. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (2), the temperature of static curing is 30~60 ℃ and the time of static curing is 24~48h; the pressure of pre-compression treatment is 2~10MPa and the time of pre-compression treatment is 20~40min.

7. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (3), the extrusion temperature is 30~100℃, the extrusion speed is 10~60 mm / min, the degreasing temperature is 150~200℃; and / or, the thickness of the calendered film is 100~300μm.

8. The polytetrafluoroethylene microporous membrane according to claim 1, characterized in that, In step (4), the longitudinal stretching temperature is 180~250℃ and the longitudinal stretching ratio is 6~9 times; the transverse stretching temperature is 120~150℃ and the transverse stretching ratio is 6~10 times; the sintering and shaping temperature is 330~360℃.

9. A proton exchange membrane, characterized in that, Includes the polytetrafluoroethylene microporous membrane according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Positive electrode material of lithium ion battery and preparation method thereof

    CN103050684A

  • Anti-ultraviolet barrier film and preparation method thereof

    CN108582904A