A screening method for key factors affecting ionic conductivity in oxide solid electrolyte synthesis
By using orthogonal experimental design to screen key factors in the synthesis of solid electrolytes, the uncertainty of factor screening in the synthesis process was resolved, the repeatability of experimental results and production efficiency were improved, and the cost was reduced.
Patent Information
- Application Number
- CN202311018808.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-14
AI Technical Summary
In the process of synthesizing solid electrolytes, existing technologies make it difficult to accurately screen the key factors affecting ionic conductivity, resulting in poor reproducibility of experimental results, high costs, and low efficiency.
Orthogonal experimental design was adopted. Key factors were identified through literature review, multiple orthogonal arrays were designed, ionic conductivity experiments were conducted, the contribution and range of each factor were calculated, the optimal combination and important factors were determined, and the parameters with the greatest influence were screened out.
This method enables the accurate screening of key factors affecting ionic conductivity in a small number of experimental samples, improving experimental repeatability and production efficiency while reducing R&D costs.
Smart Images

Figure CN117074474B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes. Background Technology
[0002] Since their introduction to the market, lithium-ion batteries have been widely used in various electronic devices, weaponry, aerospace systems, and electric vehicles, serving as an advanced energy storage device capable of highly efficient chemical-to-electrical energy conversion. However, due to the limitations of traditional liquid lithium batteries, they are difficult to adapt to high-voltage cathode materials and low-potential, high-theoretical-capacity lithium metal anodes, thus failing to meet the ever-increasing energy density demands of today's society for advanced energy storage and electrical applications. Furthermore, during charging and discharging, uneven lithium-ion deposition can easily lead to the formation of lithium dendrites, which can impact the liquid electrolyte membrane, causing short circuits and creating a series of safety hazards. The leakage of organic electrolytes and their flammability, explosiveness, and corrosiveness are also problems that urgently need to be addressed in the future development and application of lithium batteries. Compared to liquid lithium-ion batteries, solid-state lithium-ion batteries possess superior mechanical properties, stronger oxidation-reduction resistance, and higher electrochemical stability and safety. Solid electrolytes have received increasing research and attention in recent years, especially in fields requiring high-safety energy storage facilities such as aviation, aerospace, and electric vehicles. This is because they can replace the flammable liquid electrolyte in lithium-ion batteries, significantly improving battery safety.
[0003] However, the synthesis of solid electrolytes involves many steps, and the parameters selected in each step can significantly affect the ionic conductivity of the final synthesized solid electrolyte sheet. Although literature review can provide a general understanding of the mechanisms by which various parameters affect ionic conductivity, in actual production, due to differences in experimental equipment and materials, the results obtained from the literature are difficult to reproduce with good accuracy. However, if the optimal ratio can be selected and the most important influencing parameter among all factors can be identified (the correct selection of this parameter has the greatest impact on the final ionic conductivity), not only can the experimental scheme be determined quickly, but the number of experiments to synthesize similar materials can also be effectively reduced, the experimental time shortened, and industrial costs reduced. Summary of the Invention
[0004] In view of the above-mentioned technical problems in the prior art, the purpose of this invention is to provide a method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes.
[0005] The technical solution adopted in this invention is as follows:
[0006] A method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes includes the following steps:
[0007] 1) Through literature review, some important factors affecting ionic conductivity in the synthesis of solid electrolytes were preliminarily determined. These important factors include the raw materials for synthesizing solid electrolytes, the molar ratio of each non-oxygen element in the solid electrolyte is determined according to the chemical formula of the solid electrolyte, and a series of raw material samples composed of different forms of components containing non-oxygen elements are set up.
[0008] 2) Determine the appropriate orthogonal array type. To avoid randomness, the series of raw material samples set in step 1) are distributed, arranged, and combined, and multiple orthogonal arrays are established using the important factor parameters determined in step 1). There is at least one different raw material sample between each pair of orthogonal arrays.
[0009] 3) Experimental results of ionic conductivity under each group of conditions in multiple orthogonal arrays were obtained through experiments;
[0010] 4) Based on the experimental results in the orthogonal array, calculate the contribution factor K of each level value of each factor parameter to the ionic conductivity, and calculate the average value corresponding to each factor parameter. The value is calculated separately for each factor. The range R is used to obtain the optimal combination of factors and parameters in the synthesis of solid electrolytes, as well as the most important influencing factors in the synthesis process.
[0011] Furthermore, in step 4), the parameter with the highest contribution for each factor is selected. By combining the value levels, we can obtain the level combination value with the highest ionic conductivity, which is the optimal level combination of the factor parameters.
[0012] Further, in step 4), the magnitude of the change in ionic conductivity caused by the change in the level of each factor is obtained based on the value of R. The larger the value of R, the greater the influence of the corresponding factor on the ionic conductivity, and thus the importance of each factor can be obtained.
[0013] Furthermore, step 4) also includes the following analysis steps for the results of the orthogonal array: comparing the raw material sample parameters involved in the optimal combination of factor parameters obtained from multiple orthogonal arrays, and taking the raw material sample with the highest frequency of occurrence in the optimal combination as the optimal raw material sample parameter for synthesizing solid electrolyte.
[0014] Furthermore, the main influencing factors mentioned in step 1) include raw material samples, synthesis temperature, and sintering temperature.
[0015] Furthermore, the raw material samples contain components of Ti source, Li source, Al source and P source, and the molar ratio of the four non-oxygen elements Ti, Li, Al and P is the same in different raw material samples.
[0016] Furthermore, the synthesis process of solid electrolytes includes the following steps:
[0017] S1: All raw material samples were weighed according to the proportions of each component, C1-C4 alcohol solvent was added, and the mixture was ball-milled and mixed evenly.
[0018] S2: Place the ball-milled and mixed raw materials into a drying oven to dry and remove excess moisture;
[0019] S3: The dried material is placed in a muffle furnace for calcination. The synthesis temperature of the calcination is set to carry out the reaction. The synthesis time is the same at different synthesis temperatures so that the reaction can be fully achieved at this synthesis time to obtain the raw powder precursor.
[0020] S4: The raw powder precursor is ball-milled, dried, and then cold-pressed into blocks. It is then sintered at a set sintering temperature. The sintering time is the same at different sintering temperatures, so that full sintering can be achieved at this sintering time, thus synthesizing a solid electrolyte.
[0021] The beneficial effects achieved by this invention are:
[0022] (1) This invention utilizes the concept of traditional orthogonal experiments, requiring only a small number of experimental samples to more accurately screen key factors affecting ionic conductivity in the solid-phase synthesis of solid electrolyte sheets.
[0023] (2) In the embodiments of the present invention, all five randomly selected orthogonal arrays have a high degree of consistency in the selection of optimal parameters and the determination of the most important factors, indicating that the method is highly reliable.
[0024] (3) The method of the present invention can be used to efficiently screen key factors affecting ionic conductivity in the synthesis of solid electrolytes, determine the optimal combination of factor parameters, identify the most important influencing factors, greatly reduce R&D costs and improve production efficiency. Detailed Implementation
[0025] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0026] Example 1:
[0027] The invention relates to a solid-state method for synthesizing NASICON (sodium fast ion conduction) Li. 1.3 Al 0.3 Ti 1.7 The method of the present invention will be described in detail using (PO4)3(LATP) as an example.
[0028] 1. Literature review reveals that several parameters potentially affecting the ionic conductivity of NASICON (sodium fast ionic conductor) LATP via solid-state synthesis are: raw materials, synthesis temperature, and sintering temperature. Therefore, common raw materials used in solid-state reactions were selected (see Table 1); synthesis temperatures were 700℃, 800℃, 900℃, and 1000℃, corresponding to levels 1, 2, 3, and 4 respectively; sintering temperatures were 750℃, 850℃, 950℃, and 1050℃, also corresponding to levels 1, 2, 3, and 4 respectively. Thus, the level number for the raw materials was determined to be 5, the level number for the synthesis temperature to be 4, and the level number for the sintering temperature to be 4.
[0029] Table 1 Common combinations of raw materials and their corresponding serial numbers
[0030]
[0031] The molecular formula of the oxide solid electrolyte prepared according to the different combinations of raw materials in Table 1 is Li. 1.3 Al 0.3 Ti 1.7 (PO4)3, the molar ratio of Ti, Li, Al and P in different raw materials is 1.7:1.3:0.3:3.
[0032] The experiment for synthesizing oxide solid electrolytes under different influencing factors includes the following steps:
[0033] 1. After weighing all the raw materials according to the measured amount, add an equal mass of isopropanol and put them into a ball mill to mix evenly.
[0034] Ball milling conditions: ball-to-material ratio of 5:1; rotation speed of 500 rpm; alternating forward and reverse rotation mode: 10 min forward rotation, 10 min reverse rotation, and 10 min interval in between; total ball milling time of 30 h.
[0035] 2. Place the mixed raw materials in a drying oven at 60℃ for 12 hours to remove excess moisture.
[0036] 3. The dried material is placed in a muffle furnace for calcination. The calcination synthesis time is fixed at 10 hours, and the calcination synthesis temperature is set at 700℃, 800℃, 900℃, and 1000℃ respectively to form LATP raw powder.
[0037] 4. The calcined material is then ball-milled and dried to obtain LATP powder (the ball-milling and drying steps are the same as steps 1 and 2).
[0038] 5. LATP powder was cold-pressed into blocks under a pressure of 400 MPa, and then sintered. The sintering time was fixed at 10 hours, and the sintering temperatures were set at 750℃, 850℃, 950℃, and 1050℃, respectively.
[0039] 6. Obtain LATP electrolyte tablets.
[0040] 2. Due to the inconsistent number of levels among the three factors, a mixed orthogonal array needs to be designed for calculation. However, since this invention requires the design of multiple different orthogonal arrays to demonstrate the reliability of orthogonal method-based optimization screening of parameters for synthesizing solid electrolytes, the number of levels for the raw materials is still determined to be 4, except that the selection of these 4 levels is randomly assigned across multiple orthogonal arrays. The specific allocation is shown in Table 2. The scheme presented in this invention proposes to design 5 orthogonal arrays to jointly screen the key factors affecting ionic conductivity in LATP solid-phase synthesis.
[0041] Table 2
[0042]
[0043] 3. Design orthogonal arrays and conduct corresponding experiments. Analyze the experimental results of ionic conductivity for each group and perform calculations and analyses on the orthogonal arrays. The orthogonal array designs are shown in Tables 3, 4, 5, 6, and 7, corresponding to orthogonal arrays 1, 2, 3, 4, and 5, respectively. In the orthogonal arrays, K1, K2, K3, and K4 represent the contributions of the four levels (1, 2, 3, and 4) of the corresponding factors to the ionic conductivity; while... These represent the average contribution values. Combining the factors with the highest contribution levels yields the optimal combination for the highest ionic conductivity. The range R is used to determine the magnitude of the change in ionic conductivity caused by the change in the level of each factor. The larger the value of R, the greater the influence of the corresponding factor on the ionic conductivity, and the more important it is to pay attention to and focus on in industrial production.
[0044] 4. Analyze the results of the orthogonal array. From the factors corresponding to... The highest combined values of ionic conductivity can be obtained by using orthogonal tables (highlighted in bold and underlined). Combined with Table 2, it can be seen that, except for orthogonal table 2, the optimal ratios for orthogonal tables 1, 3, 4, and 5 all yield the highest ionic conductivity with LATP-T as the raw material, a synthesis temperature of 900℃, and a sintering temperature of 950℃. However, the optimal ratios for orthogonal table 2 all yield the highest ionic conductivity with LATP-CK as the raw material, a synthesis temperature of 900℃, and a sintering temperature of 950℃. The only difference in the results is the choice of raw material. This difference arises because orthogonal table 2 does not consider LATP-T. Therefore, it can still be considered that the optimal parameters for the solid-state synthesis of NASICON (sodium fast ionic conductor) LATP are LATP-T, a synthesis temperature of 900℃, and a sintering temperature of 950℃, and the results of all orthogonal tables are consistent. Furthermore, comparing the range R values of each factor in each orthogonal table (the maximum value is highlighted in yellow), it can be found that the results of each orthogonal table are also consistent, with the sintering temperature being the most influential factor. In summary, all five randomly selected orthogonal arrays reached highly consistent conclusions regarding the selection of optimal parameters and the determination of the most important factors, indicating that the method is highly reliable.
[0045] Table 3
[0046]
[0047] Table 4
[0048]
[0049] Table 5
[0050]
[0051]
[0052] Table 6
[0053]
[0054]
[0055] Table 7
[0056]
[0057] The unit of ionic conductivity in Tables 3-7 is mS / cm.
[0058] This invention focuses specifically on the solid-state synthesis of NASICON (sodium fast ion conductor) LATP, but other synthesis methods include hydrothermal synthesis and glass melting. The synthesized solid electrolyte materials include perovskite, LISICON, and garnet types. The method of this invention allows for efficient screening of key factors affecting ionic conductivity in solid electrolyte synthesis, determination of optimal ratios, and identification of the most significant influencing factors, thereby greatly reducing R&D costs and improving production efficiency.
Claims
1. A method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes, characterized in that... Includes the following steps: 1) Through literature review, some important factors affecting ionic conductivity in the synthesis of solid electrolytes were preliminarily determined. These important factors include the raw materials for synthesizing solid electrolytes, the molar ratio of each non-oxygen element in the solid electrolyte is determined according to the chemical formula of the solid electrolyte, and a series of raw material samples composed of different forms of components containing non-oxygen elements are set up. 2) Determine the appropriate orthogonal array type. To avoid randomness, the series of raw material samples set in step 1) are distributed, arranged, and combined, and multiple orthogonal arrays are established using the important factor parameters determined in step 1). There is at least one different raw material sample between each pair of orthogonal arrays. 3) Experimental results of ionic conductivity under each group of conditions in multiple orthogonal arrays were obtained through experiments; 4) Based on the experimental results in the orthogonal array, calculate the contribution factor K of each important factor parameter's level value to the ionic conductivity, and calculate the average value corresponding to each important factor parameter. The values are then calculated separately for each important factor parameter. The range R is used to obtain the optimal combination of important parameters in the synthesis of solid electrolytes and the most important influencing factors in the synthesis process.
2. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 1, characterized in that... In step 4), select the parameter with the highest contribution for each important factor. By combining the value levels, we can obtain the optimal combination of the levels that yields the highest ionic conductivity, which is the optimal combination of the important factor parameters.
3. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 1, characterized in that... In step 4), the magnitude of the change in ionic conductivity caused by the change in the level of each important factor parameter is obtained based on the value of R. The larger the value of R, the greater the influence of the corresponding important factor parameter on the ionic conductivity, and thus the importance of each important factor parameter can be obtained.
4. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 1, characterized in that... Step 4) also includes the following analysis steps for the results of the orthogonal array: comparing the raw material sample parameters involved in the optimal combination of important factor parameters obtained from multiple orthogonal arrays, and taking the raw material sample with the highest frequency in the optimal combination as the optimal raw material sample parameter for synthesizing solid electrolyte.
5. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 1, characterized in that... Step 1) The key parameters include raw material sample, synthesis temperature and sintering temperature.
6. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 1, characterized in that... The raw material samples contain components of Ti source, Li source, Al source and P source, and the molar ratio of non-oxygen elements Ti, Li, Al and P is the same in different raw material samples.
7. The method for screening key factors affecting ionic conductivity in the synthesis of oxide solid electrolytes as described in claim 6, characterized in that... The synthesis process of solid electrolytes includes the following steps: S1: All raw material samples were weighed according to the proportions of each component, C1-C4 alcohol solvent was added, and the mixture was ball-milled and mixed evenly. S2: Place the ball-milled and mixed raw materials into a drying oven to dry and remove excess moisture; S3: The dried material is placed in a muffle furnace for calcination. The synthesis temperature of the calcination is set to carry out the reaction. The synthesis time is the same at different synthesis temperatures so that the reaction can be fully achieved at this synthesis time to obtain the raw powder precursor. S4: The raw powder precursor is ball-milled, dried, and then cold-pressed into blocks. It is then sintered at a set sintering temperature. The sintering time is the same at different sintering temperatures, so that full sintering can be achieved at this sintering time, thus synthesizing a solid electrolyte.