A method for producing ultra-high purity copper using metallic copper in a chlorinated system
By employing oxidation-dissolution conversion, solid-liquid separation, and electrolysis steps in a chlorination system, high-purity copper can be directly produced, solving the problems of difficult impurity removal and environmental issues in traditional processes, and achieving efficient and low-cost production of ultra-high-purity copper.
Patent Information
- Application Number
- CN202311063291.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-22
AI Technical Summary
Existing technologies make it difficult to produce high-purity copper on a large scale, especially ultra-high-purity copper above 5N. Furthermore, traditional sulfuric acid systems have issues with the difficulty in removing impurities and environmental problems.
Using a chlorination system, ultra-high purity copper of 5N or higher is directly produced through steps such as oxidation-dissolution conversion, solid-liquid separation, back dissolution, and electrolysis. This includes mixing metallic copper raw materials with copper anode tail liquid from diaphragm electrolysis and an oxidant to form cuprous chloride crystals, performing solid-liquid separation and filtration, and finally electrolyzing to obtain ultra-high purity copper.
It achieves a wide range of raw material sources, simple process, low energy consumption, stable product quality, and no wastewater discharge, with production costs only 30% of traditional processes.
Smart Images

Figure CN117089891B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal smelting technology, and in particular to a method for producing ultra-high purity copper using metallic copper in a chlorination system. Background Technology
[0002] Copper is one of the most widely used non-ferrous metals. With the continuous progress and development of industry, the demand for copper, especially high-quality copper, is increasing. 1# and 0# refined copper are mainly used in the manufacture of conductive materials and copper alloys, while high-purity copper above 5N is mainly used in high-end semiconductor chips and the electronics industry.
[0003] Currently, the production of 1# (99.95%) and 0# (99.995%) copper metal both employ the sulfuric acid electrolytic refining method. Due to the limitations of this process, a single electrolysis cannot break through the 5N high-purity copper quality standard. High-purity copper above 5N is produced by repeatedly electrolytically refining 1# or 0# copper metal, resulting in unstable quality, difficulty in electrolyte purification, and challenges in large-scale industrial production. This leads to excessively high production costs and limits market expansion for copper above 5N. Furthermore, the traditional sulfuric acid copper refining process struggles to reduce sulfur impurities to trace levels. Even after multiple electrolytic refining processes, it is difficult to reach the 6N copper standard, requiring further electrolytic refining using a nitric acid system. This process fails to address the issue of impurity accumulation in the electrolyte during refining, leading to unstable product quality. Additionally, the introduction of the nitric acid system results in large quantities of nitric acid-containing wash water that is difficult to dispose of, causing significant environmental problems. Summary of the Invention
[0004] The purpose of this invention is to provide a method for producing ultra-high purity copper using metallic copper in a chlorination system. The method of this invention has the characteristics of wide availability of raw materials, simple process flow, easy control, low energy consumption, good product quality, stable product quality, and green environmental protection with no wastewater discharge.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a method for producing ultra-high purity copper using metallic copper in a chlorination system, comprising the following steps:
[0007] A mixture of metallic copper raw material, copper anode tailings from diaphragm electrolysis, and an oxidant is subjected to oxidative dissolution conversion. The metallic copper raw material dissolves and transforms into cuprous chloride crystals, yielding a cuprous chloride slurry. The oxidative dissolution conversion temperature is 30–80°C, and the pH value is maintained at 0–4 during the process. The copper anode tailings from diaphragm electrolysis contain 50 g / L ≤ Cl. - ≤250g / L, 5g / L≤Cu 2+ ≤50g / L, 1g / L≤Cu +≤10g / L, pH value is 0~4.
[0008] The cuprous chloride slurry was subjected to solid-liquid separation to obtain mother liquor and crude cuprous chloride crystals.
[0009] The crude cuprous chloride crystals were dissolved in the tailings of the copper cathode in a diaphragm electrolysis process, followed by filtration to remove insoluble impurities, yielding a high-purity copper ion solution. The tailings of the copper cathode in the diaphragm electrolysis solution contained 50 g / L ≤ Cl... - ≤250g / L, 5g / L≤Cu + ≤50g / L, 1g / L≤Cu 2+ ≤10g / L, pH value is 0~4.
[0010] The high-purity copper ion solution is electrolyzed to obtain ultra-high-purity copper; the purity of the ultra-high-purity copper is above 5N.
[0011] Preferably, the oxidation-dissolution conversion time is 60–200 min.
[0012] Preferably, the solid-liquid ratio of the copper raw material and the tailings of the diaphragm electrolytic copper anode is (5-200) kg: 1 m³. 3 .
[0013] Preferably, the oxidant includes pure oxygen, air, hydrogen peroxide, or chlorine.
[0014] Preferably, the concentration of the cuprous chloride slurry is 30-200 g / L; and the total concentration of copper ions in the clear liquid is 0.1-10 g / L.
[0015] Preferably, before the re-dissolution, the crude cuprous chloride crystals are washed with water.
[0016] Preferably, after obtaining the mother liquor, the process further includes: adding ammonia or ammonium bicarbonate to the mother liquor to neutralize it to a pH of 6-8, then introducing hydrogen sulfide gas or adding ammonium sulfide, so that the heavy metal ions in the mother liquor are converted into sulfide precipitates or carbonate precipitates, filtering to obtain filtrate and filter residue; and returning the filtrate to the oxidation-dissolution-conversion process.
[0017] Preferably, the temperature of the remelting is 40–60°C.
[0018] Preferably, the total concentration of copper ions in the high-purity copper ion solution is 50–100 g / L.
[0019] Preferably, in the electrolysis process, the cathode liquid temperature is maintained at 40–80°C; and the cathode plate current density is 100–500 A / m. 2 ;
[0020] During the electrolysis process, the anolyte temperature is maintained at 40–80°C, and the pH value is 0–4.
[0021] This invention provides a method for producing ultra-high purity copper using metallic copper in a chlorination system, comprising the following steps: mixing metallic copper raw material, copper anode tailings from diaphragm electrolysis, and an oxidant for oxidative dissolution conversion; the metallic copper raw material dissolves and converts into cuprous chloride crystals to obtain cuprous chloride slurry; the oxidative dissolution conversion temperature is 30–80°C; the pH value is maintained at 0–4 during the oxidative dissolution conversion process; and the concentration of Cl in the copper anode tailings from diaphragm electrolysis is ≤50 g / L. - ≤250g / L, 5g / L≤Cu 2+ ≤50g / L, 1g / L≤Cu + ≤10g / L; The cuprous chloride slurry is subjected to solid-liquid separation to obtain mother liquor and crude cuprous chloride crystals; The crude cuprous chloride crystals are placed in the tailings of the diaphragm electrolytic copper cathode for back dissolution, and then filtered to remove insoluble impurities to obtain a high-purity copper ion solution; The copper ion solution in the tailings of the diaphragm electrolytic copper cathode has a concentration of ≤50g / L Cl - ≤250g / L, 5g / L≤Cu + ≤50g / L, 1g / L≤Cu 2+ The concentration of copper ions is ≤10 g / L, and the pH value is 0–4. Electrolysis of the high-purity copper ion solution yields ultra-high-purity copper; the purity of the ultra-high-purity copper is ≥5N.
[0022] The method of this invention has the advantages of wide availability of raw materials, simple process flow, and can directly produce high-purity copper of 5N or above in one electrolysis. It has reliable impurity separation, is easy to control, has stable product quality, low energy consumption (only 30% of traditional processes), is green and environmentally friendly, and has no wastewater discharge. Attached Figure Description
[0023] Figure 1 This is a flow chart of the purification process of the present invention. Detailed Implementation
[0024] This invention provides a method for producing ultra-high purity copper using metallic copper in a chlorination system, comprising the following steps:
[0025] A mixture of metallic copper raw material, copper anode tailings from diaphragm electrolysis, and an oxidant is subjected to oxidative dissolution conversion. The metallic copper raw material dissolves and transforms into cuprous chloride crystals, yielding a cuprous chloride slurry. The oxidative dissolution conversion temperature is 30–80°C, and the pH value is maintained at 0–4 during the process. The copper anode tailings from diaphragm electrolysis contain 50 g / L ≤ Cl. - ≤250g / L, 5g / L≤Cu 2+ ≤50g / L, 1g / L≤Cu + ≤10g / L, pH value is 0~4.
[0026] The cuprous chloride slurry was subjected to solid-liquid separation to obtain mother liquor and crude cuprous chloride crystals.
[0027] The crude cuprous chloride crystals were dissolved in the tailings of the copper cathode in a diaphragm electrolysis process, followed by filtration to remove insoluble impurities, yielding a high-purity copper ion solution. The tailings of the copper cathode in the diaphragm electrolysis solution contained 50 g / L ≤ Cl... - ≤250g / L, 5g / L≤Cu + ≤50g / L, 1g / L≤Cu 2+ ≤10g / L, pH value is 0~4.
[0028] The high-purity copper ion solution is electrolyzed to obtain ultra-high-purity copper; the purity of the ultra-high-purity copper is above 5N.
[0029] This invention involves mixing metallic copper raw material, copper anode tail liquid from diaphragm electrolysis, and an oxidant for oxidation, dissolution, and conversion. The metallic copper raw material dissolves and is converted into cuprous chloride crystals to obtain cuprous chloride slurry.
[0030] In this invention, the purity of the copper raw material is preferably 90.0% to 99.995%. This invention does not have special requirements regarding the shape of the copper raw material; in embodiments of this invention, it is specifically copper wire.
[0031] In this invention, the tailings solution of the diaphragm electrolytic copper anode contains copper chloride and ammonium chloride, and may or may not contain sodium chloride; the tailings solution of the diaphragm electrolytic copper anode contains 5 g / L ≤ Cu 2+ ≤50g / L, 1g / L≤Cu + ≤10g / L, 50g / L≤Cl - The concentration of ammonium ions is preferably 3.5–5 mol / L, and the concentration of ammonium ions is preferably ≤250 g / L. The pH value of the tail liquid of the diaphragm electrolytic copper anode is preferably 0–4, and more preferably 1–3.
[0032] In this invention, the preferred solid-liquid ratio of the copper raw material and the tailings of the diaphragm electrolytic copper anode solution is (5-200) kg: 1 m³. 3 More preferably, it is (20-180) kg: 1 m 3 A further preferred ratio is (50-150) kg: 1 m 3 .
[0033] In this invention, the oxidation-dissolution conversion is preferably carried out under stirring conditions; the temperature of the oxidation-dissolution conversion is 30–80°C, preferably 40–70°C, more preferably 50–60°C; and the pH value is maintained at 0–4, preferably 1–3, during the oxidation-dissolution conversion process. This invention maintains the pH value within the above range during the oxidation-dissolution conversion process by adding electrolytic anolyte tailings.
[0034] In the oxidation-dissolution conversion process, the metallic copper raw material dissolves and is oxidized by copper chloride and oxidant in the tail liquid of the diaphragm electrolytic copper anode to convert it into cuprous chloride crystals. The reaction formula for the oxidation by copper chloride is Cu + CuCl2 = 2CuCl.
[0035] In this invention, the oxidant preferably includes pure oxygen, air, hydrogen peroxide, or chlorine.
[0036] In this invention, the oxidant is used to oxidize metallic copper into monovalent copper and divalent copper.
[0037] After the oxidation-dissolution conversion reaction is completed, the metallic copper raw material exists as cuprous chloride solid in the cuprous chloride slurry. In this invention, the concentration of the cuprous chloride slurry is preferably 30-200 g / L, and the total concentration of copper ions in the clear liquid (including Cu) is... + and Cu 2+ The preferred concentration is 0.1–10 g / L.
[0038] After obtaining cuprous chloride slurry, the present invention performs solid-liquid separation on the cuprous chloride slurry to obtain mother liquor and crude cuprous chloride crystals.
[0039] In this invention, the solid-liquid separation method is preferably centrifugal separation, with a centrifuge separation factor of 300-1500, more preferably 400-1300, and even more preferably 500-1000. This invention separates impurities dissolved in the mother liquor from cuprous chloride crystals through centrifugal separation.
[0040] After obtaining crude cuprous chloride crystals, the present invention places the crude cuprous chloride crystals in the tail liquid of the copper cathode of the diaphragm electrolysis for back dissolution, and then filters to remove insoluble impurities to obtain a high-purity copper ion solution.
[0041] In this invention, the tailings solution of the diaphragm electrolytic copper cathode contains copper chloride and ammonium chloride, and may or may not contain sodium chloride. In this invention, the tailings solution of the diaphragm electrolytic copper cathode contains 50 g / L ≤ Cl... - ≤250g / L, 5g / L≤Cu 2+ ≤50g / L, 1g / L≤Cu + ≤10g / L; pH value is 0~4; ammonium ion concentration is preferably 3.5~5mol / L.
[0042] In this invention, the liquid-to-solid ratio of the crude cuprous chloride crystals and the tailings from the diaphragm electrolytic copper cathode is preferably 5-50 kg: 1 m³. 3 More preferably, it is 10-40 kg: 1 m 3 A further preferred ratio is 20–30 kg: 1 m 3 .
[0043] In this invention, the preferred temperature for the back dissolution is 40–60°C. During the back dissolution process, cuprous chloride crystals are dissolved into the tail liquid of the copper cathode in diaphragm electrolysis. Cuprous chloride is insoluble in solutions with low chloride ion concentrations and exists in solid form, while it is soluble in solutions with high chloride ion concentrations and exists as monovalent copper ions.
[0044] In this invention, the re-dissolution time is preferably 30–200 min, more preferably 50–150 min. After re-dissolution is completed, the present invention uses filtration to remove insoluble impurities, obtaining a high-purity copper ion solution. In this invention, the filtration is preferably pressure filtration.
[0045] In this invention, the total concentration of copper ions in the high-purity copper ion solution is preferably 50–100 g / L, more preferably 60–90 g / L, and even more preferably 70–80 g / L; the ratio of divalent copper ion concentration to monovalent copper ion concentration is >10:1. In this invention, the copper ions in the high-purity copper ion solution mainly exist in the form of monovalent copper.
[0046] Prior to the re-dissolution, the crude cuprous chloride crystals are preferably washed with water. In this invention, the water used for washing is preferably purified water. This invention utilizes water washing to further purify the crude cuprous chloride crystals.
[0047] After the water washing is completed, the present invention obtains a washing liquid. Preferably, the mother liquor is purified and then returned to the oxidation-dissolution-conversion process, or the washing liquid and mother liquor are purified together and then returned to the oxidation-dissolution-conversion process. In the present invention, the main components of the washing liquid and mother liquor are copper chloride, cuprous chloride, and ammonium chloride (possibly containing sodium chloride) solutions.
[0048] In this invention, when purifying the mother liquor, the purification preferably includes: adding ammonia or ammonium bicarbonate to the mother liquor to neutralize it to a pH of 6-8, then introducing hydrogen sulfide gas or adding ammonium sulfide, causing the heavy metal ions in the mother liquor to be converted into sulfide precipitates or carbonate precipitates; filtering to obtain filtrate and filter residue; and returning the filtrate to the oxidation-dissolution-conversion process. The filter residue is an impurity.
[0049] When the purified mother liquor is returned to the oxidation-dissolution conversion process, the purified mother liquor, together with the tailings from the diaphragm electrolytic copper anode, serves as the dissolving solution to oxidize and dissolve the metallic copper raw material. The dissolving solution must meet the requirement of 50 g / L ≤ Cl. - ≤250g / L; 5g / L≤Cu 2+ ≤50g / L; 1g / L≤Cu + ≤10g / L, pH value is 0~4.
[0050] After obtaining a high-purity copper ion solution, the present invention electrolyzes the high-purity copper ion solution to obtain ultra-high-purity copper; the purity of the ultra-high-purity copper is above 5N.
[0051] In this invention, the electrolysis is performed using a diaphragm electrolytic cell. The high-purity copper ion solution enters the cathode chamber of the diaphragm electrolytic cell and permeates through the diaphragm to the anode chamber to form an anolyte. During the electrolysis process, the catholyte temperature is maintained at 40–80°C, the pH value is 0–4, the monovalent copper ion concentration is ≥30 g / L, and the cathode plate current density is 100–500 A / m. 2 .
[0052] In this invention, during the electrolysis process, the anolyte temperature is maintained at 40–80°C, and the pH value is 1–4.
[0053] In this invention, the electrolysis time is preferably 96–192 hours. During the electrolysis process, the liquid level in the cathode chamber is 5–30 mm higher than the liquid level in the anode chamber.
[0054] In this invention, the anolyte produced at the graphite anode is used in the oxidation-dissolution conversion process, and chlorine gas is collected and transported to the oxidation-dissolution conversion process as an oxidant; an ultrapure electrolytic copper plate is obtained on the cathode plate in the cathode chamber, and the cathode tail liquid obtained at the cathode is used in the re-dissolution process.
[0055] After electrolysis is completed, the present invention preferably removes the cathode plate and peels off the copper plate. The copper plate is then put into the casting section for casting. The vacuum degree is 0.02-0.098 MPa and the casting temperature is 1000-1500℃. Then it is injected into the mold to obtain ultra-high purity copper ingots, rods, plates and other profiles with a purity of 99.999%-99.999999%.
[0056] Figure 1 This is a flow chart of the purification process of the present invention.
[0057] like Figure 1 As shown, this invention mixes metallic copper raw material and electrolytic anode tail liquid, adds an appropriate amount of oxidant for oxidation-dissolution conversion, and the metallic copper raw material dissolves and is converted into cuprous chloride crystals to obtain cuprous chloride slurry; the invention centrifuges the cuprous chloride slurry to obtain mother liquor and crude cuprous chloride crystals; the crude cuprous chloride crystals are placed in the tail liquid of diaphragm electrolytic copper cathode for back dissolution, and then filtered to remove insoluble impurities to obtain a high-purity copper ion solution; the high-purity copper ion solution is electrolyzed to obtain ultra-high purity copper plates; the anode tail liquid and chlorine gas generated by electrolysis are returned to the oxidation-dissolution conversion process; at the same time, the mother liquor generated by centrifugation is purified and also returned to the oxidation-dissolution conversion process for use.
[0058] The following detailed description of the method for producing ultra-high purity copper using metallic copper in a chlorination system, with reference to specific embodiments, is intended to limit the scope of protection of this invention.
[0059] Example 1
[0060] Step 1) Oxidation, dissolution, and conversion process: 50 kg of metallic copper wire (99.9% purity) is added to a 1m... 3 In the mixture of electrolytic copper anode tail liquid and mother liquor (Cu 2+ =15g / L, Cu + =2 g / L; chloride ion = 60 g / L; pH = 2); add hydrogen peroxide as an oxidant and stir until the metallic copper is completely dissolved and converted into cuprous chloride crystals suspended in the solution. The pH value is controlled at 3 by the amount of copper anolyte added, the reaction temperature is 50℃, and the oxidation-dissolution-conversion time is 200 min. After the reaction, the concentration of cuprous chloride slurry is 85 g / L; the total copper ion concentration of the clear liquid is 0.5 g / L. After the reaction, the slurry is sent to the cuprous chloride crystal separation and purification process.
[0061] Step 2) Cuprous chloride crystal separation process: This step uses a centrifuge to separate cuprous chloride crystals and mother liquor, separating impurities dissolved in the mother liquor from the cuprous chloride crystals, achieving a purification effect. After centrifugation, approximately 20 kg of purified water is used to wash the cuprous chloride crystals for further purification. After separation and purification, the mother liquor and washing liquid enter the dissolution purification process, and then return to Step 1); the resulting approximately 85 kg of crude cuprous chloride crystals are fed into the cuprous chloride crystal re-dissolution purification process.
[0062] Step 3) Mother liquor purification process: The mother liquor separated from cuprous chloride enters the purification tank, where ammonia water is first added to neutralize it to a pH of around 6-8. Then, an appropriate amount of ammonium sulfide is added to remove metal ions from the solution. The solution is then filtered using a filter press, and the filtrate is sent to the oxidation-dissolution-conversion process. The filter residue is discarded as impurities.
[0063] Step 4) Cuprous chloride crystal re-dissolution process: The crude powdered cuprous chloride crystals obtained in Step 2) are added to the electrolyte containing the electrolytic cathode tailings (Cu). 2+ =6g / L, Cu + =45g / L; chloride ion =170g / L; pH =1.5) in a stirred tank, with a liquid-to-solid ratio of 10kg:1m 3 The temperature was controlled at 50℃, the pH value at around 2, and the total copper ion concentration at 90 g / L; the re-dissolution time was 60 min. Then, the solution was filtered using a filter press to remove insoluble impurities and filter residue, yielding a high-purity copper ion solution. This high-purity monovalent copper ion solution then proceeded to the electrolysis process.
[0064] Step 5) Electrolysis process: Electrolysis is performed using a diaphragm electrolytic cell. A high-purity monovalent copper ion solution enters the cathode chamber of the diaphragm electrolytic cell, and the cathode current density is 200 A / m. 2 In the anode chamber, the anolyte and chlorine gas generated at the graphite anode are collected and transported to the oxidation-dissolution conversion process for use as oxidants. Ultrapure electrolytic copper plates are obtained on the cathode plates in the cathode chamber. After electrolysis for a certain time (96 hours), the cathode plates are removed and the copper plates are peeled off. The resulting copper plates are then fed into the casting section. The cathode tailings enter the remelting process, while the anode tailings are returned to the oxidation-dissolution conversion process.
[0065] Step 6) Melting and casting process: The obtained high-purity copper plate is put into a graphite crucible vacuum melting and casting furnace for melting and casting, with a vacuum degree of 0.09 MPa and a melting and casting temperature of 1200℃. Then it is injected into a mold to obtain 99.99999% ultra-high purity copper ingots.
[0066] Example 2
[0067] Step 1) Oxidation, dissolution, and conversion process: 100 kg of copper wire (99.9% purity) is added to a 1m... 3 In the mixture of electrolytic copper anode tail liquid and mother liquor (Cu 2+ =15g / L, Cu + =2 g / L; chloride ion = 60 g / L; pH = 2); add hydrogen peroxide as an oxidant and stir until the metallic copper is completely dissolved and converted into cuprous chloride crystals suspended in the solution. The pH value is controlled at 3 by the amount of copper anolyte added, the reaction temperature is 50℃, and the oxidation-dissolution-conversion time is 200 min. After the reaction, the concentration of cuprous chloride slurry is 85 g / L; the total copper ion concentration of the clear liquid is 0.5 g / L. After the reaction, the slurry is sent to the cuprous chloride crystal separation and purification process.
[0068] Step 2) Cuprous chloride crystal separation process: This step uses a centrifuge to separate cuprous chloride crystals and mother liquor, separating impurities dissolved in the mother liquor from the cuprous chloride crystals, achieving a purification effect. After centrifugation, approximately 20 kg of purified water is used to wash the cuprous chloride crystals for further purification. After separation and purification, the mother liquor and washing liquid enter the dissolution purification process, and then return to Step 1); the resulting approximately 170 kg of crude cuprous chloride crystals are fed into the cuprous chloride crystal re-dissolution purification process.
[0069] Step 3) Mother liquor purification process: The mother liquor separated from cuprous chloride enters the purification tank, where ammonia water is first added to neutralize it to a pH of around 6-8. Then, an appropriate amount of ammonium sulfide is added to remove metal ions from the solution. The solution is then filtered using a filter press, and the filtrate is sent to the oxidation-dissolution-conversion process. The filter residue is discarded as impurities.
[0070] Step 4) Cuprous chloride crystal re-dissolution process: The crude powdered cuprous chloride crystals obtained in Step 2) are added to the electrolyte containing the electrolytic cathode tailings (Cu). 2+ =6g / L, Cu + =45g / L; chloride ion =170g / L; pH =1.5) in a stirred tank, with a liquid-to-solid ratio of 10kg:1m 3 The temperature was controlled at 50℃, the pH value at around 2, and the total copper ion concentration at 90 g / L; the re-dissolution time was 60 min. Then, the solution was filtered using a filter press to remove insoluble impurities and filter residue, yielding a high-purity copper ion solution. This high-purity monovalent copper ion solution then proceeded to the electrolysis process.
[0071] Step 5) Electrolysis process: Electrolysis is performed using a diaphragm electrolytic cell. A high-purity monovalent copper ion solution enters the cathode chamber of the diaphragm electrolytic cell, and the cathode current density is 200 A / m. 2 In the anode chamber, the anolyte and chlorine gas generated at the graphite anode are collected and transported to the oxidation-dissolution conversion process for use as oxidants. Ultrapure electrolytic copper plates are obtained on the cathode plates in the cathode chamber. After electrolysis for a certain time (96 hours), the cathode plates are removed and the copper plates are peeled off. The resulting copper plates are then fed into the casting section. The cathode tailings enter the remelting process, while the anode tailings are returned to the oxidation-dissolution conversion process.
[0072] Step 6) Melting and casting process: The obtained high-purity copper plate is put into a graphite crucible vacuum melting and casting furnace for melting and casting, with a vacuum degree of 0.09 MPa and a melting and casting temperature of 1200℃. Then it is injected into a mold to obtain 99.99999% ultra-high purity copper ingots.
[0073] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for producing ultra-high purity copper using metallic copper in a chlorination system, comprising the following steps: A mixture of metallic copper raw material, copper anode tailings from diaphragm electrolysis, and an oxidant is subjected to oxidative dissolution conversion. The metallic copper raw material dissolves and transforms into cuprous chloride crystals, yielding a cuprous chloride slurry. The oxidative dissolution conversion temperature is 30-80℃, and the pH value is maintained at 0-4 during the process. The copper anode tailings from diaphragm electrolysis contain 50g / L ≤Cl. - ≤250g / L, 5g / L≤Cu 2+ ≤50g / L, 1g / L≤Cu + ≤10g / L, pH value 0~4; the solid-liquid ratio of the copper raw material and the diaphragm electrolytic copper anode tail liquid is (5~200) kg: 1m 3 ; The cuprous chloride slurry was subjected to solid-liquid separation to obtain mother liquor and crude cuprous chloride crystals. The crude cuprous chloride crystals were dissolved in the tailings of the copper cathode in a diaphragm electrolysis process, followed by filtration to remove insoluble impurities, yielding a high-purity copper ion solution. The tailings of the copper cathode in the diaphragm electrolysis solution contained 50 g / L ≤ Cl... - ≤250g / L, 5g / L≤Cu + ≤50g / L, 1g / L≤Cu 2+ ≤10g / L, pH value is 0~4; The high-purity copper ion solution is electrolyzed to obtain ultra-high-purity copper; the purity of the ultra-high-purity copper is above 5N. After obtaining the mother liquor, the process further includes: adding ammonia or ammonium bicarbonate to the mother liquor to neutralize it to a pH of 6-8, then introducing hydrogen sulfide gas or adding ammonium sulfide, so that the heavy metal ions in the mother liquor are converted into sulfide precipitates or carbonate precipitates, filtering to obtain filtrate and filter residue; and returning the filtrate to the oxidation-dissolution-conversion process.
2. The method according to claim 1, characterized in that, The oxidation-dissolution conversion time is 60~200 min.
3. The method according to claim 1, characterized in that, The oxidant includes pure oxygen, air, hydrogen peroxide, or chlorine.
4. The method according to claim 1, characterized in that, The concentration of the cuprous chloride slurry is 30~200g / L; the total concentration of copper ions in the clear liquid is 0.1~10g / L.
5. The method according to claim 1, characterized in that, Before the re-dissolution, the crude cuprous chloride crystals are washed with water.
6. The method according to claim 1, characterized in that, The temperature for remelting is 40~60℃.
7. The method according to claim 1 or 6, characterized in that, The total concentration of copper ions in the high-purity copper ion solution is 50~100g / L.
8. The method according to claim 1, characterized in that, During the electrolysis process, the cathode liquid temperature is maintained at 40~80℃; the cathode plate current density is 100~500A / m. 2 ; During the electrolysis process, the anolyte temperature is maintained at 40~80℃; the pH value is 0~4.
Citation Information
Patent Citations
Regeneration method of acidic etching solution
CN110106506A
Method of obtaining copper from sulphurized concentrates
US4016056A