A method for preparing pure iron by waste chloride molten salt electrodeposition
By screening, remelting, grinding, and electrolyzing waste chloride molten salt, pure iron materials are prepared, solving the problem of the difficulty in recycling waste chloride molten salt, realizing efficient resource utilization and environmentally friendly treatment, and obtaining high-purity pure iron products.
Patent Information
- Application Number
- CN202311099698.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-08-28
AI Technical Summary
In existing technologies, waste chloride molten salts are difficult to recycle effectively, especially elements such as Fe²⁺ and Fe³⁺, leading to serious environmental pollution and resource waste. Furthermore, the problem of solid waste treatment generated by the molten salt chlorination process has not been effectively solved.
By screening, remelting, and grinding waste chloride molten salt, adding electrolytes such as NaCl and CaCl₂, controlling electrochemical parameters, and electrolyzing under inert gas protection, pure iron materials are prepared by deposition. Controllable electrodeposition is achieved by utilizing the deposition potential differences of metal elements in complex chloride molten salt.
This method enables the efficient resource utilization of waste chloride molten salt, reduces the amount of solid waste, and produces pure iron materials with high deposition rates and dense deposition layers, thus achieving both economic benefits and environmental protection characteristics.
Smart Images

Figure CN117107301B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource recycling and metallurgical technology, specifically relating to a method for preparing pure iron from waste chloride molten salt deposition. Background Technology
[0002] Molten salt chlorination is an important industrial method for producing TiCl4, especially suitable for titanium raw materials with high calcium and magnesium impurity content. It is widely used in major TiCl4 production enterprises in Russia, Ukraine, Kazakhstan, and my country. However, due to the complex composition of the molten salt waste chloride, it is difficult to utilize effectively, and there are currently no successful resource recovery technologies for its application both domestically and internationally. Most factories generally adopt a "crushing-lime mixing-landfill or stockpiling" method for disposal, but this method fails to effectively solve the environmental pollution problem caused by chlorides, leading to increasingly serious environmental pollution.
[0003] my country is a major producer and exploiter of titanium resources, which has secured its position as the world's largest producer of titanium dioxide and sponge titanium. However, my country's titanium resources are characterized by low grade and high levels of calcium and magnesium impurities. While molten salt chlorination is suitable for high-value utilization, it presents challenges such as the large volume of waste chloride molten salt and difficulties in its clean utilization. The resource-based treatment of waste chloride molten salt has become a technological bottleneck restricting the high-value-added utilization of my country's titanium resources. The latest process for the resource-based utilization of waste chloride molten salt, namely "high-efficiency leaching with molten salt quenching - purification and crystallization - NaCl crystal re-chlorination furnace circulation - NaCl brine refining," recovers NaCl, but still retains a significant amount of Fe in the waste chloride molten salt. 2+ Fe 3+ However, it has not been effectively recycled. Compared with the production of TiCl4 by boiling chlorination, molten salt chlorination has a better feedstock window and adaptability, but its salt discharge volume is large. It is used by many enterprises in China, but the solid waste after regular salt discharge is difficult to treat. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for preparing pure iron by electrodeposition of waste chloride molten salt, comprising the following steps:
[0005] Step 1: The waste chloride molten salt generated in the TiCl4 production process of molten salt chlorination is crushed, sieved, and then remelted and purified at 700-850℃ for 1-24 hours under inert gas protection. It is then ground into powder to obtain pre-molten salt powder, and its Cl, Na, O and Fe components are analyzed.
[0006] Step 2: Optionally, add 5% to 30% NaCl and / or 1% to 10% CaCl2 to the pre-melted salt powder, mix and pulverize to obtain a mixed new salt;
[0007] Step 3: Add the pre-melted salt powder or the mixed new salt to a crucible protected by an inert gas and heat to 200-400°C, and keep it at that temperature for 1-8 hours to remove moisture from the raw materials; then, further increase the temperature to 500-900°C and continue to keep it at that temperature for 12-48 hours to obtain molten salt.
[0008] Step 4: Using the molten salt obtained in Step 3 as the electrolyte, connect the cathode and anode, and apply an electrolyte at a current density of 50–500 mA / cm². 2 Pre-electrolysis is performed within the range for 0.5 to 4 hours, and the cathode is removed after purification.
[0009] Step 5: Insert a new cathode and deposit it at a constant voltage of 1.3 to 3.0 V for 3 to 44 hours. Remove the cathode, collect the cathode product, clean the electrolyte in the cathode product with deionized water using ultrasonic cleaning, then with anhydrous ethanol, and finally dry it in a vacuum drying oven to obtain pure iron material.
[0010] Further, in step 2, CaCl2 and NaCl are added according to the range of O (oxygen) content in the pre-melted salt powder. When the O content is below 31%, no CaCl2 or NaCl needs to be added; when the O content is between 32% and 35%, 5% to 10% CaCl2 is added based on the weight of the pre-melted salt powder; when the O content is above 36%, 1% to 5% CaCl2 and 5% to 30% NaCl are added based on the weight of the pre-melted salt powder. In addition, the Fe element content in the pre-melted salt powder should reach 6% to 35% of the total weight of the pre-melted salt, and should be positively correlated with the weight of the cathode product and the yield of pure iron material.
[0011] Further, in step 1, the crushed waste chloride molten salt is sieved using a 2cm sieve, and the material passing through the sieve is collected.
[0012] Furthermore, in steps 1 and 2, an Fw-80 or FTT-2500 milling machine is used for milling.
[0013] Furthermore, in step 1, the inert gas is argon.
[0014] Furthermore, in step 3, the crucible is selected from one of high-purity graphite crucible, corundum crucible, and magnesium oxide crucible, with high-purity graphite crucible being preferred.
[0015] Further, in step 4, the cathode is selected from one of high-purity graphite rods (sheets), iron mesh (sheets), and tungsten rods; the anode is selected from one of high-purity graphite rods (sheets), graphite crucibles, ferrosilicon rods (sheets), and scrap iron rods (sheets), preferably ferrosilicon rods (sheets), scrap iron rods (sheets), and other iron-containing soluble anodes. The soluble anode refers to an anode that can dissolve into metal ions and enter the solution when current passes through it.
[0016] Furthermore, in step 5, deposition is performed under a constant voltage of 2.0–3.0V.
[0017] Furthermore, by periodically injecting pre-molten salt powder or mixing new salt, and repeating steps 1-5, continuous production of zero-carbon ironmaking can be achieved.
[0018] Furthermore, in step 5, the iron obtained by electrodeposition in the cathode product mainly comes from the reduction of iron elements in the waste chloride molten salt of the electrolyte, as well as the iron-containing soluble anode dissolution and reduction.
[0019] Furthermore, the pure iron material produced by the method of the present invention can be a pure iron film, pure iron grains, or pure iron powder.
[0020] Technical effect
[0021] The inventors discovered that the chlorination process chlorinates iron oxides in titanium slag into FeCl2 and FeCl3, which have better conductivity and solubility, and further generates Na6FeCl8 and Na2FeCl4 in the reaction, which can improve the efficiency of iron electrolysis. The main components of the waste chloride molten salt are Na2FeCl4 and Na6FeCl8. Compared with FeCl3, which also meets the requirements of conductivity and solubility, it is cheaper. Na6FeCl8 and others have stronger conductivity and can dissolve in large quantities in the electrolyte. Therefore, the waste chloride molten salt generated in the process of producing TiCl4 by molten salt chlorination is selected as raw material. The combination of various chloride molten salts contained therein can lower the overall melting point and realize low-temperature electrolytic reduction of iron. By controlling the electrochemical parameters, metallic iron can be selectively deposited smoothly on the electrode, which can achieve almost zero raw material cost and zero carbon iron smelting, with good economic and social benefits.
[0022] However, the following difficulties exist when directly electrolyzing the waste chloride molten salt generated in the TiCl4 production process using molten salt chlorination: 1. The waste chloride molten salt has a complex physical structure, containing elements such as Na, Mg, Mn, Al, Ca, and Si in addition to Fe, making it difficult to achieve single iron deposition; 2. The waste chloride molten salt also contains a large amount of pyroxene phase and oxide phase, which reduces the conductivity of molten salt electrolysis, increases viscosity, and is not conducive to mass transfer; 3. At 800℃, the waste chloride molten salt exhibits the coexistence of solid, liquid, and gas phases, with large property fluctuations and the formation of substances such as low-boiling-point FeCl3, which seriously affects the electrolysis efficiency.
[0023] In this invention, the relative contents of elements such as iron and oxygen in the treated waste chloride molten salt are first determined. Breakthroughly, the oxygen content is used as an indicator of the oxide content affecting the fluidity of the molten salt. Appropriate electrolytes such as sodium chloride and calcium chloride are added for dilution, thereby improving the fluidity of the molten salt and enabling its successful electrolysis to prepare pure iron materials. This invention utilizes the different deposition potentials of various metal elements in complex chloride molten salt waste for controlled electrodeposition, enabling stable and controllable deposition and recovery of iron from solid waste, reducing the amount of solid waste by 10%-40%.
[0024] Furthermore, after electrolysis, the cathode product is ultrasonically cleaned with deionized water, then cleaned with anhydrous ethanol, and finally vacuum dried, which can avoid rapid oxidation during iron separation. Molten salt electrolysis also has the advantages of high deposition rate and obtaining a dense deposition layer, and is safe and environmentally friendly. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the process for preparing pure iron materials in a preferred embodiment of the present invention;
[0026] Figure 2 This is the XRD pattern of the product obtained in Embodiment 1 of the present invention;
[0027] Figure 3 This is a typical cyclic voltammetry curve of molten salt used in Example 1 of the present invention;
[0028] Figure 4 These are surface microstructure images of pure iron grains prepared on high-purity graphite rods according to Example 1 of the present invention, and corresponding EDS energy spectrum images of the pure iron grains.
[0029] Figure 5 This is a cross-sectional morphology diagram of the pure iron film prepared on an iron sheet in Example 2 of the present invention, and the corresponding EDS energy spectrum of the pure iron film.
[0030] Figure 6 These are the microstructure images and corresponding EDS spectra of the pure iron film material prepared on the graphite crucible cathode in Example 3 of this invention.
[0031] Figure 7 These are XRD patterns of the raw materials used in Embodiments 1-3 of the present invention, wherein curve 1 is the XRD pattern of the raw materials in Embodiments 1 and 2 of the present invention, and curve 2 is the XRD pattern of the raw materials in Embodiment 3 of the present invention. Detailed Implementation
[0032] The following description, with reference to the accompanying drawings, illustrates several preferred embodiments of the present invention to make its technical content clearer and easier to understand. The present invention can be embodied in many different forms, and the scope of protection of the present invention is not limited to the embodiments mentioned herein.
[0033] Example 1
[0034] In this embodiment, pure iron is prepared by electrodeposition of waste chloride molten salt, including the following steps:
[0035] Step 1: The waste chloride molten salt from the TiCl4 chlorination production process of a certain company was used. It was crushed, sieved through a 2cm screen, and the undersize was collected. This undersize was then remelted and purified at 850℃ for 12 hours under argon protection. The purified powder was then ground using an Fw-80 pulverizer. XRF (X-ray fluorescence spectrometry) analysis revealed that the main components were Cl, Na, O, and Fe, accounting for 41.93%, 9.3%, 4.59%, and 30.04% by mass, respectively. The main phases were Na6FeCl8 and Na2FeCl4. Figure 7 As shown in curve 1 above, cyclic voltammetry was performed on it, and the results are as follows. Figure 3 As shown, the electrochemical window is -2 to 2V, and the scan rate is 0.02V / s. The three electrodes are: a graphite crucible as the counter electrode, a high-purity graphite rod one as the working electrode, and a high-purity graphite rod two as the reference electrode. This can partially reflect the electrochemical characteristics and reduction potential of waste chloride molten salt, proving that the deposition of iron is theoretically feasible, and serving as a reference for setting the cell voltage in two-electrode electrolysis.
[0036] Step 2: Considering the O content is less than 31%, there is no need to add sodium chloride or calcium chloride;
[0037] Step 3: Add 100g of pre-melted salt powder to a graphite crucible, and use the graphite crucible as the anode, and two graphite rods as the impurity removal electrode and cathode respectively. Heat the crucible to 400℃ under an argon atmosphere, hold for 4 hours, and then heat it to 850℃ for electrolysis.
[0038] Step 4: Perform a current density of 300 mA / cm at this temperature. 2 The electrode was pre-electrolyzed for 1 hour, and then the impurity removal electrode was removed. Another graphite rod was inserted as the cathode, and deposition was carried out at a constant voltage of 2.0V for 8 hours. The cathode was then removed, and 14.57g of cathode product was collected.
[0039] Step 5: Wash the cathode product with deionized water and vacuum dry to obtain pure iron grains, the XRD pattern of which is shown below. Figure 2 As shown, the peaks marked are Fe and those not marked are C. It can be seen that the Fe peak is extremely strong, while the C peak only shows a weak peak at 26°, indicating that pure iron with a low C content was successfully obtained.
[0040] The surface morphology and EDS spectrum of the obtained pure iron grains are as follows: Figure 4 As shown, the pure iron grains can grow completely, which is beneficial for the preparation of high-purity materials and can be used to further produce pure iron.
[0041] Example 2
[0042] The same raw materials and methods as in Example 1 were used to prepare pure iron material, with the difference that: in this example, an alumina crucible was used, two graphite rods were used as the impurity removal electrode and the anode, respectively, and a pure iron sheet was used as the cathode substrate. After deposition at 650°C and a deposition potential of 1.5V for 8 hours, the cathode was removed, and the cathode sheet gained 5.66g in weight. The cathode product was then washed with deionized water and vacuum dried to obtain a pure iron film. The cross-sectional morphology and the corresponding EDS spectrum of the pure iron film are shown in the figure. Figure 5 As shown, a thin iron film with small grains and high porosity is formed, which can be further used as an iron catalytic support substrate.
[0043] Compared with the results of Example 1, it was found that using a graphite crucible as both the container and the anode was more conducive to electrolytic deposition, thereby obtaining more pure iron material products.
[0044] Example 3
[0045] In this embodiment, pure iron is prepared by electrodeposition of waste chloride molten salt, as follows: Figure 1 As shown, it includes the following steps:
[0046] Step 1: The waste chloride molten salt produced by a certain company during the molten salt chlorination process of TiCl4 was used. After sorting, screening, and crushing, XRF analysis showed that the main components were Cl, Na, O, and Fe, accounting for 39.18%, 8.33%, 41.93%, and 28.84% by mass, respectively. The main phases were Na6FeCl8, Na2FeCl4, and complex pyroxene oxides that had not undergone chlorination. Figure 7 The lower curve 2 has relatively poor fluidity and molten salt stability;
[0047] Step 2: Add 15% NaCl and 5% CaCl2 (by mass fraction) of waste chloride molten salt. Mix and pulverize using an FTT-2500 pulverizer to obtain a new mixed salt.
[0048] Step 3: Add 100g of mixed fresh salt to a graphite crucible, using the graphite crucible as the cathode and two graphite rods as the impurity removal electrode and anode, respectively. Heat to 400℃ under an argon atmosphere and hold for 1 hour, then increase the temperature to 800℃.
[0049] Step 4: Perform a current density of 50 mA / cm² at this temperature. 2 After 1 hour of pre-electrolysis, the impurity-removing cathode is removed and a new graphite crucible cathode is inserted.
[0050] Step 4: Deposit at a constant voltage of 2.5V for 12 hours. Wash the cathode product with deionized water and vacuum dry to obtain an iron film, which weighs 8.84g. The microstructure and corresponding EDS spectrum of the pure iron film material are shown below. Figure 6 As shown, a thin iron film with large grains, uniform thickness, and good flexibility is formed, which can be further used as a precursor for ferroelectric materials or wearable flexible materials.
[0051] The electrolysis conditions and X-ray fluorescence spectrometry (XRF) detection results of the electrodeposition products in each embodiment are shown in Table 1 below.
[0052] Table 1. Electrolysis conditions and X-ray fluorescence spectrometry (XRF) results of electrodeposition products in each embodiment
[0053]
[0054] The XRF results from the above examples show that the Fe (wt%) in the products of implementations 1 and 3 meets the standard for pure iron; and the main influencing factors for obtaining pure iron by electrolysis include the selection of electrode materials, electrolysis voltage and temperature.
[0055] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.
Claims
1. A method for preparing pure iron by electrodeposition of waste chloride molten salt, comprising the following steps: Step 1: The waste chloride molten salt generated in the TiCl4 production process of molten salt chlorination is crushed, sieved, and then remelted and purified at 700-850℃ for 1-24 hours under inert gas protection. It is then ground into powder to obtain pre-molten salt powder, and its Cl, Na, O and Fe components are analyzed. Step 2: Optionally, add 5% to 30% NaCl and / or 1% to 10% CaCl2 to the pre-melted salt powder, mix and pulverize to obtain a new mixed salt; Step 3: Add the pre-melted salt powder or the mixed new salt to a crucible protected by an inert gas and heat to 200-400°C, and keep it at that temperature for 1-8 hours to remove moisture from the raw materials; then, further increase the temperature to 500-900°C and continue to keep it at that temperature for 12-48 hours to obtain molten salt. Step 4: Using the molten salt obtained in Step 3 as the electrolyte, connect the cathode and anode, and apply an electrolyte at a current density of 50–500 mA / cm². 2 Pre-electrolysis is performed within the range for 0.5 to 4 hours, and the cathode is removed after purification. Step 5: Insert a new cathode and deposit it under a constant voltage of 1.3 to 3.0 V for 3 to 44 hours. Remove the cathode, collect the cathode product, clean the electrolyte in the cathode product with deionized water using ultrasonic cleaning, then with anhydrous ethanol, and finally dry it in a vacuum drying oven to obtain pure iron material. In step 2, CaCl2 and NaCl are added according to the range of O content in the pre-melted salt powder. When the O content is below 31%, no CaCl2 or NaCl needs to be added; when the O content is between 32% and 35%, 5% to 10% CaCl2 is added based on the weight of the pre-melted salt powder; when the O content is above 36%, 1% to 5% CaCl2 and 5% to 30% NaCl are added based on the weight of the pre-melted salt powder.
2. The method according to claim 1, wherein, The Fe content in the pre-melted salt powder is 6% to 35% of the total weight of the pre-melted salt.
3. The method according to claim 1, wherein, In step 1, the inert gas is argon.
4. The method according to claim 1, wherein, In step 3, the crucible is selected from one of the following: high-purity graphite crucible, corundum crucible, and magnesium oxide crucible.
5. The method according to claim 1, wherein, In step 4, the cathode is selected from one of the following: high-purity graphite rod, high-purity graphite sheet, iron mesh, iron sheet, and tungsten rod.
6. The method according to claim 1, wherein, The anode is selected from one of the following: high-purity graphite rod, high-purity graphite sheet, graphite crucible, ferrosilicon rod, ferrosilicon sheet, scrap iron rod, and scrap iron sheet.
7. The method according to claim 1, wherein, In step 5, deposition is performed at a constant voltage of 2.0–3.0V.
8. The method according to claim 1, wherein, The pure iron material is a pure iron film, pure iron grains, or pure iron powder.
Citation Information
Patent Citations
Method for preparing pure iron through molten salt electrolysis method
CN110528029A
Method for preparing high-purity iron through high-temperature fused salt electrodeposition
CN114232033A