A semiconductor structure and a method of fabricating the same
By performing doping treatment and forming a doped layer on the surface of the isolation trench, the problems of large leakage current and short data retention time in semiconductor memory are solved, achieving higher electrical performance and data stability.
Patent Information
- Application Number
- CN202210524597.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-05-13
AI Technical Summary
In existing technologies, as the integration density of semiconductor manufacturing processes increases, the increased integration density of memory leads to problems such as large leakage current, short data retention time, and loss of target stored charge data.
In the fabrication of semiconductor structures, a doped layer is formed on the surface of the isolation trench, and word lines are formed in the isolation trench. This increases the hole concentration around the word lines and reduces leakage current. At the same time, increasing the depth or width of the word lines can further reduce leakage current.
It effectively reduces leakage current, improves data retention time, reduces the loss of stored charge data, and improves the electrical performance of semiconductor structures.
Smart Images

Figure CN117116846B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of semiconductor technology, and in particular to a semiconductor structure and its fabrication method. Background Technology
[0002] As the integration density in semiconductor manufacturing processes continues to increase, improving the integration density of memory has become a trend. Consequently, the size of integrated circuits is gradually shrinking, which increases the difficulty of memory fabrication. Memory structures fabricated using current processes often suffer from problems such as high leakage current, short data retention time, and loss of data due to the target stored charge.
[0003] Therefore, optimizing memory manufacturing processes is a pressing technical problem that needs to be solved at this stage. Summary of the Invention
[0004] This disclosure provides a method for fabricating a semiconductor structure, comprising: providing a substrate; forming isolation trenches in the substrate to form a plurality of discrete active regions in the substrate, wherein the projection of the active regions in a direction perpendicular to the substrate plane extends along a first direction; doping at least a portion of the surface of the isolation trenches to form a doped layer; filling the isolation trenches with a dielectric layer to form an isolation structure; patterning the active regions and the isolation structure to form a groove extending along a second direction, wherein the first direction intersects the second direction; and forming word lines within the grooves.
[0005] In some embodiments, forming isolation trenches in the substrate to form a plurality of discrete active regions in the substrate includes: forming a first mask pattern on the substrate, the first mask pattern having a plurality of first pattern regions spaced apart along a first direction and gaps located between each adjacent first pattern region, wherein the plurality of first pattern regions are simultaneously spaced apart along a third direction; transferring the first mask pattern into the substrate to form active regions defined by the first pattern regions and isolation trenches defined by the gaps in the substrate.
[0006] In some embodiments, a protective layer is formed on the substrate before the isolation trench is formed in the substrate; after the protective layer is formed, the protective layer and the substrate are etched to form the isolation trench, and the unetched protective layer is formed on the active region.
[0007] In some embodiments, after the isolation trench is filled with a dielectric layer to form an isolation structure, the protective layer on the active region is removed.
[0008] In some embodiments, forming isolation trenches in the substrate to form a plurality of discrete active regions in the substrate includes: forming a second mask pattern on the substrate, the second mask pattern having a plurality of second pattern regions extending along a first direction and gaps between adjacent second pattern regions, wherein the second pattern regions are spaced apart along a third direction, the third direction intersecting the first direction; transferring the second mask pattern to the substrate to form a plurality of preset patterns and a first isolation trench located between the preset patterns in the substrate; filling the first isolation trench with a first dielectric layer; forming a third mask pattern on the substrate, the third mask pattern having a plurality of discrete pattern holes, each pattern hole being arranged along the third direction, each pattern hole exposing a portion of the preset pattern; transferring the pattern holes to the preset pattern to form a second isolation trench in the preset pattern to define the preset pattern as the active region.
[0009] In some embodiments, at least a portion of the surface of the isolation trench is doped to form a doped layer, including: doping the sidewalls and bottom of the second isolation trench to form the doped layer on the surface of the second isolation trench; filling the second isolation trench with a second dielectric layer, wherein the first isolation trench and the second isolation trench form the isolation trench, and the first dielectric layer and the second dielectric layer form the isolation structure.
[0010] In some embodiments, after forming the doped layer and before forming the isolation structure, the method further includes: forming a third sacrificial layer covering the doped layer on the surface of the second isolation trench; etching a portion of the third sacrificial layer; forming an opening in the third sacrificial layer that exposes the bottom of the second isolation trench; performing ion doping along the opening to the bottom of the second isolation trench; forming an auxiliary doped layer at the bottom of the second isolation trench; and removing the third sacrificial layer after forming the auxiliary doped layer.
[0011] In some embodiments, after forming the doped layer and before forming the isolation structure, the method further includes: forming a fourth sacrificial layer covering the doped layer on the surface of the second isolation trench; etching a portion of the fourth sacrificial layer to form an opening in the fourth sacrificial layer exposing the bottom of the second isolation trench; etching the substrate along the opening to form an auxiliary isolation trench below the second isolation trench; after forming the auxiliary isolation trench, removing the fourth sacrificial layer; and filling the second isolation trench and the auxiliary isolation trench with a second dielectric layer, wherein the first dielectric layer and the second dielectric layer form the isolation structure.
[0012] In some embodiments, the doped layer is formed by ion implantation, wherein the ions used in the ion implantation process include one or more of boron ions, boron difluoride ions and indium ions, and the energy range of the ion implantation process is 1 KeV to 30 KeV; the thickness of the doped layer is 10 nm to 40 nm.
[0013] In some embodiments, the auxiliary doped layer is formed by ion implantation, wherein the ions used in the ion implantation process include one or more of boron ions, boron difluoride ions, and indium ions, and the energy range of the ion implantation process is 20 KeV to 50 KeV; the thickness range of the auxiliary doped layer is 20 nm to 80 nm.
[0014] In some embodiments, patterning the active region and the isolation structure to form grooves extending along a second direction includes: forming a word line mask having a plurality of strip patterns extending along a second direction intersecting a first direction; etching the substrate using the word line mask as a mask to form a plurality of grooves extending along the second direction, wherein a portion of the grooves are formed within the isolation trench, and the ratio of the depth of the groove to the depth of the isolation trench is greater than 78%; or, the ratio of the width of the groove to the width of the isolation trench is less than 40%.
[0015] This disclosure also provides a semiconductor structure, including: a substrate; an isolation structure including an isolation trench and a first dielectric layer located within the isolation trench, the isolation structure defining the substrate as a plurality of discrete active regions, the projection of the active regions in the vertical direction extending along a first direction; a doped layer located at least on the sidewall of the isolation trench between the plurality of adjacent active regions along the first direction; a groove extending along a second direction intersecting the first direction and passing through the active regions and the isolation structure; and a word line located in the groove.
[0016] In some embodiments, the thickness of the doped layer ranges from 10 nm to 40 nm, and the doped layer includes one or more of boron, fluorine, and indium.
[0017] In some embodiments, the semiconductor structure further includes a barrier layer located between the doped layer and the substrate, the barrier layer comprising carbon.
[0018] In some embodiments, the semiconductor structure further includes an auxiliary doping layer located at the bottom of the isolation trench, the auxiliary doping layer having a thickness greater than that of the doped layer.
[0019] In some embodiments, the isolation structure further includes an auxiliary isolation structure, the auxiliary isolation structure including an auxiliary isolation trench formed at the bottom of the isolation trench and the medium layer located within the auxiliary isolation trench.
[0020] In some embodiments, the isolation trench includes a first isolation trench and a second isolation trench. The first isolation trench is formed between each of the adjacent active regions along a third direction, and the second isolation trench is formed between each of the adjacent active regions along a first direction. The bottom of the second isolation trench has an auxiliary doped layer, the thickness of which is greater than the thickness of the doped layer. The first isolation trench is filled with a first dielectric layer, and the second isolation trench is filled with a second dielectric layer. The first dielectric layer and the second dielectric layer form the isolation structure.
[0021] In some embodiments, the isolation trench includes a first isolation trench and a second isolation trench. The first isolation trench is formed between each of the active regions adjacent in a third direction, and the second isolation trench is formed between each of the active regions adjacent in a first direction. The bottom of the second isolation trench has an auxiliary isolation trench. The second isolation trench and the auxiliary isolation trench are filled with a second dielectric layer, and the first isolation trench is filled with a first dielectric layer. The first dielectric layer and the second dielectric layer form the isolation structure.
[0022] In some embodiments, a portion of the groove is located within the isolation trench, and the ratio of the depth of the groove to the depth of the isolation trench is greater than 78%; or, the ratio of the width of the groove to the width of the isolation trench is less than 40%.
[0023] In this embodiment, the surface of a portion of the isolation trench is doped to form a doped layer. Subsequently, after word lines are formed within the isolation trench, the doped layer increases the hole concentration around the word lines, thereby reducing leakage current caused by the activation of adjacent word lines. Under the same gate voltage, the increased hole concentration makes it more difficult to form an inversion layer, thus hindering the formation of electron channels. Simultaneously, the doped layer surrounding the word line formation region allows for increased word line depth or width, further reducing leakage current.
[0024] Additional aspects and advantages of this disclosure will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this disclosure. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of this disclosure or in the conventional art, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1A flowchart illustrating a method for fabricating a semiconductor structure according to an embodiment of this disclosure;
[0027] Figures 2a-2q This is a schematic diagram of a semiconductor structure during its fabrication process, provided by an embodiment of the present disclosure.
[0028] Figures 3a-3c This is a schematic diagram of the fabrication process of another semiconductor structure provided in this embodiment of the present disclosure;
[0029] Figures 4a-4j This is a schematic diagram of the fabrication process of another semiconductor structure provided in this embodiment of the present disclosure;
[0030] Figures 5a-5c This is a schematic diagram of another semiconductor structure provided in the present disclosure during the fabrication process.
[0031] Figure label:
[0032] 21-Substrate; 22-Protective layer; 23-First mask pattern; 231-First patterned region; 232-Gap between first patterned regions; 24-Isolation trench; 241-First isolation trench; 242-Second isolation trench; 25-Active region; 251-Preset pattern; 26-Doped layer; 27-First sacrificial layer; 28-Opening; 29-Auxiliary doped layer; 30-Dielectric layer; 301-First dielectric layer; 302-Second dielectric layer; 31-Isolation junction Structure; 32-First doped region; 33-Second doped region; 34-Word line mask; 35-Groove; 36-Word line; 361-Conductive material; 37-Word line capping layer; 38-Second sacrificial layer; 39-Auxiliary isolation structure; 391-Auxiliary isolation trench; 40-Second mask pattern; 401-Second pattern area; 402-Gap between second pattern areas; 41-Third mask pattern; 411-Pattern hole; 42-Third sacrificial layer; 43-Fourth sacrificial layer. Detailed Implementation
[0033] Exemplary embodiments of the present disclosure will now be described in more detail with reference to the accompanying drawings. While exemplary embodiments of the present disclosure are shown in the drawings, it should be understood that the present disclosure may be implemented in various forms and should not be limited to the specific embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.
[0034] In the accompanying drawings, for clarity, the dimensions of layers, areas, and elements, as well as their relative dimensions, may be exaggerated. The same reference numerals denote the same elements throughout.
[0035] It should be understood that when an element or layer is referred to as "on," "adjacent to," "connected to," or "coupled to" other elements or layers, it may be directly on, adjacent to, connected to, or coupled to other elements or layers, or there may be intervening elements or layers. Conversely, when an element is referred to as "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or portions, these elements, components, areas, layers, and / or portions should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or portion from another element, component, area, layer, or portion. Therefore, without departing from the teachings of this disclosure, the first element, component, area, layer, or portion discussed below may be referred to as a second element, component, area, layer, or portion. And the discussion of a second element, component, area, layer, or portion does not imply that the first element, component, area, layer, or portion necessarily exists in this disclosure.
[0036] Spatial relation terms such as “below,” “under,” “below,” “under,” “above,” “above,” etc., are used herein for convenience of description to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of the device in use and operation. For example, if the device in the figure is flipped, then the element or feature described as “below,” “under,” or “below” other elements or features will be oriented “above” other elements or features. Therefore, the exemplary terms “below” and “under” can include both above and below orientations. The device may be otherwise oriented (rotated 90 degrees or otherwise) and the spatial descriptive terms used herein will be interpreted accordingly.
[0037] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “comprise” and / or “comprising,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.
[0038] In buried word line memory, word lines exist within the isolation trenches between adjacent memory cells. When the word line adjacent to the target memory cell is activated, the charge in the well region of the transistor corresponding to the target memory cell redistributes under the influence of the high voltage and electric field of the adjacent word line. Near the adjacent word line, minority carrier electrons in the well region accumulate under the influence of the electric field, forming a channel. When different potentials are stored on both sides of this adjacent word line, a voltage difference is created, allowing charge to flow from one side to the other through this channel, resulting in leakage current and causing the loss of the target stored data.
[0039] Based on the above, in order to improve the aforementioned problems, this disclosure provides a method for fabricating a semiconductor structure, see attached figure. Figure 1 The preparation method includes:
[0040] Step 101: Provide a substrate;
[0041] Step 102: Form isolation trenches in the substrate to form a plurality of discrete active regions in the substrate, wherein the projection of the active regions in a direction perpendicular to the substrate plane extends along a first direction;
[0042] Step 103: Doping at least a portion of the surface of the isolation trench to form a doped layer;
[0043] Step 104: Fill the isolation trench with a dielectric layer to form an isolation structure;
[0044] Step 105: Pattern the active region and the isolation structure to form a groove extending along a second direction, wherein the first direction intersects the second direction;
[0045] Step 106: Form letter lines within the groove.
[0046] In this embodiment, the surface of a portion of the isolation trench is doped to form a doped layer. Subsequently, after word lines are formed within the isolation trench, the doped layer increases the hole concentration around the word lines, thereby reducing leakage current. Under the same gate voltage, the increased hole concentration makes it more difficult to equalize the electron concentration and hole concentration on the silicon surface, thus hindering the formation of an inversion layer and electron channels. Simultaneously, the doped layer surrounding the word line formation region allows for an effective increase in the depth or width of the word lines, further reducing leakage current.
[0047] Figures 2a-2q This is a schematic diagram illustrating the fabrication process of a semiconductor structure according to an embodiment of the present disclosure. The fabrication method of the semiconductor structure provided in this embodiment will be further described in detail below with reference to the accompanying drawings. In detailing the embodiments of this disclosure, for ease of explanation, the schematic diagrams may be partially enlarged, deviating from the general scale. Furthermore, the schematic diagrams are merely examples and should not limit the scope of protection of this application.
[0048] First, as attached Figure 2a As shown, step 101 is performed to provide a substrate 21. The substrate 21 may include at least one elemental semiconductor material (e.g., a silicon (Si) substrate, a germanium (Ge) substrate), at least one III-V compound semiconductor material, at least one II-VI compound semiconductor material, at least one organic semiconductor material, or other semiconductor materials known in the art. In one specific embodiment, the substrate 21 is a silicon substrate, which may be doped or undoped.
[0049] Next, as attached Figures 2b-2d As shown, step 102 is performed to form an isolation trench 24 in the substrate to form a plurality of discrete active regions 25 in the substrate 21, the projection of the active regions in the direction perpendicular to the substrate plane extending along a first direction.
[0050] In some embodiments, see Appendix Figure 2b - Appendix Figure 2d The method involves forming isolation trenches in the substrate to form a plurality of discrete active regions in the substrate, including: forming a first mask pattern 23 on the substrate, the first mask pattern 23 having a plurality of first pattern regions 231 spaced apart along a first direction and gaps 232 located between each adjacent first pattern region, wherein the plurality of first pattern regions 231 are simultaneously spaced apart along a third direction; transferring the first mask pattern 23 to the substrate 21, and forming active regions 25 defined by the first pattern regions 231 and isolation trenches 24 defined by the gaps in the substrate 21.
[0051] In some embodiments, see Appendix Figure 2b and attached Figure 2d Before forming the isolation trench 24 in the substrate, a protective layer 22 is formed on the substrate; after forming the protective layer 22, the protective layer 22 and the substrate 21 are etched to form the isolation trench 24, and the unetched protective layer is formed on the active region 25.
[0052] Specifically, first, see the appendix. Figure 2b A protective layer 22 is formed on the substrate. The formation process of the protective layer 22 includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or a combination thereof. The material of the protective layer includes, but is not limited to, nitrides, such as silicon nitride.
[0053] Next, see the appendix. Figure 2c , Figure 2c Figure I in the figure is a top view schematic diagram of the semiconductor structure provided in an embodiment of this disclosure. Figure 2c Figure II in the figure is a cross-sectional view taken along line AA' in Figure I. A first mask pattern 23 is formed on the substrate. The first mask pattern 23 has a plurality of first pattern areas 231 arranged at intervals along a first direction and gaps 232 located between each adjacent first pattern area. The plurality of first pattern areas 231 are arranged at intervals along a third direction.
[0054] Next, see the appendix. Figure 2d The first mask pattern 23 is transferred to the substrate 21, forming an active region 25 defined by the area of the first pattern 231 and an isolation trench 24 defined by the gap. In practice, the protective layer 22 and the substrate 21 are etched to form the isolation trench 24, with the unetched portion of the protective layer 22 formed on the active region 25. The isolation trench 24 can be formed by wet etching, dry etching, or a combination thereof.
[0055] Then, proceed to step 103, see appendix. Figure 2e The surface of at least a portion of the isolation trench 24 is doped to form a doped layer 26.
[0056] In some embodiments, the doped layer is formed using an ion implantation process. The ions used in the ion implantation process include one or more of boron ions, boron difluoride ions, and indium ions. The energy range of the ion implantation process is 1 keV to 30 keV; the thickness of the doped layer ranges from 1 nm to 40 nm. Doping with large-volume ions can prevent excessive ion implantation depth and avoid affecting transistor characteristics. In practice, the energy of the ion implantation process can be, for example, 2 keV, 8 keV, 13 keV, 20 keV, 24 keV, 25.6 keV, or 27 keV. Appropriate energy ensures that ions are distributed only around the isolation trench without affecting the electrical properties of other areas of the substrate. Too low an energy will result in poor isolation, while too high an energy may cause ion diffusion, affecting the electrical properties of other areas of the substrate. In practice, the thickness of the doped layer can be, for example, 2 nm, 10 nm, 15 nm, 18 nm, or 28 nm. An appropriate doped layer thickness can prevent electrical shifts without affecting the concentration in the well region. Too low a thickness will not effectively suppress leakage current, while too high a thickness may affect the electrical characteristics of other areas of the substrate.
[0057] In some embodiments, before the doped layer is formed using an ion implantation process, the method further includes: doping the isolation trench using an ion implantation process to form a barrier layer (not shown in the figure), the barrier layer surrounding the sidewalls and bottom of the isolation trench, the ions used in the ion implantation process including carbon ions. By providing the barrier layer, the diffusion of the doped layer can be prevented, thus preventing it from affecting the electrical characteristics of other areas of the substrate.
[0058] In some embodiments, see Appendix Figure 2f - Appendix Figure 2h After forming the doped layer, the method further includes: forming a first sacrificial layer covering the doped layer on the surface of the isolation trench; etching a portion of the first sacrificial layer; forming an opening in the first sacrificial layer that exposes the bottom of the isolation trench; performing ion doping treatment on the bottom of the isolation trench along the opening; forming an auxiliary doped layer at the bottom of the isolation trench; and removing the first sacrificial layer after forming the auxiliary doped layer.
[0059] Specifically, first, see the appendix. Figure 2f A first sacrificial layer 27 covering the doped layer is formed on the surface of the isolation trench. A portion of the first sacrificial layer 27 is etched to form an opening 28 in the first sacrificial layer 27 exposing the bottom of the isolation trench. The formation process of the first sacrificial layer 27 includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or combinations thereof. The formation process of the opening can be, for example, wet etching, dry etching, or combinations thereof.
[0060] Next, see the appendix. Figure 2g An ion doping process is performed on the bottom of the isolation trench 24 along the opening 28 to form an auxiliary doped layer 29 at the bottom of the isolation trench.
[0061] In some embodiments, the auxiliary doped layer is formed using an ion implantation process. The ions used in the ion implantation process include one or more of boron ions, boron difluoride ions, and indium ions. The energy range of the ion implantation process is 20 keV to 50 keV. The thickness of the auxiliary doped layer ranges from 20 nm to 80 nm. In practice, the energy of the ion implantation process can be, for example, 34 keV, 45.6 keV, or 47 keV. The thickness of the auxiliary doped layer can be, for example, 49 nm, 66 nm, or 78 nm. In other embodiments, the energy range of the ion implantation process forming the auxiliary doped layer is greater than the energy range of the ion implantation process forming the doped layer, and the thickness of the auxiliary doped layer is greater than the thickness of the doped layer. Thus, a relatively shallow doping is used in the upper and middle parts of the isolation trench to reduce the impact of doping on the substrate's electrical properties. Simultaneously, a relatively large dose and high energy secondary doping can be used at the bottom of the isolation trench without affecting the transistor's electrical properties and better avoiding crosstalk between adjacent word lines.
[0062] Next, see the appendix. Figure 2h After forming the auxiliary doped layer 29, the first sacrificial layer 27 is removed.
[0063] Then, proceed to step 104, see appendix. Figure 2i An isolation structure 31 is formed by filling the isolation trench 24 with a dielectric layer 30. The dielectric layer 30 can be filled with the isolation trench 24 using processes such as atomic layer deposition (ALD) or chemical vapor deposition (CVD) to form the isolation structure 31. The material of the dielectric layer 30 includes, but is not limited to, oxides, such as silicon oxide.
[0064] In some embodiments, as shown in the appendix Figure 2j As shown, after filling the isolation trench 24 with dielectric layer 30 to form isolation structure 31, the protective layer 22 on the active region is removed. Here, planarization processes, such as chemical mechanical polishing (CMP) and / or etching processes, can be used to remove the protective layer 22 on the active region.
[0065] In the above scheme, an auxiliary doped layer is formed by secondary doping at the bottom of the isolation trench, thereby further reducing crosstalk between adjacent word lines. It should be understood that the scheme for optimizing the isolation trench is not limited to this; in other embodiments, see the appendix. Figures 3a-3c After forming the doped layer, the method further includes: forming a second sacrificial layer covering the doped layer on the surface of the isolation trench; etching a portion of the second sacrificial layer to form an opening in the second sacrificial layer that exposes the bottom of the isolation trench; etching the substrate along the opening to form an auxiliary isolation trench below the isolation trench; after forming the auxiliary isolation trench, removing the second sacrificial layer and filling the isolation trench and the auxiliary isolation trench with the dielectric layer to form the isolation structure.
[0066] Specifically, first, see the appendix. Figure 2e The surface of at least a portion of the isolation trench 24 is doped to form a doped layer 26.
[0067] Next, see the appendix. Figure 3a A second sacrificial layer 38 is formed on the surface of the isolation trench 24, covering the doped layer 26. A portion of the second sacrificial layer 38 is etched, forming an opening 28 in the second sacrificial layer 38 that exposes the bottom of the isolation trench 24. The formation process of the second sacrificial layer 38 includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or combinations thereof. The formation process of the opening can be, for example, wet etching, dry etching, or combinations thereof.
[0068] Next, see the appendix. Figure 3b The substrate is etched along the opening 28 to form an auxiliary isolation trench 391 below the isolation trench. The formation process of the auxiliary isolation trench 391 can be, for example, wet etching, dry etching, or a combination thereof.
[0069] Next, see the appendix. Figure 3c After forming the auxiliary isolation trench 391, the second sacrificial layer is removed, and the dielectric layer 30 is filled into the isolation trench 24 and the auxiliary isolation trench 391 to form the isolation structure 31. The dielectric layer 30 can be filled into the isolation trench 24 and the auxiliary isolation trench 391 using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD). The material of the dielectric layer 30 includes, but is not limited to, oxides, such as silicon oxide.
[0070] Thus, the insulating properties of the dielectric layer 30 within the auxiliary isolation trench 391 further reduce the obstruction of electronic crosstalk between adjacent word lines. In related technologies, high aspect ratio isolation trenches are difficult to fabricate, and excessively deep etching of the isolation trenches can lead to a smaller active region area, reducing utilization. The embodiments of this disclosure do not affect the active region area during the etching of the auxiliary isolation trench, and compared to methods that form an auxiliary doped layer, they also save one ion doping process.
[0071] The above embodiment is one scheme for performing steps 102, 103, and 104. Specifically, a mask with a complete active region pattern is first formed, and the mask pattern is directly transferred to the substrate to form the active region. An isolation trench is then formed in one step, followed by the formation of a doped layer on the sidewalls of the isolation trench to reduce leakage current and prevent crosstalk between adjacent word lines. It should be understood that the scheme of forming the isolation trench and doping at least a portion of its surface is not limited to this. This disclosure also provides another scheme for performing steps 102, 103, and 104, see appendix. Figure 4a - Appendix Figure 4j Among them, attached Figure 4a - Appendix Figure 4e and appendix Figure 4j Figure I in the diagram is a top view of the semiconductor structure during the fabrication process. Figure 4f-4i and appendix Figure 4j Figure II in the diagram is a cross-sectional schematic diagram of the semiconductor structure during the fabrication process.
[0072] In some embodiments, as shown in the appendix Figure 4a - Appendix Figure 4eAs shown, forming isolation trenches in the substrate to form multiple discrete active regions in the substrate includes: forming a second mask pattern on the substrate, the second mask pattern having multiple second pattern regions extending along a first direction and gaps between adjacent second pattern regions, wherein the second pattern regions are spaced apart along a third direction, the third direction intersecting the first direction; transferring the second mask pattern to the substrate to form multiple preset patterns and a first isolation trench located between the preset patterns in the substrate; filling the first isolation trench with a first dielectric layer; forming a third mask pattern on the substrate, the third mask pattern having multiple discrete pattern holes, each pattern hole being arranged along the third direction, each pattern hole exposing a portion of the preset pattern; transferring the pattern holes to the preset pattern to form a second isolation trench in the preset pattern to define the preset pattern as the active region.
[0073] In some embodiments, as shown in the appendix Figure 4f - Appendix Figure 4j As shown, at least a portion of the surface of the isolation trench is doped to form a doped layer, including: doping the sidewalls and bottom of the second isolation trench to form the doped layer on the surface of the second isolation trench; filling the second isolation trench with a second dielectric layer, wherein the first isolation trench and the second isolation trench form the isolation trench, and the first dielectric layer and the second dielectric layer form the isolation structure.
[0074] Due to the increasing density of integrated circuits, forming isolation trenches in a single step is quite challenging. This disclosure describes a step-by-step method for forming isolation trenches, which reduces the difficulty and cost of patterning processes. Furthermore, by performing necessary doping on the isolation trenches between multiple adjacent active regions in the first direction, leakage current is effectively reduced.
[0075] For details, please see the appendix. Figure 4a First, a second mask pattern 40 is formed on the substrate. The second mask pattern 40 has a plurality of second pattern regions 401 extending along a first direction and gaps 402 located between each adjacent second pattern region. The second pattern regions 401 are arranged at intervals along a third direction, which intersects with the first direction.
[0076] Next, see the appendix. Figure 4b The second mask pattern 40 is transferred to the substrate, forming a plurality of preset patterns 251 and a first isolation trench 241 located between the preset patterns. Here, the first isolation trench 241 can be formed by wet etching, dry etching, or a combination thereof.
[0077] Next, see the appendix. Figure 4cThe first dielectric layer 301 is filled into the first isolation trench 241.
[0078] Then, see appendix. Figure 4d A third mask pattern 41 is formed on the substrate. The third mask pattern has a plurality of discrete pattern holes 411, each pattern hole being arranged along the third direction, and each pattern hole exposing a portion of the preset pattern 251. In actual operation, the portions of the preset pattern 251 exposed by each pattern hole can be arranged in a hexagonal array.
[0079] Next, see Appendix Figure 4e The patterned aperture is transferred into the preset pattern, and a second isolation trench 242 is formed in the preset pattern to define the preset pattern as the active region 25. Here, the second isolation trench 242 can be formed by wet etching, dry etching, or a combination thereof.
[0080] Then, see appendix. Figure 4f The sidewalls and bottom of the second isolation trench 242 are doped to form the doped layer 26 on the surface of the second isolation trench 242.
[0081] In some embodiments, after forming the doped layer, the method further includes: forming a third sacrificial layer covering the doped layer on the surface of the second isolation trench; etching a portion of the third sacrificial layer; forming an opening in the third sacrificial layer that exposes the bottom of the second isolation trench; performing ion doping treatment on the bottom of the second isolation trench along the opening; forming an auxiliary doped layer at the bottom of the second isolation trench; and removing the third sacrificial layer after forming the auxiliary doped layer.
[0082] For details, please see the appendix. Figure 4g A third sacrificial layer 42 covering the doped layer is formed on the surface of the second isolation trench 242. A portion of the third sacrificial layer 42 is etched to form an opening 28 in the third sacrificial layer 42 exposing the bottom of the second isolation trench 242. The formation process of the third sacrificial layer 42 includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or combinations thereof. The formation process of the opening can be, for example, wet etching, dry etching, or combinations thereof.
[0083] Next, see the appendix. Figure 4h An ion doping process is performed on the bottom of the second isolation trench 242 along the opening to form an auxiliary doped layer 29 at the bottom of the second isolation trench 242.
[0084] In some embodiments, the auxiliary doped layer is formed using an ion implantation process. The ions used in the ion implantation process include one or more of boron ions, boron difluoride ions, and indium ions. The energy range of the ion implantation process is 20 keV to 50 keV. The thickness of the auxiliary doped layer ranges from 20 nm to 80 nm. In practice, the energy of the ion implantation process can be, for example, 34 keV, 45.6 keV, or 47 keV. The thickness of the auxiliary doped layer can be, for example, 49 nm, 66 nm, or 78 nm. In other embodiments, the energy range of the ion implantation process for forming the auxiliary doped layer is greater than that of the ion implantation process for forming the doped layer, and the thickness of the auxiliary doped layer is greater than that of the doped layer. Thus, a relatively shallow doping is used in the upper and middle parts of the second isolation trench to reduce the impact of doping on the substrate electrical properties. At the same time, a relatively large dose and high energy secondary doping can be used at the bottom of the second isolation trench without affecting the transistor electrical properties and better avoiding crosstalk between adjacent word lines.
[0085] Then, see appendix. Figure 4i After forming the auxiliary doped layer 29, the third sacrificial layer 42 is removed.
[0086] Next, see Appendix Figure 4j A second dielectric layer 302 is filled into the second isolation trench 242. The first isolation trench 241 and the second isolation trench 242 form the isolation trench 24, and the first dielectric layer 301 and the second dielectric layer 302 form the isolation structure 31. The second dielectric layer 302 can be filled into the isolation trench 24 to form the isolation structure 31 using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD). The material of the second dielectric layer 302 includes, but is not limited to, oxides, such as silicon oxide. In actual operation, the materials of the second dielectric layer 302 and the first dielectric layer 301 can be the same.
[0087] In the above scheme, an auxiliary doped layer is formed by secondary doping at the bottom of the isolation trench, thereby further reducing crosstalk between adjacent word lines. It should be understood that the scheme for optimizing the isolation trench is not limited to this; in other embodiments, see the appendix. Figures 5a-5cAfter forming the doped layer, the method further includes: forming a fourth sacrificial layer covering the doped layer on the surface of the second isolation trench; etching a portion of the fourth sacrificial layer to form an opening in the fourth sacrificial layer that exposes the bottom of the second isolation trench; etching the substrate along the opening to form an auxiliary isolation trench below the second isolation trench; after forming the auxiliary isolation trench, removing the fourth sacrificial layer; and filling the second isolation trench and the auxiliary isolation trench with a second dielectric layer, wherein the first dielectric layer and the second dielectric layer form the isolation structure.
[0088] Specifically, first, see the appendix. Figure 4h The sidewalls and bottom of the second isolation trench 242 are doped, and the doped layer 26 is formed on the surface of the second isolation trench 242.
[0089] Next, see the appendix. Figure 5a A fourth sacrificial layer 43, covering the doped layer 26, is formed on the surface of the second isolation trench 242. A portion of the fourth sacrificial layer 43 is etched to form an opening in the fourth sacrificial layer 43 exposing the bottom of the second isolation trench. The formation process of the fourth sacrificial layer 43 includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or combinations thereof. The formation process of the opening can be, for example, wet etching, dry etching, or combinations thereof.
[0090] Next, see the appendix. Figure 5b The substrate is etched along the opening 28 to form an auxiliary isolation trench 391 below the second isolation trench 242. The formation process of the auxiliary isolation trench 391 can be, for example, wet etching, dry etching, or a combination thereof.
[0091] Then, see appendix. Figure 5c After forming the auxiliary isolation trench 391, the fourth sacrificial layer 43 is removed, and the second dielectric layer 302 is filled into the second isolation trench 242 and the auxiliary isolation trench 391. The first dielectric layer 301 and the second dielectric layer 302 form the isolation structure 31. The second dielectric layer 302 can be filled into the isolation trench 242 and the auxiliary isolation trench 391 using processes such as atomic layer deposition (ALD) and chemical vapor deposition (CVD). The material of the second dielectric layer 302 includes, but is not limited to, oxides, such as silicon oxide. In practice, the material of the first dielectric layer 301 and the material of the second dielectric layer 302 can be the same.
[0092] In some embodiments, as shown in the appendix Figure 2kAs shown, after filling the isolation trench 24 with a dielectric layer 30 to form an isolation structure 31, the method further includes: performing a first doping process on the bottom of the active region to form a first doped region 32 at the bottom of the active region, the isolation trench extending into the first doped region 32 in a direction perpendicular to the substrate plane; performing a second doping process on the active region above the first doped region 32 to form a second doped region 33 above the first doped region 32, the dopant ion type of the second doped region 33 being opposite to the dopant ion type of the first doped region 32. Thus, electrical isolation is achieved by doping the active region, and the distribution of dopant ions is adjusted by regulating the doping process to achieve a better doping effect. Here, the first and second doped regions can be formed by diffusion or ion implantation. In practice, the first doped region 32 can be a P-well (P-type doped region), and the second doped region 33 can be an N-type doped region.
[0093] Next, proceed to step 105, as shown in the attached document. Figure 2l and attached Figure 2m As shown, the active region and the isolation structure are patterned to form a groove extending along a second direction, wherein the first direction intersects the second direction.
[0094] In some embodiments, as shown in the appendix Figure 2l and attached Figure 2m As shown, patterning the active region and the isolation structure to form grooves extending along a second direction includes: forming a word line mask having a plurality of strip patterns extending along a second direction intersecting a first direction; etching the substrate using the word line mask as a mask to form a plurality of grooves extending along the second direction, wherein a portion of the grooves are formed within the isolation trench, and the ratio of the depth of the groove to the depth of the isolation trench is greater than 78%; or, the ratio of the width of the groove to the width of the isolation trench is less than 40%.
[0095] For details, please see the appendix. Figure 2l First, a word line mask 34 is formed, which has multiple strip-shaped patterns extending along a second direction intersecting the first direction. In practice, atomic layer deposition (ALD), chemical vapor deposition (CVD), and other processes can be used to form the word line mask, and the word line mask is patterned to form multiple strip-shaped patterns extending along the second direction intersecting the first direction. The patterning process includes, but is not limited to, self-aligned double patterning (SADP) and self-aligned quadruple patterning (SAQP).
[0096] Next, see the appendix. Figure 2mThe substrate is etched using the word line mask 34 as a mask to form a plurality of grooves 35 extending along the second direction. Some of these grooves 35 are formed within the isolation trench, and the ratio of the groove depth H1 to the isolation trench depth H2 is greater than 78%; or, the ratio of the groove width D1 to the isolation trench width D2 is less than 40%. Here, multiple grooves extending along the second direction can be formed by wet etching, dry etching, or a combination thereof. In practice, the ratio of the groove depth H1 to the isolation trench depth H2 can be, for example, 83%, 86%, or 91%, and the ratio of the groove width D1 to the isolation trench width D2 can be, for example, 23%, 17%, or 15%. Because doping is performed beforehand around the word line formation area, the depth or width of the grooves can be effectively increased, thereby increasing the depth or width of the word lines and further reducing leakage current.
[0097] Finally, see appendix. Figure 2n - Appendix Figure 2q Step 106 is executed to form a letter line 36 in the groove 35.
[0098] In some embodiments, see Appendix Figure 2n - Appendix Figure 2q Forming word lines 36 within the groove 35 includes: filling the groove 35 with conductive material 361; etching back to remove a portion of the conductive material 361; depositing a word line capping layer 37 above the substrate, and planarizing the surface of the word line capping layer 37 to be flush with the surface of the active region, wherein the word line capping layer 37 covers the conductive material 361.
[0099] Specifically, first, see the appendix. Figure 2n The groove 35 is filled with a conductive material 361. The conductive material 361 includes, but is not limited to, tungsten, copper, titanium, tantalum, titanium nitride, tantalum nitride, metal silicide, metal alloy, or any combination thereof. The conductive material 361 can be formed using processes such as chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), physical vapor deposition (PVD), atomic layer deposition (ALD), electroplating, electroless plating, and sputtering.
[0100] Next, see the appendix. Figure 2o The conductive material is removed by etching back. Specifically, the etching back process includes, but is not limited to, wet etching processes, such as etching with a mixture containing ammonium hydroxide and hydrogen peroxide.
[0101] Then, see appendix. Figure 2p and attached Figure 2qA word line capping layer 37 is deposited above the substrate, and planarized such that the surface of the word line capping layer 37 is flush with the surface of the active region. The word line capping layer 37 covers the conductive material. The material of the word line capping layer 37 includes, but is not limited to, nitrides, such as silicon nitride. The formation process of the word line capping layer includes, but is not limited to, chemical vapor deposition (CVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), or combinations thereof.
[0102] In some embodiments, prior to depositing conductive material within the groove to form word lines, the method further includes forming a gate dielectric layer (not shown) on the surface of the groove. The material of the gate dielectric layer includes, but is not limited to, oxides, such as silicon oxide.
[0103] This disclosure also provides a semiconductor structure, see appendix. Figure 2q The semiconductor structure includes: a substrate 21; and an isolation structure 31, including an isolation trench 24 (see attached diagram). Figure 2d The isolation structure 31 defines the substrate as a plurality of discrete active regions 25 (see Appendix) and a dielectric layer 30 located within an isolation trench 24. Figure 2i The active region 25, projected vertically, extends along a first direction; a doped layer 26 is located at least on the sidewall of the isolation trench 24 between adjacent active regions 25 along the first direction; a groove 35 (see attached diagram). Figure 2m The groove 35 extends along a second direction intersecting the first direction and passes through the active region and the isolation structure; the word line 36 is located in the groove 35.
[0104] In some embodiments, the thickness of the doped layer ranges from 10 nm to 40 nm, and the doped layer includes one or more of boron, fluorine, and indium. Doping with large-volume ions can prevent excessive ion implantation depth, avoiding impact on transistor characteristics. In practice, the thickness of the doped layer can be, for example, 15 mm, 18 mm, or 28 mm. A suitable doped layer thickness can prevent electrical shifts without affecting the concentration in the well region; too little thickness will not effectively suppress leakage current, while too much thickness may affect the electrical properties of other areas of the substrate.
[0105] In some embodiments, see Appendix Figure 2q The semiconductor structure further includes an auxiliary doped layer 29, which is located at the bottom of the isolation trench 24. The thickness of the auxiliary doped layer 29 is greater than the thickness of the doped layer 26. The thickness of the auxiliary doped layer can, for example, range from 20 nm to 80 nm. Thus, a low-thickness doped layer does not affect the substrate's electrical properties, and a relatively thick auxiliary doped layer at the bottom of the isolation trench effectively avoids crosstalk between adjacent word lines.
[0106] In some embodiments, see Appendix Figure 3c The isolation structure further includes an auxiliary isolation structure 39, which includes an auxiliary isolation trench 391 formed at the bottom of the isolation trench and a dielectric layer 30 located within the auxiliary isolation trench 391. The insulating properties of the dielectric layer 30 within the auxiliary isolation trench 391 further reduce the obstruction of electronic crosstalk between adjacent word lines.
[0107] In some embodiments, see Appendix Figure 4j The isolation trench includes a first isolation trench 241 and a second isolation trench 242. The first isolation trench 241 is formed between each of the active regions 25 adjacent along a third direction, and the second isolation trench 242 is formed between each of the active regions 25 adjacent along a first direction. The bottom of the second isolation trench 242 has an auxiliary doped layer 29, the thickness of which is greater than the thickness of the doped layer 26. The first isolation trench 241 is filled with a first dielectric layer 301, and the second isolation trench 242 is filled with a second dielectric layer 302. The first dielectric layer 301 and the second dielectric layer 302 form the isolation structure.
[0108] In some embodiments, see Appendix Figure 4j and attached Figure 5c The isolation trench includes a first isolation trench 241 and a second isolation trench 242. The first isolation trench 241 is formed between each of the adjacent active regions 25 along a third direction, and the second isolation trench 242 is formed between each of the adjacent active regions 25 along a first direction. The bottom of the second isolation trench 242 has an auxiliary isolation trench 391 (see Appendix). Figure 5b The second isolation trench 242 and the auxiliary isolation trench 391 are filled with a second dielectric layer 302, and the first isolation trench 241 is filled with a first dielectric layer 301. The first dielectric layer 301 and the second dielectric layer 302 form the isolation structure.
[0109] In some embodiments, the material of the first dielectric layer 301 and the material of the second dielectric layer 302 may be the same.
[0110] In some embodiments, the semiconductor structure further includes a barrier layer (not shown) located between the doped layer and the substrate, the barrier layer comprising carbon. The barrier layer prevents the doped layer from diffusing and thus prevents it from affecting the electrical properties of other areas of the substrate.
[0111] In some embodiments, see Appendix Figure 2qThe active region includes a first doped region 32 and a second doped region 33, with the second doped region 33 located above the first doped region 32. The dopant ion types of the first doped region 32 and the second doped region 33 are opposite. The isolation trench extends into the first doped region 32 along a direction perpendicular to the substrate plane. Thus, doping the active region creates electrical isolation. By adjusting the doping process, the distribution of dopant ions can be controlled to achieve a better doping effect. Here, the first and second doped regions can be formed by diffusion or ion implantation. In practice, the first doped region 32 can be a P-well (P-type doped region), and the second doped region 33 can be an N-type doped region.
[0112] In some embodiments, see Appendix Figure 2q The semiconductor structure further includes a word line capping layer 37, which covers the word line 36 and fills the groove 35.
[0113] In some embodiments, see Appendix Figure 2q and attached Figure 2m Part of the groove is located within the isolation trench, and the ratio of the groove depth H1 to the isolation trench depth H2 is greater than 78%; or, the ratio of the groove width D1 to the isolation trench width D2 is less than 40%. In practice, the ratio of the groove depth H1 to the isolation trench depth H2 can be, for example, 83%, 86%, or 91%, and the ratio of the groove width D1 to the isolation trench width D2 can be, for example, 23%, 17%, or 15%. Because doping is performed beforehand around the word line forming area, the depth or width of the groove can be effectively increased, thereby increasing the depth or width of the word line and further reducing leakage current.
[0114] In some embodiments, the semiconductor structure further includes a gate dielectric layer (not shown) located between the surface of the word line and the groove. The material of the gate dielectric layer includes, but is not limited to, oxides, such as silicon oxide.
[0115] In summary, the embodiments of this disclosure involve doping the surface of a portion of the isolation trench to form a doped layer. Subsequently, after word lines are formed within the isolation trench, the doped layer increases the hole concentration around the word lines, thereby reducing leakage current. Under the same gate voltage, the increased hole concentration makes it more difficult to equalize the electron concentration and hole concentration on the silicon surface, thus hindering the formation of an inversion layer and electron channels. Furthermore, the doped layer surrounding the word line formation region allows for an effective increase in the depth or width of the word lines, further reducing leakage current.
[0116] It should be noted that the semiconductor structure and its fabrication method provided in this disclosure can be applied to any integrated circuit including this structure. The technical features described in each embodiment can be arbitrarily combined without conflict. Those skilled in the art can change the order of the above-described forming method steps without departing from the scope of protection of this disclosure. In the embodiments of this disclosure, some steps can be executed simultaneously or sequentially without conflict.
[0117] The above description is merely a preferred embodiment of this disclosure and is not intended to limit the scope of protection of this disclosure. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this disclosure should be included within the scope of protection of this disclosure.
Claims
1. A method for fabricating a semiconductor structure, characterized in that, include: Provide substrate; Isolation trenches are formed in the substrate to form a plurality of discrete active regions in the substrate, the projection of the active regions in a direction perpendicular to the substrate plane extending along a first direction; The surface of at least a portion of the isolation trenches is doped to form a doped layer; After the doped layer is formed, a dielectric layer is used to fill the isolation trench to form an isolation structure; The active region and the isolation structure are patterned to form a groove extending along a second direction, wherein the first direction intersects the second direction; Character lines are formed within the groove.
2. The preparation method according to claim 1, characterized in that, Isolation trenches are formed in the substrate to form a plurality of discrete active regions in the substrate, including: A first mask pattern is formed on the substrate. The first mask pattern has a plurality of first pattern regions spaced apart along a first direction and gaps between adjacent first pattern regions, wherein the plurality of first pattern regions are simultaneously spaced apart along a third direction. The first mask pattern is transferred into the substrate, where an active region defined by the first patterned area and an isolation trench defined by the gap are formed.
3. The preparation method according to claim 1, characterized in that, Before forming isolation trenches in the substrate, a protective layer is formed on the substrate; after forming the protective layer, the protective layer and the substrate are etched to form the isolation trenches, and the unetched protective layer is formed on the active region.
4. The preparation method according to claim 3, characterized in that, After filling the isolation trench with a dielectric layer to form an isolation structure, the protective layer on the active region is removed.
5. The preparation method according to claim 1, characterized in that, Isolation trenches are formed in the substrate to form a plurality of discrete active regions in the substrate, including: A second mask pattern is formed on the substrate. The second mask pattern has a plurality of second pattern regions extending along a first direction and gaps between adjacent second pattern regions, wherein the second pattern regions are spaced apart along a third direction, which intersects with the first direction. The second mask pattern is transferred into the substrate, and a plurality of preset patterns and a first isolation trench located between the preset patterns are formed in the substrate; The first dielectric layer is filled into the first isolation trench; A third mask pattern is formed on the substrate. The third mask pattern has a plurality of discrete pattern holes, each pattern hole being arranged along the third direction, and each pattern hole exposing a portion of the preset pattern. The patterned hole is transferred into the preset pattern, and a second isolation trench is formed in the preset pattern to define the preset pattern as the active area; At least a portion of the surface of the isolation trenches is doped to form a doped layer, including: The sidewalls and bottom of the second isolation trench are doped to form the doped layer on the surface of the second isolation trench; A second dielectric layer is filled in the second isolation trench, the first isolation trench and the second isolation trench form the isolation trench, and the first dielectric layer and the second dielectric layer form the isolation structure.
6. The preparation method according to claim 2, characterized in that, After the doped layer is formed but before the isolation structure is formed, the process also includes: A first sacrificial layer covering the doped layer is formed on the surface of the isolation trench, a portion of the first sacrificial layer is etched, and an opening is formed in the first sacrificial layer to expose the bottom of the isolation trench; Ion doping is performed on the bottom of the isolation trench along the opening to form an auxiliary doped layer at the bottom of the isolation trench; After the auxiliary doping layer is formed, the first sacrificial layer is removed.
7. The preparation method according to claim 2, characterized in that, After the doped layer is formed but before the isolation structure is formed, the process also includes: A second sacrificial layer covering the doped layer is formed on the surface of the isolation trench, a portion of the second sacrificial layer is etched, and an opening is formed in the second sacrificial layer to expose the bottom of the isolation trench; The substrate is etched along the opening to form an auxiliary isolation trench below the isolation trench; After the auxiliary isolation trench is formed, the second sacrificial layer is removed, and the medium layer is filled into the isolation trench and the auxiliary isolation trench to form the isolation structure.
8. The preparation method according to claim 5, characterized in that, After the doped layer is formed but before the isolation structure is formed, the process also includes: A third sacrificial layer covering the doped layer is formed on the surface of the second isolation trench, a portion of the third sacrificial layer is etched, and an opening is formed in the third sacrificial layer to expose the bottom of the second isolation trench; An ion doping process is performed on the bottom of the second isolation trench along the opening to form an auxiliary doped layer at the bottom of the second isolation trench; After the auxiliary doping layer is formed, the third sacrificial layer is removed.
9. The preparation method according to claim 5, characterized in that, After the doped layer is formed but before the isolation structure is formed, the process also includes: A fourth sacrificial layer covering the doped layer is formed on the surface of the second isolation trench, a portion of the fourth sacrificial layer is etched, and an opening is formed in the fourth sacrificial layer to expose the bottom of the second isolation trench; The substrate is etched along the opening to form an auxiliary isolation trench below the second isolation trench; After the auxiliary isolation trench is formed, the fourth sacrificial layer is removed, and the second dielectric layer is filled in the second isolation trench and the auxiliary isolation trench, wherein the first dielectric layer and the second dielectric layer form the isolation structure.
10. The preparation method according to claim 1, characterized in that, The doped layer is formed by ion implantation, and the ions used in the ion implantation process include one or more of boron ions, boron difluoride ions and indium ions. The energy range of the ion implantation process is 1 KeV~30 KeV. The thickness of the doped layer ranges from 1 nm to 40 nm.
11. The preparation method according to claim 6 or 8, characterized in that, The auxiliary doped layer is formed by ion implantation, and the ions used in the ion implantation process include one or more of boron ions, boron difluoride ions and indium ions. The energy range of the ion implantation process is 20 KeV~50 KeV. The thickness of the auxiliary doped layer ranges from 20 nm to 80 nm.
12. The preparation method according to claim 1, characterized in that, Patterning the active region and the isolation structure to form a groove extending along a second direction includes: A word line mask is formed, the word line mask having a plurality of strip patterns extending along a second direction intersecting the first direction; The substrate is etched using the word line mask to form a plurality of grooves extending along a second direction, wherein some of the grooves are formed within the isolation trench, and the ratio of the depth of the groove to the depth of the isolation trench is greater than 78%; or, the ratio of the width of the groove to the width of the isolation trench is less than 40%.
13. A semiconductor structure, characterized in that, include: Substrate; An isolation structure includes an isolation trench and a dielectric layer located within the isolation trench, the isolation structure defining a substrate as a plurality of discrete active regions, the projection of the active regions in the vertical direction extending along a first direction; A doped layer, at least located on the sidewall of the isolation trench between a plurality of adjacent active regions along a first direction, the doped layer being obtained by doping at least a portion of the surface of the isolation trench; A groove, the groove extending along a second direction intersecting the first direction and passing through the active region and the isolation structure; The letter line is located in the groove.
14. The semiconductor structure according to claim 13, characterized in that, The thickness of the doped layer ranges from 10 nm to 40 nm, and the doped layer includes one or more of boron, fluorine, and indium.
15. The semiconductor structure according to claim 13, characterized in that, It also includes an auxiliary doped layer, which is located at the bottom of the isolation trench, and the thickness of the auxiliary doped layer is greater than the thickness of the doped layer.
16. The semiconductor structure according to claim 13, characterized in that, The isolation structure further includes an auxiliary isolation structure, which includes an auxiliary isolation trench formed at the bottom of the isolation trench and the medium layer located within the auxiliary isolation trench.
17. The semiconductor structure according to claim 13, characterized in that, The isolation trench includes a first isolation trench and a second isolation trench. The first isolation trench is formed between each of the adjacent active regions along a third direction, and the second isolation trench is formed between each of the adjacent active regions along a first direction. The bottom of the second isolation trench has an auxiliary doped layer, the thickness of which is greater than the thickness of the doped layer. The first isolation trench is filled with a first dielectric layer, and the second isolation trench is filled with a second dielectric layer. The first dielectric layer and the second dielectric layer form the isolation structure.
18. The semiconductor structure according to claim 13, characterized in that, The isolation trench includes a first isolation trench and a second isolation trench. The first isolation trench is formed between each of the adjacent active regions along a third direction, and the second isolation trench is formed between each of the adjacent active regions along a first direction. The bottom of the second isolation trench has an auxiliary isolation trench. The second isolation trench and the auxiliary isolation trench are filled with a second dielectric layer, and the first isolation trench is filled with a first dielectric layer. The first dielectric layer and the second dielectric layer form the isolation structure.
19. The semiconductor structure according to claim 13, characterized in that, Part of the groove is located within the isolation trench, and the ratio of the depth of the groove to the depth of the isolation trench is greater than 78%; or, the ratio of the width of the groove to the width of the isolation trench is less than 40%.
Citation Information
Patent Citations
Semiconductor structure and manufacturing method thereof
CN110957318A
Manufacturing method of semiconductor device and semiconductor device
CN111211122A