Semiconductor structure and method of forming the same

By setting a dedicated channel layer structure in the semiconductor structure, the carrier mobility of NMOS and PMOS transistors is improved, solving the problem of insufficient performance in the prior art and achieving a process improvement with high compatibility and low cost.

CN117116854BActive Publication Date: 2026-11-20SEMICON MFG INT (SHANGHAI) CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210528457.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-16
Publication Date
2026-11-20
Estimated Expiration
2042-05-16

AI Technical Summary

Technical Problem

In existing semiconductor structures, the performance of NMOS and PMOS transistors has not yet reached its optimal level, and there is a lack of highly compatible and low-cost methods for forming N-type Si channels and P-type SiGe channels.

Method used

A first channel layer is formed in the P-type region to improve the carrier mobility of the PMOS transistor, and a second channel layer including a central channel film and a sidewall channel film is formed in the N-type region to improve the carrier mobility of the NMOS transistor. These channel layers are formed through specific process steps.

Benefits of technology

It improves the performance of NMOS and PMOS transistors, has high process compatibility and low cost, and achieves performance enhancement for NMOS and PMOS transistors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117116854B_ABST
    Figure CN117116854B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, the method comprising: removing a partial thickness of a first channel layer of an N-type region in a direction parallel to the substrate to form a first trench, the first trench being enclosed by the remaining first channel layer and an adjacent sacrificial layer or by the remaining first channel layer and an adjacent sacrificial layer and a spacer layer; filling a sidewall channel film in the first trench; removing the remaining first channel layer of the N-type region to form a second trench between the sidewall channel film and the adjacent sacrificial layer or between the sidewall channel film and the adjacent sacrificial layer and the spacer layer; and filling a center channel film in the second trench, the center channel film and the sidewall channel film being in contact to form a second channel layer, the second channel layer being used to improve the carrier mobility of an NMOS transistor channel. The embodiments of the present application improve the performance of the semiconductor structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a semiconductor structure and a method for forming the same. Background Technology

[0002] With the rapid development of semiconductor manufacturing technology, semiconductor devices are evolving towards higher component density and higher integration, and semiconductor process nodes are continuously shrinking in accordance with Moore's Law. Transistors, as the most basic semiconductor devices, are currently widely used. Therefore, as the component density and integration of semiconductor devices increase, the channel length of transistors must be continuously shortened to adapt to the shrinking process nodes.

[0003] To better adapt to the requirements of proportionally shrinking device dimensions, semiconductor technology has gradually begun to transition from planar transistors to three-dimensional transistors with higher efficiency, such as gate-all-around (GAA) transistors. In a GAA transistor, the gate surrounds the channel area from all sides. Compared with planar transistors, GAA transistors have stronger control over the channel and can better suppress short-channel effects.

[0004] However, the performance of current semiconductor structures still needs to be improved. Summary of the Invention

[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, which improves the performance of NMOS transistors and PMOS transistors, and has high process compatibility and low process cost.

[0006] To address the aforementioned problems, embodiments of the present invention provide a semiconductor structure, comprising: a substrate including a P-type region for forming a PMOS transistor and an N-type region for forming an NMOS transistor; a plurality of protrusions protruding from the substrate; a first channel structure layer suspended on the protrusions of the P-type region, the first channel structure layer including one or more spaced-apart first channel layers, the first channel layer being used to improve the carrier mobility of the PMOS transistor channel; and a second channel structure layer suspended on the protrusions of the N-type region, the second channel structure layer including one or more spaced-apart second channel layers, the second channel layer including a central channel film and sidewall channel films located on the sidewalls of the central channel film, the second channel layer being used to improve the carrier mobility of the NMOS transistor channel.

[0007] Accordingly, embodiments of the present invention also provide a method for forming a semiconductor structure, comprising: providing a substrate, the substrate including a P-type region for forming a PMOS transistor and an N-type region for forming an NMOS transistor; the substrate including a substrate, a plurality of protrusions protruding from the substrate, one or more sequentially stacked layers located on the protrusions, and a limiting layer located on top of the stack, each of the stacks including a sacrificial layer and a first channel layer located on the sacrificial layer; the first channel layer being used to improve the carrier mobility of the PMOS transistor channel; and removing a portion of the thickness of the first channel layer of the N-type region along a direction parallel to the substrate to form a first trench. The first trench is formed between the remaining first channel layer and an adjacent sacrificial layer, or between the remaining first channel layer and an adjacent sacrificial layer and a limiting layer; a sidewall channel film is filled in the first trench; the remaining first channel layer of the N-type region is removed, so that the sidewall channel film and the adjacent sacrificial layer, or the sidewall channel film and the adjacent sacrificial layer and limiting layer, form a second trench; a central channel film is filled in the second trench, and the central channel film and the sidewall channel film are in contact to form a second channel layer, which is used to improve the carrier mobility of the NMOS transistor channel; after the central channel film is formed, the limiting layer is removed.

[0008] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages: In the semiconductor structure provided by the embodiments of the present invention, a first channel layer for improving the carrier mobility of the PMOS transistor channel is provided in the P-type region, and a second channel layer is provided in the N-type region. The second channel layer includes a central channel film and a sidewall channel film located on the sidewall of the central channel film. The second channel layer is used to improve the carrier mobility of the NMOS transistor channel, which is beneficial to improving the performance of the NMOS transistor and the PMOS transistor. It also has high process compatibility and low process cost.

[0009] In the semiconductor structure formation method provided by this embodiment of the invention, in the step of providing a substrate, the first channel layer is used to improve the carrier mobility of the PMOS transistor channel; then, along a direction parallel to the substrate, a portion of the thickness of the first channel layer in the N-type region is removed to form a first trench, and a sidewall channel film is filled in the first trench. Subsequently, the remaining first channel layer in the N-type region is removed to form a second trench, and a central channel film is filled in the second trench. The central channel film and the sidewall channel film are in contact to form a second channel layer. The second channel layer is used to improve the carrier mobility of the NMOS transistor channel. Thus, this embodiment of the invention forms both a first channel layer in the P-type region to improve the carrier mobility of the PMOS transistor channel and a second channel layer in the N-type region to improve the carrier mobility of the NMOS transistor channel, which is beneficial to improving the performance of both NMOS and PMOS transistors, and has high process compatibility and low process cost. Attached Figure Description

[0010] Figure 1 This is a schematic diagram of a semiconductor structure according to an embodiment of the present invention; Figures 2 to 19 This is a schematic diagram of the structure corresponding to each step in one embodiment of the semiconductor structure formation method of the present invention. Detailed Implementation

[0011] As can be seen from the background technology, the performance of current semiconductor structures still needs to be improved.

[0012] Specifically, for N-type GAA transistors, using Si as the channel layer material is beneficial for improving the carrier mobility of the N-type GAA transistor channel; for P-type GAA transistors, using SiGe as the channel layer material is beneficial for improving the carrier mobility of the P-type GAA transistor channel.

[0013] However, there is currently no publicly available method for simultaneously forming N-type Si channels and P-type SiGe channels with low process costs.

[0014] To address the technical issues, the semiconductor structure provided in this embodiment of the invention includes a first channel layer in the P-type region for improving the carrier mobility of the PMOS transistor channel, and a second channel layer in the N-type region. The second channel layer includes a central channel film and a sidewall channel film located on the sidewall of the central channel film. The second channel layer is used to improve the carrier mobility of the NMOS transistor channel, which is beneficial to improving the performance of both NMOS and PMOS transistors. Furthermore, it offers high process compatibility and low process cost.

[0015] To make the above-mentioned objects, features, and advantages of the embodiments of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. (Reference) Figure 1The diagram shows a schematic representation of an embodiment of the semiconductor structure of the present invention.

[0016] like Figure 1 As shown, in this embodiment, the semiconductor structure includes: a substrate 100, which includes a P-type region 100P for forming a PMOS transistor and an N-type region 100N for forming an NMOS transistor; a plurality of protrusions 110 protruding from the substrate 100; a first channel structure layer 250 suspended on the protrusions 110 of the P-type region 100P, the first channel structure layer 250 including one or more first channel layers 22 spaced apart and suspended, the first channel layers 22 being used to improve the carrier mobility of the PMOS transistor channel; and a second channel structure layer 260 suspended on the protrusions 110 of the N-type region 100N, the second channel structure layer 260 including one or more second channel layers 30 spaced apart and suspended, the second channel layer 30 including a central channel film 24 and sidewall channel films 23 located on the sidewalls of the central channel film 24, the second channel layer 30 being used to improve the carrier mobility of the NMOS transistor channel.

[0017] The substrate 100 is used to provide a process platform for subsequent processes. In this embodiment, the substrate 100 is used to provide a process platform for forming a gate-all-around (GAA) transistor (i.e., a gate-all-around transistor).

[0018] In this embodiment, the substrate 100 is a silicon substrate, that is, the material of the substrate 100 is single-crystal silicon. In other embodiments, the substrate material may also be one or more of germanium, silicon germanide, silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride. The substrate may also be other types of substrates such as silicon-on-insulator substrates or germanium-on-insulator substrates.

[0019] In this embodiment, the protrusion 110 and the substrate 100 are an integral structure, and the protrusion 110 and the substrate 100 are made of the same material, silicon. In other embodiments, the material of the protrusion may be different from that of the substrate. The material of the protrusion may be other suitable materials, such as one or more of germanium, silicon germanide, silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride.

[0020] In this embodiment, the semiconductor structure further includes an isolation layer 210 located on the substrate 100 and surrounding the protrusion 110. The isolation layer 210 exposes a first channel structure layer 250 and a second channel structure layer 260.

[0021] The isolation layer 210 is used to isolate adjacent protrusions 110 and also to isolate the substrate 100 from the gate structure. In this embodiment, the material of the isolation layer 210 is silicon oxide. The material of the isolation layer 210 can also be other insulating materials, such as one or more of silicon oxide, silicon nitride, silicon oxynitride, and silicon germanium oxide.

[0022] As an example, the top surface of the insulating layer 210 is flush with the top surface of the protrusion 110. In other embodiments, the top surface of the insulating layer may be lower than the top surface of the protrusion.

[0023] In this embodiment, the semiconductor structure further includes a pad layer 125 located between the protrusion 110 and the isolation layer 210 and between the substrate 100 and the isolation layer 210.

[0024] The padding layer 125 is used to improve the adhesion between the protrusion 110 and the isolation layer 210, and between the substrate 100 and the isolation layer 210. In this embodiment, the material of the padding layer 125 is silicon oxide.

[0025] The first channel structure layer 250 is used to provide a conductive channel for the PMOS transistor. Specifically, the first channel layer 22 is used to provide a conductive channel for the PMOS transistor.

[0026] In this embodiment, the stacking direction of the first channel layer 22 is perpendicular to the surface of the substrate 100.

[0027] As an example, in the first channel structure layer 250, the number of first channel layers 22 is three. In other embodiments, the number of first channel layers may also be other, such as two, four, five, etc.

[0028] In this embodiment, to improve the performance of the PMOS transistor, SiGe channel technology can be used, and the material of the first channel layer 22 is silicon germanide. As an example, the molar percentage of germanium in the first channel layer 22 is 5% to 25%.

[0029] In other embodiments, the material of the first channel layer may also be other materials that can improve the carrier mobility of the PMOS transistor channel, for example, the material of the first channel layer may also be one or more of germanium, gallium nitride, gallium arsenide and indium gallium nitride.

[0030] The second channel structure layer 260 is used to provide a conductive channel for the NMOS transistor. Specifically, the second channel layer 30 is used to provide a conductive channel for the NMOS transistor.

[0031] In this embodiment, the stacking direction of the second channel layer 30 is perpendicular to the surface of the substrate 100.

[0032] As an example, in the second channel structure layer 260, the number of second channel layers 30 is three. In other embodiments, the number of second channel layers may also be other, such as two, four, five, etc.

[0033] In this embodiment, the material of the second channel layer 30 is silicon to improve the performance of the NMOS transistor. In other embodiments, the material of the second channel layer can also be other materials that can improve the carrier mobility of the NMOS transistor channel, such as one or more of silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride.

[0034] The central channel membrane 24 and the sidewall channel membrane 23 are used to form the second channel layer 30.

[0035] The sidewall channel membrane 23 serves to provide support during the formation of the central channel membrane 24.

[0036] In this embodiment, the material of the central channel film 24 is the same as that of the sidewall channel film 23, which is beneficial to improving process compatibility and allows the second channel layer 30 to contain only one material, which is beneficial to improving the formation and quality of the second channel layer 30, thereby improving the performance of the PMOS transistor.

[0037] In this embodiment, the materials of the central channel film 24 and the sidewall channel film 23 include silicon. In other embodiments, the central channel film and the sidewall channel film can also be other materials capable of improving the carrier mobility of the NMOS transistor channel. In still other embodiments, the materials of the central channel film and the sidewall channel film can also be different.

[0038] In this embodiment, the thickness of the sidewall channel film 23 along the direction parallel to the substrate 100 is 1 nanometer to 10 nanometers.

[0039] In this embodiment, the semiconductor structure further includes: a first gate structure 230, which spans the first channel structure layer 250 and fills the space between adjacent first channel layers 22 and between the protrusion 110 of the P-type region 100P and the first channel layer 22, and the first gate structure 230 surrounds the first channel layer 22; and a first source / drain doped region (not shown), which is located on both sides of the first gate structure 230 and contacts the end of the first channel layer 22.

[0040] The first gate structure 230 is used to control the opening and closing of the conductive channel of the PMOS transistor.

[0041] In this embodiment, the first gate structure 230 is a metal gate structure. The first gate structure 230 includes a first gate dielectric layer (not shown) and a first gate electrode layer (not shown) located on the first gate dielectric layer. The first gate dielectric layer is used to isolate the first gate electrode layer from the first channel layer 22.

[0042] The first source / drain doped region is used as the source or drain of the PMOS transistor. When the PMOS transistor is working, the first source / drain doped region is used to provide a source of charge carriers.

[0043] In this embodiment, the first source / drain doped region includes a stress layer doped with ions. This stress layer provides stress to the channel region, thereby improving carrier mobility. In this embodiment, the first source / drain doped region includes a stress layer doped with p-type ions, and the stress layer is made of Si or SiGe.

[0044] The second gate structure 240 is used to control the opening and closing of the conductive channel of the NMOS transistor.

[0045] In this embodiment, the second gate structure 240 is a metal gate structure, which includes a second gate dielectric layer (not shown) and a second gate electrode layer (not shown) located on the second gate dielectric layer. The second gate dielectric layer is used to isolate the second gate electrode layer and the second channel layer 30.

[0046] In this embodiment, the semiconductor structure further includes: a second gate structure 240, which spans the second channel structure layer 260 and fills the space between adjacent second channel layers 30 and between the protrusion 110 of the N-type region 100N and the second channel layer 30, and the second gate structure 240 surrounds the second channel layer 30; and a second source / drain doped region (not shown), which is located on both sides of the second gate structure 240 and contacts the end of the second channel layer 30.

[0047] The second source / drain doped region is used as the source or drain of the NMOS transistor. When the NMOS transistor is operating, the second source / drain doped region provides a carrier source. In this embodiment, the second source / drain doped region includes a stress layer doped with N-type ions, and the stress layer is made of Si or SiC.

[0048] Accordingly, the present invention also provides a method for forming a semiconductor structure. Figures 2 to 19 This is a schematic diagram of the structure corresponding to each step in one embodiment of the semiconductor structure formation method of the present invention. The semiconductor structure formation method of this embodiment will be described in detail below with reference to the accompanying drawings.

[0049] refer to Figure 2 A substrate 10 is provided, including a P-type region 100P for forming a PMOS transistor and an N-type region 100N for forming an NMOS transistor. The substrate 10 includes a substrate 100, a plurality of protrusions 110 protruding from the substrate 100, one or more stacked layers 120 located on the protrusions 110, and a limiting layer 130 located on top of the stacked layers 120. Each stacked layer 120 includes a sacrificial layer 21 and a first channel layer 22 located on the sacrificial layer 21. The first channel layer 22 is used to improve the carrier mobility of the PMOS transistor channel.

[0050] The substrate 10 is used to provide a process platform for subsequent processes. In this embodiment, the substrate 10 is used to provide a process platform for forming a gate-all-around (GAA) transistor (i.e., a gate-all-around transistor).

[0051] In this embodiment, the substrate 100 is a silicon substrate. In other embodiments, the substrate material may also be one or more of germanium, silicon germanide, silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride. The substrate may also be other types of substrates such as silicon-on-insulator substrates or germanium-on-insulator substrates.

[0052] In this embodiment, the protrusion 110 and the substrate 100 are an integral structure, and the protrusion 110 and the substrate 100 are made of the same material, silicon. In other embodiments, the material of the protrusion may be different from that of the substrate. The material of the protrusion may be other suitable materials, such as one or more of germanium, silicon germanide, silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride.

[0053] The stack 120 provides a process basis for the subsequent formation of a first channel layer 22 with suspended space separation in the P-type region 100P and a second channel layer with suspended space separation in the N-type region 100N.

[0054] Specifically, the first channel layer 22 is used to provide a conductive channel for the field-effect transistor, and the sacrificial layer 21 is used to support the first channel layer 22, thereby providing a process basis for the subsequent implementation of the spaced floating arrangement of the first channel layer 22. The sacrificial layer 21 is also used to occupy space for the subsequent formation of the gate structure.

[0055] In this embodiment, the material of the first channel layer 22 includes silicon germanide, the material of the sacrificial layer 21 includes silicon germanide, and the molar percentage of germanium in the sacrificial layer 21 is greater than the molar percentage of germanium in the first channel layer 22.

[0056] The material of the first channel layer 22 includes silicon germanide, which is beneficial for improving the carrier mobility of the PMOS transistor channel. In other embodiments, the material of the first channel layer may also be other materials that can improve the carrier mobility of the PMOS transistor channel, such as one or more of germanium, gallium nitride, gallium arsenide, and indium gallium nitride.

[0057] The molar percentage of germanium in the sacrificial layer 21 is greater than that in the first channel layer 22, which results in an etching selectivity between the materials of the sacrificial layer 21 and the first channel layer 22. This reduces the probability of damage to the first channel layer 22 in the subsequent removal of the sacrificial layer 21, thereby improving the channel layer quality of the PMOS transistor and consequently improving the performance of the PMOS transistor.

[0058] The molar percentage of germanium in the first channel layer 22 should not be too low or too high. If the molar percentage of germanium in the first channel layer 22 is too low, the effect of improving the carrier mobility of the PMOS transistor channel will not be significant. If the molar percentage of germanium in the first channel layer 22 is too high, the difference between the molar percentage of germanium in the first channel layer 22 and the sacrificial layer 21 will be too small, resulting in a low etching selectivity between the first channel layer 22 and the sacrificial layer 21, which will increase the probability of damage to the first channel layer 22 during the subsequent removal of the sacrificial layer 21. Therefore, in this embodiment, the molar percentage of germanium in the first channel layer 22 is 5% to 25%.

[0059] The molar percentage of germanium in the sacrificial layer 21 should not be too low or too high. If the molar percentage of germanium in the sacrificial layer 21 is too low, the difference between the molar percentage of germanium in the sacrificial layer 21 and the first channel layer 22 will be too small, making it difficult to increase the etching selectivity between the sacrificial layer 21 and the first channel layer 22. If the molar percentage of germanium in the sacrificial layer 21 is too high, it will increase the difficulty of forming the sacrificial layer 21. Therefore, in this embodiment, the molar percentage of germanium in the sacrificial layer 21 is 30% to 50%.

[0060] In this embodiment, there are multiple stacks 120, and the stacking direction of the multiple stacks 120 is perpendicular to the surface of the substrate 100. As an example, there are three stacks 120. In other embodiments, there may be other numbers of stacks, such as two, four, five, etc.

[0061] The limiting layer 130 is used to define the location for the formation of the second channel layer in the future.

[0062] In this embodiment, the limiting layer 130 and the sacrificial layer 21 are made of the same material, which is beneficial for improving process compatibility. In other embodiments, the material of the limiting layer may be different from that of the sacrificial layer.

[0063] Continue to refer to Figure 2 The forming method further includes forming a first pad layer 125 on the top of the substrate 100, the sidewall of the protrusion 110, the sidewall of the stack 120, and the top surface and sidewall of the limiting layer 130.

[0064] The first padding layer 125 serves to protect the stack 120 in subsequent process steps and also improves the adhesion between the protrusion 110 and the substrate 100 and the subsequent isolation layer.

[0065] In this embodiment, the material of the first liner layer 125 includes silicon oxide.

[0066] refer to Figures 3 to 4After providing the substrate 10, the forming method further includes: forming a first cover film 145 around the protrusion 110 on the substrate 100, the first cover film 145 covering the sidewalls of the stack 120 located in the P-type region 100P and the sidewalls and top of the limiting layer 130, and exposing the stack 120 and the limiting layer 130 located in the N-type region 100N.

[0067] The first cover film 145 is used to protect the P-type region 100P during the subsequent removal of a portion of the thickness of the first channel layer 22 of the N-type region 100N in a direction parallel to the substrate 100, and during the formation of the sidewall channel film.

[0068] In this embodiment, the material of the first cover film 145 is a dielectric material so that the material of the first cover film 145 can be retained for use as an insulating layer. As an example, the material of the first cover film 145 includes one or more of silicon oxide, silicon nitride, and silicon oxynitride.

[0069] Specifically, in this embodiment, the step of forming the first covering film 145 includes: like Figure 3 As shown, an initial cover film 140 is formed on the substrate 100 surrounding the protrusion 110, the stack 120, and the limiting layer 130. The initial cover film 140 also covers the top of the limiting layer 130. Specifically, the initial cover film 140 covers the first pad layer 125.

[0070] Subsequently, a portion of the initial cover film 140 of thickness located in the N-type region 100N is removed, and the remaining initial cover film 140 is used as the first cover film 145.

[0071] As an example, a flow-through chemical vapor deposition (FCVD) process is used to form the initial capping film 140. The FCVD process has a high gap-filling capability, which is beneficial for improving the filling and quality of the initial capping film 140 between the stacks 120 and between the protrusions 110.

[0072] like Figure 4 As shown, a portion of the initial cover film 140 of the thickness located in the N-type region 100N is removed, and the remaining initial cover film 140 is used as a first cover film 145, which exposes the stack 120 and the limiting layer 130 of the N-type region 100N.

[0073] Specifically, in this embodiment, the first pad layer 125 located in the N-type region 100N is used as the stop position to remove the initial cover film 140 of a certain thickness located in the N-type region 100N. This helps to reduce the probability of the process of removing the initial cover film 140 of a certain thickness located in the N-type region 100N causing mis-etching of the stack 120 of the N-type region 100N.

[0074] Correspondingly, the first cover film 145 exposes the first padding layer 125 of the N-type region 100N.

[0075] Therefore, in this embodiment, after removing the initial cover film 140 of a portion thickness located in the N-type region 100N, and before removing the first channel layer 22 of a portion thickness of the N-type region 100N in a direction parallel to the substrate 100, the method for forming the semiconductor structure further includes: removing the sidewalls of the stack 120 located in the N-type region 100N, and the first pad layer 125 on the top surface and sidewalls of the limiting layer 130, thereby exposing the stack 120 of the N-type region 100N.

[0076] Specifically, an isotropic etching process (e.g., wet etching) is used to remove the first pad layer 125 on the sidewalls of the stack 120 located in the N-type region 100N, as well as on the top surface and sidewalls of the limiting layer 130. The first pad layer 125 has a relatively small thickness; therefore, the etching process for removing the first pad layer 125 on the sidewalls of the stack 120 located in the N-type region 100N, as well as on the top surface and sidewalls of the limiting layer 130, is simple and has high process compatibility.

[0077] refer to Figure 5 Along a direction parallel to the substrate 100, a portion of the thickness of the first channel layer 22 of the N-type region 100N is removed to form a first trench 150. The first trench 150 is formed between the remaining first channel layer 22 and the adjacent sacrificial layer 21, or between the remaining first channel layer 22 and the adjacent sacrificial layer 21 and the limiting layer 130. The first trench 150 provides space for the subsequent formation of the sidewall channel film.

[0078] It should be noted that the removal thickness of the first channel layer 22 of the N-type region 100N along the direction parallel to the substrate 100 should not be too small or too large. If the removal thickness is too small, the size of the first trench 150 along the direction parallel to the substrate 100 will be too small, and the thickness of the sidewall trench film subsequently formed in the first trench 150 will also be too small. This will easily increase the probability that the sidewall trench film will be completely consumed during the subsequent removal of the remaining first trench layer 22 of the N-type region 100N. If the removal thickness is too large, the size of the remaining first trench layer 22 of the N-type region 100N will be too small, which will easily lead to the mechanical strength of the remaining first trench layer 22 of the N-type region 100N being too low. This will easily increase the probability that the sacrificial layer 21 of the N-type region 100N will collapse, and will also easily increase the process difficulty of the subsequent removal of the remaining first trench layer 22 of the N-type region 100N. Furthermore, if the size of the second trench formed by the subsequent removal of the remaining first trench layer 22 of the N-type region 100N is too small, it will easily increase the process difficulty of the subsequent formation of the central trench film in the second trench. Therefore, in this embodiment, the removal thickness of the first channel layer 22 of the N-type region 100N along the direction parallel to the substrate 100 is 1 nanometer to 10 nanometers.

[0079] In this embodiment, an isotropic etching process is used to remove a portion of the thickness of the first channel layer 22 of the N-type region 100N along a direction parallel to the substrate 100. The isotropic etching process has the characteristics of isotropic etching, thereby enabling the etching of the first channel layer 22 of the N-type region 100N along a direction parallel to the substrate 100.

[0080] refer to Figure 6 The first groove 150 is filled with a sidewall channel membrane 23.

[0081] The sidewall trench membrane 23 is used to subsequently form a second trench layer with the central trench membrane, and also to define the formation position of the central trench membrane during the subsequent formation of the central trench membrane. In addition, the sidewall trench membrane 23 also serves to support the sacrificial layer 21 located in the N-type region 100N during the subsequent removal of the remaining first trench layer 22 in the N-type region 100N and the formation of the central trench membrane, thereby preventing the sacrificial layer 21 from collapsing or tilting, and thus ensuring the formation of the second trench layer.

[0082] Accordingly, the sidewall channel film 23 is made of a material that can improve the carrier mobility of the NMOS transistor channel. As an example, the material of the sidewall channel film 23 is silicon, which not only improves the carrier mobility of the NMOS transistor channel, but also reduces process costs and improves process compatibility.

[0083] In other embodiments, the material of the sidewall channel film may also be other materials that can improve the carrier mobility of the NMOS transistor channel, such as silicon carbide, gallium nitride, gallium arsenide and indium gallium nitride.

[0084] In this embodiment, the process of filling the sidewall channel membrane 23 in the first trench 150 includes an epitaxial process. Specifically, in this embodiment, the step of forming the sidewall channel membrane 23 includes: using an epitaxial process, epitaxially growing a first channel epitaxial layer (not shown) inside and outside the first trench 150, the first channel epitaxial layer also being formed on the sidewall of the sacrificial layer 21 in the N-type region 100N, and on the top and sidewall of the limiting layer 130; removing the first channel epitaxial layer located on the sidewall of the sacrificial layer 21 and the limiting layer 130 in the N-type region 100N, the remaining first channel epitaxial layer located in the first trench 150 being used as the sidewall channel membrane 23.

[0085] In this embodiment, a combination of isotropic and anisotropic etching processes is used to remove the first channel epitaxial layer on the sidewalls of the sacrificial layer 21 and the limiting layer 130 located in the N-type region 100N. The isotropic etching process is used to reduce the size of the first channel epitaxial layer along a direction parallel to the substrate 100, while the anisotropic etching process is used to make the sidewalls of the remaining first channel epitaxial layer flush with the sidewalls of the sacrificial layer 21.

[0086] It should be noted that, in this embodiment, during the process of forming the sidewall channel film 23 using an epitaxial process, a sacrificial channel film 25 is also formed on top of the limiting layer 130 in the N-type region 100N. Specifically, in the step of removing the first channel epitaxial layer located on the sidewall of the sacrificial layer 21 in the N-type region 100N, a portion of the thickness of the first channel epitaxial layer located on top of the limiting layer 130 in the N-type region 100N is retained as the sacrificial channel film 25.

[0087] Reference Figures 7 to 9 , Figure 8 yes Figure 7 A sectional view along the xx direction. Figure 9 Based on Figure 8 The cross-sectional view shows that after forming the sidewall channel membrane 23, the forming method further includes: forming a cutting groove 270 of the limiting layer 130, the sacrificial layer 21, and the first channel layer 22 along the extension direction of the protrusion 110 on the N-type region 100N, thereby exposing the first channel layer 22 of the N-type region 100N.

[0088] A cutting groove 170 is formed to disconnect the limiting layer 130, the sacrificial layer 21, the first channel layer 22, and the protrusion 110 at the desired location to form the active region pattern of the N-type region 100N. Furthermore, the cutting groove 170 exposes the first channel layer 22 of the N-type region 100N for subsequent removal of the remaining first channel layer 22 of the N-type region 100N.

[0089] It should be noted that, in this embodiment, after forming the sidewall channel film 23 and before forming the cleavage groove 170, the method for forming the semiconductor structure further includes: forming a filling layer 165 located in the N-type region 100N, wherein the filling layer 165 covers the sidewalls of the sidewall channel film 23 and the sacrificial layer 21, as well as the sidewalls and top of the limiting layer 130. Specifically, the filling layer 165 is formed on the first cover film 145 of the N-type region.

[0090] The filler layer 165 is used to provide a flat surface for subsequent processing steps.

[0091] In this embodiment, the filler layer 165 is made of a dielectric material. Therefore, after removing the remaining first channel layer 22 of the N-type region 100N and forming the central channel film, it is not necessary to remove the remaining filler layer 165, which simplifies the process steps. As an example, the filler layer 165 may be made of one or more of silicon oxide, silicon nitride, and silicon oxynitride.

[0092] In this embodiment, a flow-through chemical vapor deposition process is used to form the filler layer 165.

[0093] In other embodiments, the filler layer material can also be spin-on carbon (SOC). Accordingly, a spin coating process is used to form the filler layer. The spin coating process is simple, has low processing cost, and is beneficial for improving the flatness of the top surface of the filler layer.

[0094] Accordingly, in the step of forming the cutting groove 170, the cutting groove 170 also penetrates the filling layer 165 of the N-type region 100N along the extending direction perpendicular to the protrusion 110.

[0095] It should be noted that, in this embodiment, after forming the sidewall channel film 23 and before forming the filling layer 165, the method for forming the semiconductor structure further includes: forming a second pad layer 155 on the sidewall of the N-type region sidewall channel film 23 and the sidewall of the sacrificial layer 21 limiting layer.

[0096] The second liner layer 155 is used to protect the sidewall channel membrane 23 of the N-type region 100N. As an example, the material of the second liner layer 155 includes one or more of silicon, silicon oxide, silicon nitride, and silicon oxynitride.

[0097] refer to Figure 10 and Figure 11 , Figure 11 yes Figure 10 A cross-sectional view along the xx direction shows the removal of the remaining first channel layer 22 in the N-type region 100N, so that the sidewall channel membrane 23 and the adjacent sacrificial layer 21, or the sidewall channel membrane 23 and the adjacent sacrificial layer 21 and the limiting layer 130, form a second trench 160.

[0098] The second trench 160 provides space for the formation of the central trench membrane and also defines the formation area of ​​the central trench membrane. In the step of forming the second trench 160, the sidewall trench membrane 23 serves as a support to prevent the sacrificial layer 21 from collapsing or tilting.

[0099] Specifically, in this embodiment, by removing the remaining first channel layer 22 located in the N-type region 100N through the sidewall of the first channel layer 22 exposed by the cutting groove 170, the process of forming the cutting groove 170 and removing the remaining first channel layer 22 located in the N-type region 100N can be integrated, which is beneficial to improving the process integration and process compatibility, and also simplifies the process steps and reduces the process cost.

[0100] In this embodiment, an isotropic etching process is used to remove the remaining first channel layer 22 of the N-type region 100N. The isotropic etching process has the characteristics of isotropic etching, which makes it easy to remove the remaining first channel layer 22 located in the N-type region 100N.

[0101] refer to Figure 12 and Figure 13 , Figure 13 yes Figure 12 A cross-sectional view along the xx direction shows that the second trench 160 is filled with a central channel film 24, and the central channel film 24 and the sidewall channel film 23 are in contact to form a second channel layer 30. The second channel layer 30 is used to improve the carrier mobility of the NMOS transistor channel.

[0102] The central channel film 24 and the sidewall channel film 23 are in contact to form a second channel layer 30. The second channel layer 30 is used to improve the carrier mobility of the NMOS transistor channel. Thus, in this embodiment, a first channel layer 22 for improving the carrier mobility of the PMOS transistor channel is formed in the P-type region 100P, and a second channel layer 30 for improving the carrier mobility of the NMOS transistor channel is formed in the N-type region 100N. This is beneficial to improving the performance of the NMOS transistor and the PMOS transistor, and has high process compatibility and low process cost.

[0103] In this embodiment, the material of the central channel film 24 is the same as that of the sidewall channel film 23, which is beneficial to improve process compatibility and makes the second channel layer 30 the same material, which is beneficial to improve the formation and quality of the second channel layer 30, thereby improving the performance of the PMOS transistor.

[0104] In this embodiment, the material of the central channel film 24 includes silicon. In other embodiments, the central channel film may also be made of other materials capable of improving the carrier mobility of the NMOS transistor channel. In still other embodiments, the material of the central channel film may also be other materials capable of improving the carrier mobility of the NMOS transistor channel, for example, the material of the central channel film may also be one or more of silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride.

[0105] In other embodiments, the materials of the central channel membrane and the sidewall channel membrane may also be different.

[0106] In this embodiment, the material of the second channel layer 30 has a high etching selectivity ratio with the material of the sacrificial layer 21, thereby reducing the probability of damage to the second channel layer 30 in the subsequent step of removing the sacrificial layer 21, thus ensuring the quality of the second channel layer 30 and improving the performance of the NMOS transistor accordingly.

[0107] In this embodiment, the process of filling the central channel membrane 24 in the second trench 160 includes an epitaxial process. Specifically, the step of forming the central channel membrane 24 includes: using an epitaxial process to form a second channel epitaxial layer (not shown) in the second trench 160, the second channel epitaxial layer also being formed on the sidewalls of the sacrificial layer 21, the limiting layer 130, and the sacrificial channel membrane 25 exposed in the cutting groove 170; removing the second channel epitaxial layer located on the sidewalls of the sacrificial layer 21, the limiting layer 130, and the sacrificial channel membrane 25, leaving the remaining second channel epitaxial layer in the second trench 160 as the central channel membrane 24.

[0108] In this embodiment, a combination of isotropic and anisotropic etching is used to remove the second channel epitaxial layer located on the sidewall of the sacrificial layer 21. The isotropic etching is used to perform lateral etching of the second channel epitaxial layer along a direction parallel to the substrate 100, while the anisotropic etching process is used to make the sidewall of the remaining second channel epitaxial layer flush with the sidewall of the sacrificial layer 21.

[0109] In this embodiment, after the second channel layer 30 is formed, the sacrificial layer 21 located in the P-type region 100P and the adjacent first channel layer 22 located on the sacrificial layer 21 are used to form a first channel stack (not shown), and the sacrificial layer 21 located in the N-type region 100N and the adjacent second channel layer 30 located on the sacrificial layer 21 are used to form a second channel stack (not shown).

[0110] In this embodiment, the sacrificial layer 21 in the first trench stack and the second trench stack is the same, thereby avoiding the introduction of additional sacrificial layer 21 material, which in turn helps to improve process compatibility.

[0111] It should be noted that in this embodiment, a first channel layer 22 for improving the carrier mobility of the PMOS transistor channel is formed in the P-type region 100P, and a second channel layer 30 for improving the carrier mobility of the NMOS transistor channel is formed in the N-type region 100N. No additional photomask is required, thereby improving the performance of both NMOS and PMOS transistors, while also improving process compatibility and saving process costs.

[0112] refer to Figure 14 This shows that based on Figure 13The cross-sectional view shows that after forming the central channel film 24, the method of forming the semiconductor structure further includes: forming a second cover film 180 filled in the cut groove 170, the second cover film 180, the fill layer 165, and the first cover film 145 forming the cover layer 190.

[0113] The cover layer 190 is used to protect the first channel layer 22 and the second channel layer 30 in the subsequent step of removing the limiting layer 130.

[0114] In this embodiment, the material of the second cover film 180 is a dielectric material, thereby making the material of the cover layer 190 a dielectric material. The corresponding cover layer 190 is used to form an isolation layer in the future, so that the cover layer 190 does not need to be removed.

[0115] In this embodiment, the process for forming the second capping film 180 includes a flow chemical vapor deposition process.

[0116] In this embodiment, the filling layer 165 is used as an example of a dielectric material for illustration, and the filling layer 165 is retained as an example for illustration. In other embodiments, after forming the second channel layer and before removing the limiting layer, the method for forming the semiconductor structure further includes: removing the filling layer; after removing the filling layer, forming a second capping film on the first capping film of the N-type region, the second capping film covering the sidewalls of the second channel layer and the sacrificial layer, and also located above the top of the limiting layer, the second capping film and the first capping film constituting a capping layer.

[0117] refer to Figure 15 and Figure 16 , Figure 16 yes Figure 15 A cross-sectional view along the xx direction shows the removal of the cover layer 190 above the top surface of the limiting layer 130, exposing the limiting layer 130. The limiting layer 130 is exposed to facilitate subsequent removal.

[0118] In this embodiment, a planarization process is used to remove the cover layer 190 that extends above the top surface of the limiting layer 130. As an example, a chemical mechanical planarization process is used to remove the cover layer 190 that extends above the top surface of the limiting layer 130.

[0119] In the step of removing the cover layer 190 above the top surface of the limiting layer 130, the sacrificial channel membrane 25 and the second liner 155 layer above the top surface of the limiting layer 130 are also removed.

[0120] refer to Figure 17 After the central channel membrane 24 is formed, the limiting layer 130 is removed.

[0121] Remove the limiting layer 130 so that the subsequent first pseudo-gate structure can span the first channel stack, and the second pseudo-gate structure can span the second channel stack.

[0122] In this embodiment, the step of removing the limiting layer 130 includes: removing the limiting layer 130 exposed by the cover layer 190. Specifically, in this embodiment, one or both of dry etching and wet etching processes are used to remove the limiting layer 130.

[0123] In this embodiment, the material of the cover layer 190 is a dielectric material. (Referring to the reference...) Figure 18 The method for forming a semiconductor structure further includes: after removing the limiting layer, removing a portion of the thickness of the cover layer 190, and using the remaining cover layer 190 as an isolation layer 210, which exposes the sacrificial layer 21, the first channel layer 22, and the second channel layer 30.

[0124] The isolation layer 210 is used to isolate adjacent protrusions 110 and also to isolate the substrate 100 from the subsequent gate structure.

[0125] In this embodiment, a portion of the cover layer 190 is removed, and the remaining cover layer 190 is used as an isolation layer 210. This combines the process of forming the second channel layer 30 with the process of forming the isolation layer 210, which is beneficial to improving process integration and process compatibility.

[0126] refer to Figure 19 The method for forming the semiconductor structure further includes: after removing the limiting layer 130, forming a first dummy gate structure (not shown) spanning the first channel stack and a second dummy gate structure (not shown) spanning the second channel stack; forming a first source / drain doped region (not shown) in the first channel stack on both sides of the first dummy gate structure; forming a second source / drain doped region (not shown) in the second channel stack on both sides of the second dummy gate structure; removing the first dummy gate structure to form a first gate opening (not shown), exposing the first channel stack; removing the sacrificial layer exposed by the first gate opening to form a first A through-slot (not shown) is formed, which is connected to a first gate opening; a first gate structure 230 is filled in the first gate opening and the first through-slot, and the first gate structure 230 surrounds the first channel layer 22; a second dummy gate structure is removed to form a second gate opening (not shown), exposing the second channel stack; the sacrificial layer exposed by the second gate opening is removed to form a second through-slot (not shown), which is connected to the second gate opening; a second gate structure 240 is filled in the second gate opening and the second through-slot, and the second gate structure 240 surrounds the second channel layer 30.

[0127] The first pseudo-gate structure is used to occupy space for the formation of the first gate structure.

[0128] As an example, the first dummy gate structure includes a first dummy gate oxide layer and a first dummy gate layer located on the first dummy gate oxide layer. The material of the first dummy gate oxide layer includes one or more of silicon oxide and silicon oxynitride. The material of the first dummy gate layer includes polycrystalline silicon or amorphous silicon.

[0129] The first source / drain doped region is used as the source or drain of the PMOS transistor. When the PMOS transistor is working, the first source / drain doped region is used to provide a source of charge carriers.

[0130] In this embodiment, the first source / drain doped region includes a stress layer doped with ions. This stress layer provides stress to the channel region, thereby improving carrier mobility. In this embodiment, the first source / drain doped region includes a stress layer doped with p-type ions, and the stress layer is made of Si or SiGe.

[0131] In this embodiment, after removing the sacrificial layer 21 exposed by the first gate opening, one or more first channel layers 22 are suspended at intervals and the protrusions 110 are suspended at intervals to form a first channel structure layer 250.

[0132] The second pseudo-gate structure is used to occupy space for the formation of the second gate structure.

[0133] As an example, the second dummy gate structure includes a second dummy gate oxide layer and a second dummy gate layer located on the second dummy gate oxide layer. The material of the second dummy gate oxide layer includes one or more of silicon oxide and silicon oxynitride. The material of the second dummy gate layer includes polycrystalline silicon or amorphous silicon.

[0134] The second source / drain doped region is used as the source or drain of the NMOS transistor. When the NMOS transistor is operating, the second source / drain doped region provides a carrier source. In this embodiment, the second source / drain doped region includes a stress layer doped with N-type ions, and the stress layer is made of Si or SiC.

[0135] In this embodiment, after removing the sacrificial layer 21 exposed by the second gate opening, one or more second channel layers 30 are suspended at intervals and the protrusions 110 are suspended at intervals to form a second channel structure layer 260.

[0136] The first gate structure 230 is used to control the turning on and off of the conductive channel of the PMOS transistor. In this embodiment, the first gate structure 230 spans the first channel structure layer 250.

[0137] In this embodiment, the first gate structure 230 is a metal gate structure. The first gate structure 230 includes a first gate dielectric layer (not shown) and a first gate electrode layer (not shown) located on the first gate dielectric layer. The first gate dielectric layer is used to isolate the first gate electrode layer from the first channel layer 22.

[0138] The second gate structure 240 is used to control the opening and closing of the conductive channel of the NMOS transistor.

[0139] In this embodiment, the second gate structure 240 spans the second channel structure layer 260.

[0140] In this embodiment, the second gate structure 240 is a metal gate structure, which includes a second gate dielectric layer (not shown) and a second gate electrode layer (not shown) located on the second gate dielectric layer. The second gate dielectric layer is used to isolate the second gate electrode layer and the second channel layer 30.

[0141] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A semiconductor structure, characterized in that, include: The substrate includes a P-type region for forming a PMOS transistor and an N-type region for forming an NMOS transistor; Multiple protrusions protrude from the substrate; A first channel structure layer is suspended on the protrusion of the P-type region. The first channel structure layer includes one or more first channel layers that are spaced apart and suspended. The first channel layer is used to improve the carrier mobility of the PMOS transistor channel. A second channel structure layer is suspended on the protrusion of the N-type region. The second channel structure layer includes one or more second channel layers that are spaced apart and suspended. The second channel layer includes a central channel film and sidewall channel films located on the sidewalls of the central channel film. The central channel film and the sidewall channel films are in contact to form the second channel layer. The sidewall channel films are located on both sides of the central channel film in a direction parallel to the substrate. The thickness of the sidewall channel films in the direction parallel to the substrate is 1 nanometer to 10 nanometers. The second channel layer is used to improve the carrier mobility of the NMOS transistor channel.

2. The semiconductor structure as described in claim 1, characterized in that, The semiconductor structure further includes: a first gate structure that spans the first channel structure layer and fills the space between adjacent first channel layers and between the protrusion of the P-type region and the first channel layer, wherein the first gate structure surrounds the first channel layer. The first source / drain doped region is located on both sides of the first gate structure and is in contact with the end of the first channel layer; The second gate structure spans the second channel structure layer and fills the space between adjacent second channel layers and between the protrusion of the N-type region and the second channel layer, the second gate structure surrounding the second channel layer. The second source / drain doped region is located on both sides of the second gate structure and is in contact with the end of the second channel layer.

3. The semiconductor structure as described in claim 1, characterized in that, The material of the central channel membrane is the same as the material of the sidewall channel membrane.

4. The semiconductor structure as described in claim 1, characterized in that, The materials of the central channel membrane and the sidewall channel membrane include one or more of silicon, silicon carbide, gallium nitride, gallium arsenide, and indium gallium nitride.

5. The semiconductor structure as described in claim 1, characterized in that, The material of the first channel layer includes one or more of silicon germanide, germanium, gallium nitride, gallium arsenide, and indium gallium.

6. The semiconductor structure as described in claim 5, characterized in that, The molar percentage of germanium in the first channel layer is 5% to 25%.

7. A method for forming a semiconductor structure, characterized in that, include: A substrate is provided, including a P-type region for forming a PMOS transistor and an N-type region for forming an NMOS transistor; The substrate includes a substrate, a plurality of protrusions protruding from the substrate, one or more stacked layers located on the protrusions, and a limiting layer located on top of the stack. Each stack includes a sacrificial layer and a first channel layer located on the sacrificial layer. The first channel layer is used to improve the carrier mobility of the PMOS transistor channel. Along a direction parallel to the substrate, a portion of the thickness of the first channel layer of the N-type region is removed to form a first trench, which is formed by the remaining first channel layer and the adjacent sacrificial layer, or by the remaining first channel layer and the adjacent sacrificial layer and the limiting layer. In the step of removing a portion of the thickness of the first channel layer of the N-type region along a direction parallel to the substrate, the thickness of the first channel layer of the N-type region removed is 1 nanometer to 10 nanometers. The first trench is filled with a sidewall channel membrane; Remove the remaining first channel layer of the N-type region to form a second trench between the sidewall channel membrane and the adjacent sacrificial layer, or between the sidewall channel membrane and the adjacent sacrificial layer and limiting layer. A central channel film is filled in the second trench, and the central channel film and the sidewall channel film are in contact to form a second channel layer. The sidewall channel film is located on both sides of the central channel film along the direction parallel to the substrate. The second channel layer is used to improve the carrier mobility of the NMOS transistor channel. After the central channel membrane is formed, the limiting layer is removed.

8. The method for forming a semiconductor structure as described in claim 7, characterized in that, The method for forming the semiconductor structure further includes: after forming the sidewall trench film and before removing the remaining first trench layer of the N-type region, forming a cutting groove on the N-type region that cuts the limiting layer, sacrificial layer, first trench layer, and protrusion along the extending direction of the protrusion, thereby exposing the first trench layer of the N-type region; The step of removing the remaining first channel layer in the N-type region includes: removing the remaining first channel layer located in the N-type region through the sidewall of the first channel layer exposed by the cutting groove.

9. The method for forming a semiconductor structure as described in claim 8, characterized in that, After forming the sidewall trench film and before forming the cut-off groove, the method of forming the semiconductor structure further includes: forming a filling layer located in the N-type region, the filling layer covering the sidewalls of the sidewall trench film and the sacrificial layer, as well as the sidewalls and top of the limiting layer; In the step of forming the cutting groove, the cutting groove also penetrates the filling layer of the N-type region along the extending direction perpendicular to the protrusion.

10. The method for forming a semiconductor structure as described in claim 9, characterized in that, After providing the substrate, and before removing a portion of the thickness of the first channel layer of the N-type region along a direction parallel to the substrate, the method of forming the semiconductor structure further includes: forming a first cover film on the substrate surrounding the protrusion, the first cover film covering the sidewalls of the stack located in the P-type region and the sidewalls and top of the limiting layer, and exposing the stack and the limiting layer located in the N-type region; in the step of forming the fill layer, the fill layer is formed on the first cover film located in the N-type region; After forming the second channel layer and before removing the limiting layer, the method for forming the semiconductor structure further includes: A second cover film is formed to fill the cutting groove, the second cover film, the filling layer, and the first cover film together constitute a cover layer; the cover layer above the top surface of the limiting layer is removed to expose the limiting layer; Alternatively, the filler layer is removed; after removing the filler layer, a second cover film is formed on the first cover film in the N-type region, the second cover film covering the sidewalls of the second channel layer and the sacrificial layer, and also located above the top of the limiting layer, the second cover film and the first cover film constituting a cover layer; the cover layer above the top surface of the limiting layer is removed, exposing the limiting layer; The step of removing the limiting layer includes: removing the limiting layer exposed by the covering layer.

11. The method for forming a semiconductor structure as described in claim 10, characterized in that, The material of the capping layer is a dielectric material; the method of forming the semiconductor structure further includes: after removing the limiting layer, removing a portion of the thickness of the capping layer, and using the remaining capping layer as an isolation layer, wherein the isolation layer exposes the sacrificial layer, the first channel layer and the second channel layer.

12. The method for forming a semiconductor structure as described in claim 10, characterized in that, A planarization process is used to remove the cover layer that is higher than the top surface of the limiting layer.

13. The method for forming a semiconductor structure as described in claim 7, characterized in that, After the second channel layer is formed, the sacrificial layer located in the P-type region and the adjacent first channel layer located on the sacrificial layer are used to form a first channel stack, and the sacrificial layer located in the N-type region and the adjacent second channel layer located on the sacrificial layer are used to form a second channel stack. The method for forming the semiconductor structure further includes: after removing the limiting layer, forming a first pseudo-gate structure spanning the first channel stack and a second pseudo-gate structure spanning the second channel stack; A first source / drain doped region is formed in the first channel stack on both sides of the first pseudo-gate structure; A second source / drain doped region is formed in the second channel stack on both sides of the second pseudo-gate structure; Remove the first pseudo-gate structure to form a first gate opening, exposing the first channel stack; Remove the sacrificial layer exposed by the first gate opening to form a first through-slot, which is connected to the first gate opening. A first gate structure is filled in the first gate opening and the first through slot, and the first gate structure surrounds the first channel layer; Remove the second pseudo-gate structure to form a second gate opening, exposing the second channel stack; Remove the sacrificial layer exposed by the second gate opening to form a second through-slot, which is connected to the second gate opening. A second gate structure is filled within the second gate opening and the second through-hole, and the second gate structure surrounds the second channel layer.

14. The method for forming a semiconductor structure as described in claim 7, characterized in that, An isotropic etching process is used to remove a portion of the thickness of the first channel layer of the N-type region along a direction parallel to the substrate.

15. The method for forming a semiconductor structure as described in claim 7, characterized in that, An isotropic etching process is used to remove the remaining first channel layer of the N-type region.

16. The method for forming a semiconductor structure as described in claim 7, characterized in that, In the step of providing the substrate, the material of the first channel layer includes silicon germanide, the material of the sacrificial layer includes silicon germanide, and the molar percentage of germanium in the sacrificial layer material is greater than the molar percentage of germanium in the first channel layer material.

17. The method for forming a semiconductor structure as described in claim 16, characterized in that, In the step of providing the substrate, the molar percentage of germanium in the first channel layer is 5% to 25%, and the molar percentage of germanium in the sacrificial layer is 30% to 50%.

18. The method for forming a semiconductor structure as described in claim 7, characterized in that, In the step of providing the substrate, the limiting layer and the sacrificial layer are made of the same material.

Citation Information

Patent Citations

  • Semiconductor device forming method

    CN110957223A