Surface modification method of a current collector and its application in a negative electrode-free lithium battery
By depositing Ag nanoparticles on the current collector of a negative electrodeless lithium battery, the problem of poor cycle stability was solved, resulting in better battery performance and safety.
Patent Information
- Application Number
- CN202310853898.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-07-12
AI Technical Summary
The cycle stability of electrodeless lithium batteries is poor, and existing technologies have not been able to improve it.
Ag nanoparticles were deposited on the current collector using a chemical immersion method, and the surface of the copper foil was treated with silver nitrate solution, followed by heat treatment to form a uniform Ag nanoparticle layer.
It significantly improves the cycle stability and safety of electrodeless lithium batteries, enhances the uniformity of lithium deposition and coulombic efficiency, and improves the reversibility and energy density of the battery.
Smart Images

Figure CN117117199B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to current collectors, and more specifically to a surface modification method for current collectors and its application in negative electrode-free lithium batteries. Background Technology
[0002] my country's power batteries require higher energy density, and besides high-capacity cathode materials, electrodeless lithium batteries are an optimal choice. Electrodeless lithium batteries do not use active cathode materials, but instead use copper foil current collectors as the cathode, significantly reducing costs. Because the cathode uses copper foil directly instead of the highly chemically active metallic lithium, it greatly facilitates and ensures battery assembly and safety. However, electrodeless lithium batteries suffer from poor cycle stability. Surface treatment of the current collector is a feasible method to improve stability, but further research and improvement are needed to achieve stable application. Summary of the Invention
[0003] To address the poor cycle stability of existing electrodeless lithium batteries, this invention provides a surface modification method for current collectors and its application in electrodeless lithium batteries. A chemical immersion method is used to modify the surface of the current collector, uniformly depositing Ag nanoparticles on it. The resulting current collector, when used in electrodeless lithium batteries, significantly improves cycle stability.
[0004] The technical solution of this invention is as follows:
[0005] A surface modification method for a current collector employs a chemical immersion method, in which copper foil is chemically immersed in silver nitrate solution to deposit Ag+ onto the copper foil.
[0006] Furthermore, it includes the following steps:
[0007] (1) Clean the copper foil with ultrasound in ethanol and / or acetone solution and then dry it;
[0008] (2) Dilute the silver nitrate solution with ultrapure water at room temperature to a concentration of 5 x 10⁻⁶. -4 ~8x10 -4 mol / L;
[0009] (3) The copper foil obtained in step (1) is immersed in the silver nitrate solution obtained in step (2). After the reaction, the copper foil is taken out, placed in a fume hood for drying, and then placed in a muffle furnace for heat treatment to obtain surface-modified copper foil.
[0010] Furthermore, the concentration of the silver nitrate solution is 5 x 10⁻⁶. -4 ~6x10 -4 mol / L.
[0011] Furthermore, the soaking time is 2 to 6 hours, preferably 3 to 4 hours.
[0012] Furthermore, the heat treatment temperature is 200–300℃, preferably 200–250℃; the time is 1–6 hours, preferably 2–4 hours; the heat treatment adopts programmed temperature rise, and the heating rate is 2–5℃ / min.
[0013] The current collector obtained by the above method can be used as a negative electrode in a negative electrode-free lithium battery, which can significantly improve cycle stability.
[0014] Furthermore, negative electrode-free lithium batteries utilize high-nickel, cobalt-free (LiNi) technology. 0.9 Mn 0.1 O2) is the positive electrode, and the electrolyte is a mixed solution of 2M-LiDFOB and 1.6M-LiBF4.
[0015] Furthermore, the solvent of the mixed solution is DEC and FEC in a volume ratio of 2:1.
[0016] The beneficial effects of this invention are as follows:
[0017] The current collector modification method of the present invention uniformly deposits Ag nanoparticles on the current collector. The lithium-philic Ag makes the lithium deposited on the current collector more uniform, which has a good effect on suppressing lithium dendrites, and the coulombic efficiency is more stable, thus having better reversibility. When the resulting current collector is applied to high-nickel cobalt-free cathode-and-anode lithium batteries, it can effectively improve the cycle stability of the battery, obtain a high-energy-density lithium-free anode battery, and improve the cycle stability and safety of anode-free lithium batteries.
[0018] The chemical immersion method employed in this invention is low-cost, simple, and suitable for large-scale industrial production. The immersion solution can be recycled, making it significantly cheaper than spraying methods. Compared to spraying, the chemical immersion method of this invention results in more uniform Ag nanoparticles deposited on the current collector, thereby significantly improving the cycle stability of the battery. Attached Figure Description
[0019] Figure 1 This is a graph showing the cycle performance of a lithium-ion battery without a negative electrode at 0.5C, assembled with a high-nickel, cobalt-free positive electrode, untreated copper foil, and surface-treated copper foil.
[0020] Figure 2 It is untreated copper foil and surface-treated copper foil at 1mA / cm 2 1mAh / cm 2 Coulomb efficiency diagram under the given conditions.
[0021] Figure 3 The untreated copper foil and the surface-treated copper foil are at 1mAh / cm 2 SEM image of lithium deposition.
[0022] Figure 4 The surface-treated copper foil is at 1mAh / cm 2 SEM image of lithium deposition. Detailed Implementation
[0023] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited thereto.
[0024] Example 1
[0025] A 5cm x 5cm piece of copper foil was cut from a 9μm thick commercial copper foil. After ultrasonic cleaning in ethanol and acetone, the silver nitrate solution was diluted with ultrapure water to a concentration of 5 x 10⁻⁶. -4 The copper foil was then immersed in the diluted silver plating solution at a concentration of mol / L. The reaction time was controlled to be 2 hours. After drying in a fume hood, it was placed in a muffle furnace for heat treatment at 200°C for 2 hours at a heating rate of 2°C / min. After cooling, it was removed and cut into round pieces with a diameter of 14 mm.
[0026] Example 2
[0027] A 5cm x 5cm piece of copper foil was cut from a 9μm thick commercial copper foil. After ultrasonic cleaning in ethanol and acetone, the silver nitrate solution was diluted with ultrapure water to a concentration of 5 x 10⁻⁶. -4 The copper foil was then immersed in a diluted silver plating solution at a concentration of mol / L. The reaction time was controlled at 4 hours. After drying in a fume hood, it was placed in a muffle furnace for heat treatment at 200°C for 2 hours at a heating rate of 2°C / min. After cooling, it was removed and cut into circular pieces with a diameter of 14 mm.
[0028] Example 3
[0029] A 5cm x 5cm piece of copper foil was cut from a 9μm thick commercial copper foil. After ultrasonic cleaning in ethanol and acetone, the silver nitrate solution was diluted with ultrapure water to a concentration of 5 x 10⁻⁶. -4 The copper foil was then immersed in a diluted silver plating solution at a concentration of mol / L. The reaction time was controlled to be 6 hours. After drying in a fume hood, it was placed in a muffle furnace for heat treatment at 200°C for 2 hours at a heating rate of 2°C / min. After cooling, it was removed and cut into circular pieces with a diameter of 14 mm.
[0030] High-nickel cobalt-free (LiNi) 0.9 Mn 0.1O2) was used as the positive electrode, and the electrolyte was a mixed solution of 2M-LiDFOB and 1.6M-LiBF4, with DEC and FEC in a volume ratio of 2:1. The negative electrode used was copper foil treated as described above, and a high-nickel, cobalt-free, negative-electrode lithium battery was assembled. The test conditions were: 25℃, 0.5C, 2.7-4.3V.
[0031] pass Figure 1 It can be seen that the capacity of the untreated copper foil-assembled electrodeless lithium battery decays rapidly, with a specific capacity of only 30 mAh / g after 50 cycles. In contrast, the capacity of the surface-treated copper foil-assembled electrodeless lithium battery decays more slowly, with a specific capacity of 80 mAh / g after 50 cycles.
[0032] pass Figure 2 It can be seen that the coulombic efficiency of the lithium-to-copper battery assembled with treated copper foil is better than that of the untreated lithium-to-copper battery assembled with copper foil, and the coulombic efficiency and stability are both better.
[0033] By comparison Figure 3 and Figure 4 It can be seen that the lithium deposition morphology on the untreated copper foil is loose and porous, and the side reactions between lithium and electrolyte are more severe, leading to a decline in electrochemical performance. The lithium deposition morphology on the surface-treated copper foil is bulky and dense, with fewer side reactions and less performance degradation.
Claims
1. The application of a current collector obtained by a surface modification method as a negative electrode in a negative electrode-free lithium battery, characterized in that, The negative electrode-free lithium battery uses high-nickel, cobalt-free LiNi alloy. 0.9 Mn 0.1 O2 is the positive electrode, and the electrolyte is a mixed solution of 2M-LiDFOB and 1.6M-LiBF4; The surface modification method for the current collector includes the following steps: (1) Clean the copper foil with ultrasound in ethanol and / or acetone solution and then dry it; (2) Dilute the silver nitrate solution with ultrapure water at room temperature to a concentration of 5 x 10⁻⁶. -4 ~8x10 -4 mol / L; (3) The copper foil obtained in step (1) is immersed in the silver nitrate solution obtained in step (2). After the reaction, the copper foil is taken out and placed in a fume hood for drying. Then the copper foil is placed in a muffle furnace for heat treatment to obtain a surface-modified copper foil current collector. The temperature of the heat treatment is 200-250℃ and the time is 2-4 hours. The heat treatment adopts a programmed temperature rise rate of 2-5℃ / min.
2. The application according to claim 1, characterized in that, Soaking time is 2 to 6 hours.
3. The application according to claim 1, characterized in that, Soaking time is 3 to 4 hours.
4. The application according to claim 1, characterized in that, The solvent for the mixed solution is DEC and FEC in a volume ratio of 2:1.
Citation Information
Patent Citations
Carbon nano tube-Sn-M alloy cathode material and preparation method thereof
CN103022449A
Lithium battery pole plate
CN103682369A
Negative current collector of non-negative lithium battery as well as preparation method and application of negative current collector
CN115863660A