An organic polysaccharide material memristor with high biocompatibility and a preparation method thereof

By fabricating organic polysaccharide memristors with a vertical sandwich structure, the problems of difficult processing and environmental impact of xylan materials have been solved, achieving high biocompatibility and stable electrical performance, making them suitable for the biomedical field.

CN117119877BActive Publication Date: 2026-11-24NANJING UNIV OF POSTS & TELECOMM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310874733.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-17
Publication Date
2026-11-24
Estimated Expiration
2043-07-17

AI Technical Summary

Technical Problem

In existing technologies, xylan, when used as a memristor material, is difficult to process, has high adhesion, and is difficult to prepare high-quality thin films. Furthermore, traditional materials have adverse effects on the environment and organisms.

Method used

The memristor, made of organic polysaccharide material with a vertical sandwich structure, has a glass substrate, an indium tin oxide bottom electrode layer, xylan as a functional layer, and silver as a top electrode layer. It is prepared by conductive glass coating, spin coating, annealing, and vapor deposition processes, using ultrapure water as a solvent and controlling the spin coating speed and temperature to form a highly biocompatible memristor.

Benefits of technology

This invention achieves a highly biocompatible, environmentally friendly, and pollution-free memristor with stable high-to-low impedance switching performance, a simple fabrication process, and high yield, making it suitable for biomedical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117119877B_ABST
    Figure CN117119877B_ABST
Patent Text Reader

Abstract

This invention discloses a highly biocompatible organic polysaccharide memristor and its preparation method. The memristor structure comprises four parts from bottom to top: a substrate, a bottom electrode, a functional layer, and a top electrode. Using xylan as the organic layer material and ultrapure water as the solvent, a uniform and smooth thin film is obtained through spin-coating. The resulting memristor exhibits low operating voltage, high on / off ratio, and high retention characteristics (>1*10⁻⁶). 4 With its advantages in stability, the present invention features a simple structural design, easy-to-operate process, simple preparation, and high yield, making it universally applicable. It opens up an effective path for improving the overall performance of resistive switching memory with good biocompatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of organic diode memristor technology, specifically relating to a memristor made of organic polysaccharide material with high biocompatibility and its preparation method. Background Technology

[0002] Research on the memory effect of organic materials began in the 1970s, when scholars observed the transition between different resistance states in polystyrene and copper-tetracyanoquinoline (Cu-TNCQ) films. Since the 21st century, organic memory devices have made significant progress, especially with the application of small organic molecule materials with excellent structural stability, which has greatly improved the long-term cycling performance of memory during operation.

[0003] Using environmentally friendly and sustainable organic materials can reduce the use of metal oxides and compounds, thus alleviating the excessive consumption of resources and environmental degradation to some extent. Among them, natural biomaterials can be extracted directly from plants or animals without the need for complex chemical synthesis and processing, and have the potential to be combined with organisms and biodegradable medical implants. Therefore, memristors based on biomaterials are expected to have fascinating applications in biomedicine.

[0004] Xylan is a natural biopolymer extracted from plant fibers and possesses excellent biocompatibility. In biomedical applications, using xylan as a memristor material can reduce adverse reactions and rejection responses in organisms, improving the material's biocompatibility. Compared to traditional electronic materials, such as metals or inorganic materials, the use of xylan can reduce dependence on limited resources and mitigate environmental impact.

[0005] However, the current use of xylan as a memristor material still has certain shortcomings, such as its high viscosity and adhesion, which makes it difficult to perform precise processing and thin film fabrication. Therefore, it is necessary to develop processing methods and thin film fabrication technologies suitable for natural biomaterials to achieve high-quality memristor devices. Summary of the Invention

[0006] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0007] In view of the problems existing in the above and / or prior art, the present invention is proposed.

[0008] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a memristor made of organic polysaccharide material with high biocompatibility. The memristor has a vertical sandwich structure, including a base layer, a bottom electrode layer, an organic functional layer and a top electrode layer.

[0009] The organic functional layer material is xylan, with the structural formula shown in Formula A:

[0010]

[0011] In a preferred embodiment of the present invention, the substrate material is glass.

[0012] In a preferred embodiment of the present invention, the bottom electrode layer material is indium tin oxide with a thickness of 185 nm.

[0013] In a preferred embodiment of the present invention, the thickness of the organic functional layer is 70–80 nm.

[0014] In a preferred embodiment of the present invention, the top electrode layer is a silver electrode with a thickness of 20-30 nm.

[0015] Another objective of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a memristor made of highly biocompatible organic polysaccharide material.

[0016] To solve the above-mentioned technical problems, the present invention provides the following technical solution: including,

[0017] Using conductive glass as a substrate, tin oxide is coated on the substrate surface to form a bottom electrode layer, resulting in ITO conductive glass, which is then sequentially cleaned, blown dry, baked, and treated with ultraviolet ozone.

[0018] A xylan solution is spin-coated onto the bottom electrode layer of the treated ITO conductive glass, followed by annealing and film formation to obtain an organic functional layer. Then, metallic silver is vapor-deposited onto the surface of the organic functional layer to form a top electrode layer. Once the vapor deposition is complete, a memristor with high biocompatibility is obtained.

[0019] In a preferred embodiment of the present invention, the blowing is performed by blowing with nitrogen gas, and the drying is performed by placing the product in an oven for drying, wherein the drying temperature is 120°C and the drying time is 1 to 2 hours.

[0020] As a preferred embodiment of the present invention, the spin-coated xylan solution is wherein the solvent of the xylan solution is ultrapure water and the xylan concentration is 45 mg / mL. The inventors have found that when the xylan solution concentration is lower than 45 mg / mL, the memristor performance is poor due to insufficient concentration.

[0021] The spin coating speed is 500 rpm to 1000 rpm, and the spin coating time is 9 s to 30 s.

[0022] In a preferred embodiment of the present invention, the annealing temperature is 60°C and the time is 1 hour.

[0023] As a preferred embodiment of the present invention, the evaporation rate is:

[0024] Beneficial effects of this invention:

[0025] (1) This invention uses xylan as the organic layer material and ultrapure water as the solvent for spin coating of the organic layer to prepare a memristor with high biocompatibility. Compared with the prior art, it has the characteristics of being green, environmentally friendly and pollution-free.

[0026] (2) The present invention has a simple structural design, easy operation process, simple preparation and high yield, and is universally applicable, thus opening up an effective path for improving the overall performance of resistive switching memory with good biocompatibility. Attached Figure Description

[0027] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:

[0028] Figure 1 This is a structural diagram of an organic memristor device.

[0029] Figure 2 The image shows the IV curve of the organic memristor prepared in Example 1 after 150 cycles.

[0030] Figure 3 This is a distribution diagram of the IV curves SET and RESET Voltage of the organic memristor prepared in Example 1.

[0031] Figure 4 This describes the change in resistance value of the organic memristor prepared in Example 1 as it continuously switches between high and low resistance states.

[0032] Figure 5 IV curve of the memristor prepared in Comparative Example 1 of this invention

[0033] Figure 6 This is the IV curve of the organic memristor device in Comparative Example 2.

[0034] Figure 7 This is the IV curve of the organic memristor device in Comparative Example 3.

[0035] Figure 8 This is the IV curve of the organic memristor device in Comparative Example 4.

[0036] Figure 9 This is the IV curve of the organic memristor device in Comparative Example 5. Detailed Implementation

[0037] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0038] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0039] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0040] Unless otherwise specified, all raw materials used in this invention are commercially available in the field.

[0041] Example 1

[0042] This embodiment provides a method for preparing a memristor made of a highly biocompatible organic polysaccharide material. The structure of the obtained memristor is as follows: Figure 1 As shown, specifically:

[0043] 1) Using conductive glass as a substrate, a bottom electrode layer (200) with a thickness of 185nm is formed by coating tin oxide on the surface of the substrate layer (100) to obtain ITO conductive glass. It is then cleaned with ITO cleaning agent and ultrapure water for 30min, then dried and placed in an oven at 120℃ for 60min to dry, and then treated with ultraviolet ozone for 30min.

[0044] 2) A xylan solution with a concentration of 45 mg / mL and ultrapure water as solvent was spin-coated onto the bottom electrode layer (200) of the treated ITO conductive glass. First, the spin-coating was done at a speed of 500 rpm for 9 seconds, and then at a speed of 1000 rpm (the inventors found that this speed below 1000 rpm would affect the fluidity of the solution and thus affect the coating effect) for 30 seconds. The film was then annealed at 60°C for 1 hour to form an organic functional layer (300) with a thickness of 70-80 nm.

[0045] 3) Then, metallic silver is vapor-deposited on the surface of the organic functional layer (300) to form the top electrode layer (400). Specifically, the film-formed ITO conductive glass is placed in a vacuum vapor deposition equipment, and the pressure in the vacuum chamber is controlled to be 5×10⁻⁶. -4 Pa begins the process of vapor deposition of a metallic silver electrode, resulting in a silver electrode with a thickness of 20–30 nm. Once the vapor deposition is complete, a memristor with high biocompatibility is obtained.

[0046] Figure 2 The figure shows the IV curve of the organic memristor prepared in this embodiment after 150 cycles. It can be seen from the figure that the memristor has a relatively large switching capacity, approximately 10. 4 This indicates that the memristor can achieve stable switching between high and low resistance states. Figure 3 The figure shows the distribution curves of the SET and RESET voltages of the IV curve. It can be seen from the figure that the SET voltage distribution is relatively uniform (the variance of the SET voltage is 0.259), the average value of the SET voltage is about 2.23V, and the average value of the RESET voltage is -4.43V (the variance of the RESET voltage is 1.112), indicating that it has better cycle stability.

[0047] Figure 4 The diagram illustrates the change in resistance value of the memristor as it continuously switches between high and low resistance states. It can be seen that the resistance value always maintains a stable two-state distribution, indicating that the formation and erasure processes of the conductive wires inside the device are very stable, thus the device exhibits excellent electrical performance.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that the solvent for the xylan solution was changed to dimethyl sulfoxide, while the rest of the preparation process was the same as in Example 1, and the memristor of this comparative example was obtained.

[0050] Figure 5 The IV curve of the memristor prepared in Comparative Example 1 is shown in Table 1. The relevant electrical properties of the memristor in Comparative Example 1 are compared with those in Example 1.

[0051] Table 1

[0052]

[0053] By comparing with the memristor prepared in Example 1, it can be seen that the memristor prepared in Example 1 using ultrapure water as a solvent has a more stable conductive wire formation process and better electrical performance than the memristor prepared using dimethyl sulfoxide.

[0054] Comparative Example 2

[0055] The difference between this comparative example and Example 1 is that the concentration of the xylan solution was adjusted to 47.5 mg / mL, while the rest of the preparation process was the same as in Example 1, thus obtaining the memristor of this example.

[0056] like Figure 6 As shown, the IV curve of the memristor device in this comparative example exhibits significant volatility during cycling, indicating that the formation and breakage of the conductive wire are unstable at this concentration.

[0057] Comparative Example 3

[0058] The difference between this comparative example and Example 1 is that the concentration of the xylan solution was adjusted to 50 mg / mL, while the rest of the preparation process was the same as in Example 1, thus obtaining the memristor of this example.

[0059] Figure 7 The IV curves of the organic memristor device in this comparative example show that, at the same coating speed as in Example 1, the higher the solution concentration, the greater the on / off ratio of the device. However, the device is prone to exhibiting Worm characteristics, that is, there is only a process of generating conductive wires without a process of erasing, which leads to poor stability.

[0060] Comparative Example 4

[0061] The difference between this comparative example and Example 1 is that the spin coating speed was adjusted to first spin coat at 500 rpm for 9 seconds, and then spin coat at 1500 rpm for 30 seconds. The rest of the preparation process is the same as in Example 1, and the memristor of this example is obtained.

[0062] Figure 8 The IV curve of the organic memristor device in Example 4 shows that when the coating speed is increased, the switching ratio in the IV curve of the device decreases sharply to less than an order of magnitude, and the number of cycles that can be stably reproduced decreases.

[0063] Comparative Example 5

[0064] The difference between this comparative example and Example 1 is that the spin coating speed was adjusted to first spin coating at 500 rpm for 9 seconds, and then spin coating at 2000 rpm for 30 seconds. The rest of the preparation process was the same as in Example 1, and the memristor of this example was obtained.

[0065] Figure 9 The IV curve of the organic memristor device in Example 5 shows that there is no obvious read, write, and erase process in the IV curve, indicating unstable performance and a very small on / off ratio.

[0066] In summary, this invention uses xylan as the organic layer material and ultrapure water as the solvent to spin-coat a uniform and smooth thin film. The resulting memristor exhibits low operating voltage, high on / off ratio, and high retention characteristics (>1*10). 4With its advantages in stability, the present invention features a simple structural design, easy-to-operate process, simple preparation, and high yield, making it universally applicable. It opens up an effective path for improving the overall performance of resistive switching memory with good biocompatibility.

[0067] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A memristor made of a highly biocompatible organic polysaccharide material, characterized in that: The memristor has a vertical sandwich structure, including a base layer (100), a bottom electrode layer (200), an organic functional layer (300), and a top electrode layer (400). The organic functional layer (300) material is xylan, with the structural formula shown in Formula A: (Formula A); The base layer (100) is made of glass; The bottom electrode layer (200) is made of indium tin oxide and has a thickness of 185 nm. The thickness of the organic functional layer (300) is 70~80nm; The top electrode layer (400) is a silver electrode with a thickness of 20~30nm; The method for fabricating the memristor includes, Using conductive glass as a substrate, a bottom electrode layer (200) is formed by coating tin oxide on the substrate surface to obtain ITO conductive glass, which is then sequentially cleaned, blown dry, baked, and treated with ultraviolet ozone. A xylan solution is spin-coated onto the bottom electrode layer (200) of the treated ITO conductive glass, annealed, and film-formed to obtain an organic functional layer (300). Then, metallic silver is vapor-deposited on the surface of the organic functional layer (300) to form a top electrode layer (400). After the vapor deposition is completed, a memristor with high biocompatibility is obtained. The blowing is done by blowing with nitrogen gas, and the drying is done by placing the item in an oven for drying, wherein the drying temperature is 120°C and the drying time is 1 to 2 hours; The spin-coated xylan solution is wherein the solvent of the xylan solution is ultrapure water, and the xylan concentration is 45 mg / mL; the spin-coating speed is 500 rpm to 1000 rpm, and the spin-coating time is 9 s to 30 s; The annealing temperature is 60°C and the time is 1 hour; The evaporation rate is 1~1.2 Å / s.