Epoxy resin, curable resin composition, and cured product of curable resin composition

By introducing isopropylene structure and optimizing molecular weight into epoxy resin, combined with hardening accelerator and inorganic filler, the trade-off problem between heat resistance and tracking resistance of epoxy resin in the existing technology is solved, and high performance is achieved. Excellent flame retardancy and heat resistance, suitable for complex semiconductor encapsulation and substrate materials.

CN117120503BActive Publication Date: 2024-10-11NIPPON KAYAKU CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202280027910.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-30
Filing Date
2022-07-15
Publication Date
2024-10-11
Estimated Expiration
2042-07-15

Smart Images

  • Figure CN117120503B_ABST
    Figure CN117120503B_ABST
Patent Text Reader

Abstract

The present invention provides an epoxy resin, a curable resin composition and a cured product, wherein the cured product has excellent heat resistance, flame retardancy and tracking resistance. The epoxy resin is represented by the following formula (1). In formula (1), n ​​is the average value of the number of repetitions, and 1<n<20. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an epoxy resin having a specific structure, a curable resin composition, and a cured product of the curable resin composition. Background Art

[0002] Epoxy resins are widely used in electrical / electronic fields such as cast products, laminated boards, integrated circuit (IC) sealing materials, structural materials, adhesives, coatings, etc. due to their excellent electrical properties (dielectric constant / dielectric loss tangent, insulation), mechanical properties, adhesion, and thermal properties (heat resistance, etc.).

[0003] In recent years, in the electrical / electronic field, it is required that the flame retardant property, moisture resistance, adhesion, dielectric properties and other performances of resin combination be improved, highly purified, be used for making the low viscosity of filler (inorganic filler or organic filler) highly filled, be used for shortening the further improvement (patent documentation 1) of each characteristic such as the reactivity improvement of molding cycle.In addition, as structural material, in aerospace materials, leisure / sports equipment purposes etc., require the material of lightweight and excellent mechanical properties.Particularly in semiconductor sealing field, substrate (substrate itself or its peripheral materials), along with the change of described semiconductor, become complicated because of thin layer, stacking, systematization, three-dimensionalization, require the requirement characteristics such as very high level of heat resistance or high fluidity.

[0004] Furthermore, with the development of autonomous driving technology and the expansion of the electric vehicle market, various power boards and inverter boards are required to have tracking resistance (CTI resistance: Comparative Tracking Index resistance), which has not been required for FR-4 boards so far.

[0005] Generally, it is known that epoxy resins having a structure that is easily carbonized have poor tracking resistance, but have high flame retardancy.

[0006] In order to improve the heat resistance of the resin composition, an aromatic crosslinking unit is sometimes introduced, but in this case, since the main skeleton is aromatic, it is easy to carbonize, and the tracking resistance decreases. In addition, when the heat resistance is improved by high molecular weight, the molecular weight becomes large, the thermal decomposition temperature rises, and the tracking resistance decreases. That is, there is a trade-off relationship between heat resistance and tracking resistance (Non-Patent Document 1).

[0007] Under such circumstances, it is desired to develop a material that exhibits high heat resistance and simultaneously has flame retardancy and tracking resistance.

[0008] In particular, in applications such as solar power generation, wind power generation, and electric vehicles (EVs), tracking resistance is emphasized, and a relative tracking index (CTI) exceeding 600 is required.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2015-147854

[0012] Non-patent document 1: Development of multilayer materials for high reliability environments (by Sumitomo Bakelite Co., Ltd. Circuit Materials Research Department) Summary of the invention

[0013] Problems to be solved by the invention

[0014] In view of the above problems, an object of the present invention is to provide an epoxy resin and a curable resin composition whose cured product is excellent in heat resistance, flame retardancy and tracking resistance.

[0015] Technical means of solving problems

[0016] The present inventors have made intensive research to solve the above problems and have completed the present invention. That is, the present invention relates to the following [1] to [6]. In the present application, "(numerical value 1) to (numerical value 2)" means including upper and lower limits. [1]

[0018] An epoxy resin represented by the following formula (1).

[0019] [Chemistry 1]

[0020]

[0021] (In formula (1), n ​​is the average value of the number of repetitions, 1<n<20.) [2]

[0023] An epoxy resin represented by the following formula (2).

[0024] [Chemistry 2]

[0025]

[0026] (In formula (2), n is the average value of the number of repetitions, 1<n<20.) [3]

[0028] The epoxy resin according to the above item [1] or [2], wherein the weight average molecular weight as measured by gel permeation chromatography (GPC) is 400 to 3,000. [4]

[0030] A curable resin composition comprising the epoxy resin according to any one of the above items [1] to [3]. [5]

[0032] The curable resin composition according to the above item [4], further comprising a curing accelerator. [6]

[0034] A cured product obtained by curing the curable resin composition according to the above item [4] or [5].

[0035] Effects of the Invention

[0036] The present invention relates to an epoxy resin with a specific structure, a curable resin composition and a cured product thereof. The cured product has tracking resistance, heat resistance and flame retardancy.

[0037] Therefore, the present invention can be effectively used in insulating materials for electrical and electronic parts (high reliability semiconductor sealing materials, etc.) and laminated boards (printed wiring boards, build-up substrates, etc.) or various composite materials, adhesives, coatings, etc. represented by carbon fiber reinforced plastics (CFRP). BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The GPC chart of Synthesis Example 1 is shown.

[0039] Figure 2 The GPC chart of Synthesis Example 2 is shown.

[0040] Figure 3 The GPC chart of Synthesis Example 3 is shown.

[0041] Figure 4 The GPC chart of Synthesis Example 4 is shown.

[0042] Figure 5 This chart shows the GPC chart of bisphenol A novolac resin.

[0043] Figure 6 The GPC chart of Synthesis Example 5 is shown. DETAILED DESCRIPTION

[0044] The present invention is described in detail below.

[0045] The epoxy resin of the present invention is represented by the following formula (1).

[0046] [Chemistry 3]

[0047]

[0048] (In formula (1), n ​​is the average value of the number of repetitions, 1<n<20.)

[0049] The compound represented by the formula (1) has excellent tracking resistance, heat resistance and flame retardancy by adopting a molecular design in which a plurality of isopropylidene structures that are not easily carbonized are introduced while maintaining the density of the aromatic rings.

[0050] In the formula (1), the value of n can be calculated from the number average molecular weight determined by gel permeation chromatography (GPC, detector: RI (refractive index)) or the area ratio of each separated peak. The value of n is further preferably 1<n<15, and particularly preferably 1<n<10.

[0051] The weight average molecular weight determined by GPC is preferably 400 to 4500, more preferably 500 to 4000, and further preferably 1000 to 3000. When the weight average molecular weight is less than 400, it is not easy to obtain the heat resistance improvement effect brought about by the increase in molecular weight. In addition, when the weight average molecular weight is greater than 4500, it is difficult to purify by washing with water, etc. In addition, when used for semiconductor sealing materials, the viscosity is too high, and the fluidity cannot be ensured, so that the filling between the wiring becomes difficult. In addition, it is also difficult to ensure the fluidity of the prepreg in the substrate application, and the embedding property of the wiring is impaired.

[0052] The epoxy resin represented by the formula (1) is usually in a semi-solid to solid resin state at room temperature, and its softening point is preferably below 100°C, and more preferably below 90°C. When the softening point is higher than 100°C, the viscosity is high, and the fiber impregnation property decreases when the prepreg is made. In addition, its epoxy equivalent is preferably 200g / eq to 1000g / eq, and more preferably 280g / eq to 800g / eq, particularly preferably 290g / eq to 700g / eq, and most preferably 295g / eq to 600g / eq. In addition, its ICI viscosity at 150°C is preferably 0.01Pa·s to 1.2Pa·s, more preferably 0.01Pa·s to 1.0Pa·s, and more preferably 0.01Pa·s to 0.8Pa·s. If it is within the above range, when the sealing material composition is made, the appropriate fluidity as a sealing material can be ensured.

[0053] An example of a preferred structure of the epoxy resin represented by the above formula (1) is an epoxy resin represented by the following formula (2).

[0054] [Chemistry 4]

[0055]

[0056] (In formula (2), n is the average value of the number of repetitions, 1<n<20.)

[0057] The preferred range of n in the formula (2) is the same as that in the formula (1).

[0058] The epoxy resin represented by the formula (2) has low crystallinity, thereby reducing solvent solubility or the risk of crystal precipitation in a solvent.

[0059] The preparation method of the epoxy resin of the present invention is not particularly limited, and can be obtained, for example, by subjecting a phenol resin represented by the following formula (3) to addition or ring-closure reaction with an epihalohydrin in the presence of a solvent or a catalyst. The amount of the epihalohydrin used is usually 1.0 mol to 20.0 mol, preferably 1.5 mol to 10.0 mol, relative to 1 mol of the phenolic hydroxyl group of the phenol resin.

[0060] [Chemistry 5]

[0061]

[0062] (In formula (3), n is the average value of the number of repetitions, 1<n<20.)

[0063] The preferred range of n in the formula (3) is the same as that in the formula (1).

[0064] The phenol resin represented by the formula (3) has a weight average molecular weight measured by GPC of preferably 400 to 4500, more preferably 500 to 4000, and further preferably 1000 to 3000. The preferred range of the hydroxyl equivalent is 100 g / eq to 300 g / eq, more preferably 120 g / eq to 250 g / eq, and further preferably 120 g / eq to 230 g / eq. The preferred range of the melt viscosity (ICI viscosity) at 150°C is 0.01 Pa·s to 3.0 Pa·s, more preferably 0.02 Pa·s to 2.0 Pa·s, and further preferably 0.02 Pa·s to 1.5 Pa·s. The preferred range of the softening point is 40°C to 180°C, more preferably 50°C to 150°C, and further preferably 60°C to 140°C. When the softening point is less than 40°C, it is difficult to obtain the effect of improving heat resistance due to the increase in molecular weight. In addition, when the softening point is higher than 180°C, it is difficult to purify by water washing or the like. In addition, when used as a hardener for semiconductor sealing materials or when made into epoxide, the viscosity is too high and fluidity cannot be ensured, making it difficult to fill the wiring gaps. In addition, in substrate applications, it is difficult to ensure the fluidity of the prepreg, and the embedding property of the wiring is impaired.

[0065] As the alkali metal hydroxide that can be used in the epoxidation reaction, sodium hydroxide, potassium hydroxide, etc. can be listed. The alkali metal hydroxide can be a solid substance, and its aqueous solution can also be used. In the case of using an aqueous solution, it can be the following method: the aqueous solution of the alkali metal hydroxide is continuously added to the reaction system, and water and epihalohydrin are continuously distilled out under reduced pressure or under normal pressure, and then liquid separation is carried out to remove water, so that epihalohydrin is continuously returned to the reaction system. Relative to 1 mole of phenolic hydroxyl groups of phenol resin, the usage amount of alkali metal hydroxide is generally 0.9 mole to 2.5 moles, preferably 0.95 mole to 1.5 moles. If the usage amount of alkali metal hydroxide is small, the reaction will not be fully carried out. On the other hand, the situation of excessively using more than 2.5 moles of alkali metal hydroxide relative to 1 mole of phenolic hydroxyl groups of phenol resin can cause unnecessary waste to be generated by the side.

[0066] In order to promote the reaction, quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may also be added as catalysts. The usage amount of the quaternary ammonium salt is usually 0.1 g to 15 g, preferably 0.2 g to 10 g, relative to 1 mol of the phenolic hydroxyl group of the phenol resin. If the usage amount is too small, sufficient reaction promotion effect cannot be obtained. If the usage amount is too large, the amount of the quaternary ammonium salt remaining in the epoxy resin increases, so it is also possible to become the cause of deterioration of electrical reliability.

[0067] During epoxidation, in terms of reaction, it is preferred to add aprotic polar solvents such as alcohols such as methanol, ethanol, isopropanol, dimethyl sulfone, dimethyl sulfoxide, tetrahydrofuran, dioxane, etc. to react. When using alcohols, its usage is generally 2% by weight to 50% by weight relative to the usage of epihalohydrin, preferably 4% by weight to 20% by weight. In addition, when using aprotic polar solvents, its usage is generally 5% by weight to 100% by weight relative to the usage of epihalohydrin, preferably 10% by weight to 80% by weight. The reaction temperature is generally 30°C to 90°C, preferably 35°C to 80°C. The reaction time is generally 0.5 hours to 100 hours, preferably 1 hour to 30 hours.

[0068] After the reaction is completed, the epihalohydrin or solvent is removed after washing the reactant or without washing under heating and reduced pressure. In addition, in order to make an epoxy resin with less hydrolyzable halogen, the recovered epoxy resin can also be dissolved in solvents such as toluene and methyl isobutyl ketone, and an aqueous solution of alkali metal hydroxides such as sodium hydroxide and potassium hydroxide is added to react, so that the closed loop is reliable. In this case, the amount of alkali metal hydroxide used is generally 0.01 mol to 0.3 mol, preferably 0.05 mol to 0.2 mol, relative to 1 mol of phenolic hydroxyl groups of the phenol resin used in glycidylation. The reaction temperature is generally 50°C to 120°C, and the reaction time is generally 0.5 hours to 24 hours. After the reaction is completed, the generated salt is removed by filtration, washing, etc., and then the solvent is distilled off under heating and reduced pressure to obtain the epoxy resin of the present invention.

[0069] Here, the method for preparing the phenol resin represented by the formula (3) is described. The method for preparing the phenol resin represented by the formula (3) is not particularly limited. For example, by reacting bisphenol A and α,α,α',α'-tetramethylbenzenedimethanol (or diisopropenylbenzene, or α,α,α',α'-tetramethylbenzene difluoride, α,α,α',α'-tetramethylbenzene dichloride, α,α,α',α'-tetramethylbenzene dibromide, α,α,α',α'-tetramethylbenzene diiodide and other halogen compounds) under an acid catalyst in a solvent, the target phenol resin can be obtained. At this time, as a raw material, it is preferred to use a raw material substituted at the meta position. Specifically, α,α,α',α'-tetramethyl-1,3-benzenedimethanol and 1,3-diisopropenylbenzene can be listed. In addition, α,α,α',α'-tetramethyl-1,3-benzenedifluoride, α,α,α',α'-tetramethyl-1,3-benzenedichloride, α,α,α',α'-tetramethyl-1,3-benzenedibromide, α,α,α',α'-tetramethyl-1,3-benzenediodide and other halogen compounds can be listed. By using a raw material having a substitution position at the meta position, the crystallinity of the raw material and the synthesized compound can be reduced, thereby reducing the solvent solubility or the risk of crystallization in the solvent. During the synthesis, as an acid catalyst, in addition to using hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, p-toluenesulfonic acid, and methanesulfonic acid, Lewis acids such as aluminum chloride and zinc chloride, activated clay, acid clay, white carbon, zeolite, solid acids such as silica alumina, and acidic ion exchange resins can also be used. These may be used alone or in combination of two or more. The amount of the catalyst used is 0.01% to 10% by weight, preferably 0.1% to 5% by weight, relative to the total weight of bisphenol A and α,α,α',α'-tetramethylbenzenedimethanol (or diisopropenylbenzene, or halogen compounds such as α,α,α',α'-tetramethylbenzene difluoride, α,α,α',α'-tetramethylbenzene dichloride, α,α,α',α'-tetramethylbenzene dibromide, α,α,α',α'-tetramethylbenzene diiodide) as the reaction substrate. If the amount of the catalyst used is too much, there is a risk of decomposition of bisphenol A, and if the amount of the catalyst used is too little, there is a risk of slowing down the reaction. As the solvent used, for example, aromatic solvents such as toluene and xylene, aliphatic solvents such as cyclohexane and n-hexane, ethers such as diethyl ether and diisopropyl ether, ester solvents such as ethyl acetate and butyl acetate, ketone solvents such as methyl isobutyl ketone and cyclopentanone, etc., can be listed as non-water-soluble solvents, but are not limited to these, and two or more thereof can also be used in combination. In addition, in addition to the use of the non-water-soluble solvent, aprotic polar solvents can also be used in combination. For example, dimethyl sulfone, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone, etc. can be listed, and two or more thereof can also be used in combination. When using aprotic polar solvents, it is preferred to use a solvent with a higher boiling point than the non-water-soluble solvent used in combination.The reaction temperature is preferably 80°C to 150°C, more preferably 90°C to 140°C, and further preferably 100°C to 130°C. If the reaction temperature is too high, there is a risk of bisphenol A decomposition, and if the reaction temperature is too low, there is a risk that the reaction cannot proceed fully. When using an alcohol raw material, water is produced as a by-product, so it is removed from the system while azeotroping with the solvent when the temperature is raised. After the reaction is completed, the acidic catalyst is neutralized with an alkaline aqueous solution, and a water-insoluble organic solvent is added to the oil layer, and the wastewater is repeatedly washed with water until the wastewater becomes neutral, and then the solvent is removed under heating and reduced pressure. When activated clay or ion exchange resin is used, the reaction solution is filtered after the reaction is completed to remove the catalyst.

[0070] As an example of a preferred structure of the phenol resin represented by the above formula (3), a phenol resin represented by the following formula (4) can be mentioned.

[0071] [Chemistry 6]

[0072]

[0073] (In formula (4), n is the average value of the number of repetitions, 1<n<20.)

[0074] The preferred range of n in the formula (4) is the same as that in the formula (1).

[0075] Hereinafter, the curable resin composition of the present invention will be described.

[0076] In the curable resin composition of the present invention, the epoxy resin represented by the formula (1) can be used alone or in combination with other epoxy resins. When used in combination, the proportion of the epoxy resin represented by the formula (1) in all epoxy resins is preferably 10% to 98% by weight, more preferably 20% to 95% by weight, and further preferably 30% to 95% by weight. By setting the addition amount to 10% by weight or more, improved tracking resistance or high heat resistance and flame retardancy can be exhibited.

[0077] Specific examples of other epoxy resins that can be used in combination with the epoxy resin of the present invention include: polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, o-phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.); polycondensates of the above phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinyl norbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.); Polymers; polycondensates of the phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.); polycondensates of the phenols and aromatic dimethanols (benzenedimethanol, biphenyl dimethanol, etc.); polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethyl biphenyl, etc.); polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.); polycondensates of the bisphenols and various aldehydes or glycidyl ether epoxy resins, alicyclic epoxy resins, glycidylamine epoxy resins, glycidyl ester epoxy resins, etc. obtained by glycidylating alcohols, etc., are not limited to these as long as they are commonly used epoxy resins. These can be used alone or in combination of two or more.

[0078] Examples of the curing agent that can be used in the curable resin composition of the present invention include amine curing agents, acid anhydride curing agents, amide curing agents, and phenol curing agents. Specific examples of the curing agent that can be used include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,2'-diaminodiphenyl sulfone, diethyltoluenediamine, dimethylthiotoluenediamine, diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 4,4 '-Diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetramethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraisopropyldiphenylmethane, 4,4'-methylenebis(N-methylaniline), bis(aminophenyl)fluorene, 3,4'-diaminodiphenyl ether, 4,4'-diamino Diphenyl ether, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)biphenyl, 4,4'-(1,3-phenylenediisopropylidene)dianiline, 4,4'-(1,4-phenylenediisopropylidene)dianiline, naphthalene diamine, benzidine, dimethylbenzidine, international Aromatic amine compounds such as those described in Synthesis Example 1 and Synthesis Example 2 of Publication No. 2017 / 170551; aliphatic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), norbornanediamine, ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, dimer diamine, triethylenetetramine, etc., but are not limited thereto and can be used appropriately according to the properties to be imparted to the composition. In order to ensure the pot life, it is preferred to use aromatic amines, and in the case of imparting instant curability, it is preferred to use aliphatic amines. By using an amine compound containing a difunctional component as a main component as a curing agent, a highly linear network can be constructed during the curing reaction, thereby exhibiting particularly excellent toughness.In addition, amide compounds such as dicyandiamide, polyamide resin synthesized from dimer of linolenic acid and ethylenediamine; anhydride compounds such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride; bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol , bisphenol AD, etc.) or condensation products of phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, o-phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), or condensation products of the phenols and various diene compounds (dicyclopentadiene, terpenes, etc.) Polymers of the phenols described herein (including but not limited to phenolic compounds such as vinylcyclohexene, vinyl cyclohexene, norbornadiene, vinyl norbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.), or polycondensates of the phenols described herein with ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), or polycondensates of the phenols described herein with aromatic dimethanols (benzenedimethanol, biphenyl dimethanol, etc.), or polycondensates of the phenols described herein with aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), or polycondensates of the phenols described herein with aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.), or polycondensates of the bisphenols described herein with various aldehydes, and modified products thereof; imidazole, trifluoroborane-amine complex, guanidine derivatives, etc., but are not limited to these.

[0079] In the curable resin composition of the present invention, the amount of the curing agent used is preferably 0.5 to 1.5 equivalents, particularly preferably 0.6 to 1.2 equivalents, per 1 equivalent of epoxy groups of the epoxy resin. By setting the amount to 0.5 to 1.5 equivalents, good curing properties can be obtained.

[0080] When the curing reaction is carried out using the above-mentioned curing agent, a curing accelerator may be used in combination. Examples of usable hardening accelerators include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole; tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, triethanolamine, and 1,8-diazabicyclo(5,4,0)undecene-7; phosphines or phosphonium compounds such as triphenylphosphine, tri(tolyl)phosphine, tetraphenylphosphonium bromide, and tetraphenylphosphonium tetraphenylborate; organic phosphines such as tributylphosphine; metal compounds such as tin octoate; tetraphenylphosphonium-tetraphenylborate, tetraphenylphosphonium-ethyltriphenylborate, and other tetraphenylboron salts such as 2-ethyl-4-methylimidazole-tetraphenylborate and N-methylmorpholine-tetraphenylborate; carboxylic acid compounds such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthoic acid, and salicylic acid; and the like. From the viewpoint of promoting the curing reaction between the amine compound and the epoxy resin, a carboxylic acid compound such as salicylic acid is preferred. The curing accelerator may be used in an amount of 0.01 to 15 parts by weight based on 100 parts by weight of the epoxy resin as required.

[0081] Furthermore, in the curable resin composition of the present invention, an inorganic filler may be added as needed. As inorganic fillers, crystalline silica, fused silica, alumina, zircon, calcium silicate, calcium carbonate, silicon carbide, silicon nitride, boron nitride, zirconium oxide, forsterite, steatite, spinel, titanium dioxide, talc, etc. powder or beads formed by spheroidizing these, etc., can be cited, but are not limited to these. These can be used alone or in combination. The amount of these inorganic fillers used varies depending on the purpose, but for example, when used for the sealant application of a semiconductor, in terms of the heat resistance, moisture resistance, mechanical properties, flame retardancy, etc. of the cured product of the curable resin composition, it is preferably used in a proportion of 20% by weight or more in the curable resin composition, more preferably 30% by weight or more, especially in order to increase the linear expansion coefficient relative to the lead frame, and further preferably in a proportion of 70% by weight to 95% by weight.

[0082] In the curable resin composition of the present invention, a release agent may be formulated to facilitate demolding from a mold during molding. As a release agent, any of the known ones may be used, for example, ester waxes such as carnauba wax and montan wax; fatty acids such as stearic acid and palmitic acid and their metal salts; polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene, etc. These may be used alone or in combination of two or more. The amount of these release agents formulated is preferably 0.5 wt% to 3 wt% relative to all organic components. If it is less than this, demolding from the mold will deteriorate, and if it is more than this, adhesion to the lead frame, etc. will deteriorate.

[0083] In the curable resin composition of the present invention, a coupling agent may be adjusted to improve the adhesion between the inorganic filler and the resin component. As a coupling agent, any of the existing known ones can be used, for example, various alkoxysilane compounds such as vinyl alkoxysilane, epoxy alkoxysilane, styryl alkoxysilane, methacryloxyalkoxysilane, acryloxyalkoxysilane, aminoalkoxysilane, mercaptoalkoxysilane, isocyanate alkoxysilane, alkoxytitanium compounds, aluminum chelates, etc. These can be used alone or in combination of two or more. Regarding the method of adding the coupling agent, the inorganic filler surface can be treated with the coupling agent in advance and then mixed with the resin, or the inorganic filler can be mixed with the coupling agent after mixing the resin.

[0084] Furthermore, the curable resin composition of the present invention may be formulated with known additives as needed. Specific examples of usable additives include polybutadiene and modified products thereof, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide compounds, cyanate compounds, silicone gel, silicone oil, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.

[0085] The curable resin composition of the present invention is obtained by uniformly mixing the above-mentioned components. The curable resin composition of the present invention can be easily made into a cured product by the same method as the conventionally known method. For example, the curable resin composition of the present invention is obtained by fully mixing the epoxy resin and the curing agent, and the curing accelerator, inorganic filler, release agent, silane coupling agent and additives as required using an extruder, a kneader, a roller, etc. until they are uniform, and then the curable resin composition is molded by melt casting, transfer molding, injection molding, compression molding, etc., and then heated at 80°C to 200°C for 2 hours to 10 hours to obtain a cured product.

[0086] In addition, the curable resin composition of the present invention may also contain a solvent as needed. The curable resin composition (varnish) containing a solvent is impregnated into a fibrous material (substrate) such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, paper, etc. and heated and dried to obtain a prepreg, and the obtained prepreg is hot-pressed to form a cured product of the curable resin composition of the present invention. The solvent content of the curable resin composition is generally 10% to 70% by weight, preferably about 15% to 70% by weight, based on the internal ratio. As the solvent, for example, γ-butyrolactones; amide solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-dimethylimidazolidinone; sulfones such as tetramethylene sulfone; ether solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and propylene glycol monobutyl ether, preferably mono- or di-lower (carbon number 1-3) alkyl ethers of lower (carbon number 1-3) alkanediols; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, more preferably di-lower (carbon number 1-3) alkyl ketones in which two alkyl groups may be the same or different; aromatic solvents such as toluene and xylene, etc. These may be used alone or as a mixed solvent of two or more.

[0087] In addition, by applying the epoxy resin varnish on a release film and removing the solvent under heating to B-stage, a sheet-shaped adhesive (also simply referred to as a sheet) can be obtained. The sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer substrate or the like.

[0088] The cured product obtained in the present invention can be used for various purposes. Specifically, general uses of thermosetting resins such as epoxy resins can be listed, for example, adhesives, coatings, coating agents, forming materials (including sheets, films, FRP, etc.), insulating materials (including printed circuit boards, wire coatings, etc.), sealants, and additives to other resins, etc.

[0089] Examples of adhesives include adhesives for civil engineering, construction, automobiles, general business, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include adhesives for semiconductors such as interlayer adhesives for multilayer substrates such as build-up substrates, die bonding agents, and bottom fillers; bottom fillers for ball grid array (BGA) enhancement, anisotropic conductive film (ACF), anisotropic conductive paste (ACP) and other mounting adhesives.

[0090] Examples of the sealant include potting seals, immersion seals, and transfer mold seals for capacitors, transistors, diodes, light-emitting diodes, ICs, large scale integration circuits (LSIs), and the like; potting seals for ICs and LSIs such as chip on board (COB), chip on film (COF), and tape automated bonding (TAB); bottom fillers for flip chips; and sealing (including reinforcement bottom fillers) during installation of IC packages such as quad flat packages (QFPs), ball grid arrays (BGAs), and chip size packages (CSPs).

[0091] Example

[0092] Next, the present invention is described in more detail by way of examples. Unless otherwise specified, parts are parts by weight. Furthermore, the present invention is not limited to these examples. In addition, in the examples, the epoxy equivalent is measured by a method in accordance with Japanese Industrial Standards (JIS) K-7236, and the softening point is measured by a method in accordance with JIS K-7234. The softening point is measured using a softening point tester FP90 from METTLER TOLEDO. The hydroxyl equivalent is determined by acetylation of the sample with acetic anhydride in a pyridine solution, decomposition of the remaining anhydride with water after the acetylation is completed, titration with a 0.5N KOH ethanol solution by a potentiometric titrator, and determination of the amount of free acetic acid, and the hydroxyl equivalent is obtained based on the result.

[0093] GPC (Gel Permeation Chromatography) Analysis

[0094] Column: SHODEX GPC KF-601 (two), KF-602, KF-602.5, KF-603

[0095] Flow rate: 0.5ml / min.

[0096] Column temperature: 40℃

[0097] Solvent used: tetrahydrofuran (THF)

[0098] Detector: RI (differential refractometer)

[0099] [Synthesis example 1]

[0100] Add 250 parts of toluene, 142.7 parts of bisphenol A, 97.1 parts of α,α,α',α'-tetramethylbenzenedimethanol, and 2.5 parts of p-toluenesulfonic acid, raise the temperature to 125°C and react for 6 hours. The organic layer is washed with water until the waste liquid becomes neutral and concentrated to obtain 192 parts of phenol resin (P1) as a brown solid resin. The number average molecular weight Mn: 1279, the weight average molecular weight Mw: 1774, the hydroxyl equivalent is 203.8 g / eq, the ICI viscosity (150°C) is 0.82 Pa·s, and the softening point is 98.0°C. The GPC graph is shown in Figure 1 .

[0101] [Synthesis example 2]

[0102] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 180 parts of the phenol resin (P1) obtained in Synthesis Example 1, 326.7 parts of epichlorohydrin, 163.3 parts of dimethyl sulfoxide, and 3.6 parts of water were added, and the internal temperature was raised to 50°C. After 37.8 parts of sodium hydroxide were added in batches over 1.5 hours, the reaction was carried out at 55°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 500 parts of methylisobutyl ketone (MIBK) were added, and the organic layer was washed once with 500 parts of water. The organic layer was returned to the reaction container, 11.9 parts of a 30 wt% sodium hydroxide aqueous solution was added, and the reaction was carried out at 75°C for 1 hour. After cooling, the organic layer was washed four times with 100 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 201 parts of the target compound (E1) as a light yellow solid resin. The number average molecular weight Mn is 1253, the weight average molecular weight Mw is 1947, the epoxy equivalent is 298.6 g / eq, the ICI viscosity (150°C) is 0.44 Pa·s, and the softening point is 80.9°C. The GPC graph is shown in Figure 2 .

[0103] [Synthesis example 3]

[0104] Add 200 parts of toluene, 235.3 parts of phenol, 388.5 parts of α,α,α',α'-tetramethylbenzenedimethanol, and 7.6 parts of p-toluenesulfonic acid, raise the temperature to 125°C and react for 5 hours. Add 200 parts of toluene, wash the organic layer with water until the waste liquid becomes neutral and concentrate it to obtain 475 parts of phenol resin (P2) as a light yellow solid resin. The number average molecular weight Mn: 822, the weight average molecular weight Mw: 1181, and the hydroxyl equivalent is 254.0 g / eq. The GPC graph is shown in Figure 3 .

[0105] [Synthesis Example 4]

[0106] While nitrogen was purged in a flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer, 400 parts of the phenol resin (P2) obtained in Synthesis Example 3, 582.7 parts of epichlorohydrin, 291.4 parts of dimethyl sulfoxide, and 6.4 parts of water were added, and the internal temperature was raised to 50°C. After adding 67.3 parts of sodium hydroxide in batches over 1.5 hours, the mixture was reacted at 55°C for 2 hours and at 70°C for 1 hour. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 900 parts of MIBK were added, and the organic layer was washed once with 400 parts of water. The organic layer was returned to the reaction vessel, and 21.1 parts of a 30wt% sodium hydroxide aqueous solution were added, and the mixture was reacted at 75°C for 1 hour. After cooling, the organic layer was washed six times with 100 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 455 parts of the target compound (E2) as a light yellow solid resin. The number average molecular weight Mn is 827, the weight average molecular weight Mw is 1352, the epoxy equivalent is 334.0 g / eq, the ICI viscosity (150°C) is 0.17 Pa·s, and the softening point is 69.7°C. The GPC graph is shown in Figure 4 .

[0107] [Synthesis example 5]

[0108] A flask equipped with a thermometer, a cooling tube, a fractionating tube, and a stirrer was purged with nitrogen, and a bisphenol A novolac resin (a condensate of bisphenol A and formaldehyde synthesized with reference to Comparative Example 1 described in Japanese Patent Laid-Open No. 2014-198755, hydroxyl equivalent: 118 g / eq, ICI viscosity (150° C.) as the detection limit (6.8 Pa·s or more), softening point of 120.6° C., number average molecular weight Mn: 1907, weight average molecular weight Mw: 4533, GPC chart shown in FIG. 1) was added. Figure 5 . ) 100 parts, epichlorohydrin 415 parts, dimethyl sulfoxide 157 parts, water 28.2 parts, the internal temperature was raised to 35 ° C. After adding 36.1 parts of sodium hydroxide in batches over 3 hours, the reaction was carried out at 35 ° C for 2 hours and at 70 ° C for 0.5 hours. Unreacted epichlorohydrin and solvent were distilled off under heating and reduced pressure. 440 parts of MIBK were added, and the organic layer was washed once with 170 parts of water. The organic layer was returned to the reaction vessel, and 8 parts of methanol, 22.6 parts of water, and 22.6 parts of 30wt% sodium hydroxide aqueous solution were added, and the reaction was carried out at 75 ° C for 1 hour. After cooling, the organic layer was washed four times with 100 parts of water, and the solvent was distilled off under heating and reduced pressure to obtain 147.5 parts of the target compound (E3) as a light yellow solid resin. The number average molecular weight Mn is 2233, the weight average molecular weight Mw is 39351, the epoxy equivalent is 199.0 g / eq, the ICI viscosity (150°C) is 1.22 Pa·s, and the softening point is 81.6°C. The GPC graph is shown in Figure 6 .

[0109] [Example 1, Comparative Example 1, Comparative Example 2]

[0110] To the epoxy resin (E1) obtained in Synthesis Example 2, the epoxy resin (E2) obtained in Synthesis Example 4, and the epoxy resin (E3) obtained in Synthesis Example 5, a biphenyl aralkyl phenol resin (GPH-65 manufactured by Nippon Kayaku Co., Ltd.) as a curing agent, triphenylphosphine (TPP, manufactured by Tokyo Chemical Industry Co., Ltd.) as a catalyst, and silica gel (fused silica MSR-2212, manufactured by Ryosen) as an inorganic filler were respectively prepared in the ratios shown in Table 1, and the mixture was uniformly mixed and kneaded using a roll mill to obtain a curable resin composition.

[0111] The curable resin composition was crushed and tableted using a tabletting machine, and the tableted curable resin composition was transfer molded (175°C for 60 minutes to 15 minutes), and then released from the mold and cured under the conditions of 160°C for 2 hours + 180°C for 6 hours to obtain a test piece for evaluation.

[0112] The evaluation test pieces were measured under the following conditions. The results are shown in Table 1.

[0113] <Heat resistance test (Tg)>

[0114] The glass transition temperature (temperature at which tan δ reaches a maximum value) was measured using a dynamic viscoelasticity tester.

[0115] Dynamic viscoelasticity tester: DMA-2980 manufactured by TA-instruments

[0116] Heating rate: 2℃ / min

[0117] Frequency: 10Hz

[0118] <CTI test>

[0119] Applicable standards IEC-Pub.60112-2003 (4th edition) and JIS-C2134-2007

[0120] Test voltage: 400V~600V

[0121] Test solution: 0.1% ammonium chloride aqueous solution

[0122] Add 50 drops or continue to add drops until the test piece breaks.

[0123] The temperature and humidity of the test room are 21℃~23℃40%RH~45%RH

[0124] Test equipment: YST-112 tracking tester manufactured by Yamayo Testing Machine Co., Ltd.

[0125] Test sample shape: diameter 50mm, thickness 3mm

[0126] 1 point per piece

[0127] <Flame retardancy test>

[0128] The test piece was held vertically in the fixture, the flame of the burner was adjusted to a 19 mm blue flame, and the lower center of the test piece was in contact with 9.5 mm of the flame for 10 seconds. After contact with the flame, the burner was removed and the burning duration was measured. After the flame was extinguished, it was immediately in contact with the flame for 10 seconds, and then the burner was removed and the burning duration was measured. The total value of the burning time of each sample 10 times is shown in Table 1.

[0129] [Table 1]

[0130]

[0131] The numerical value after n in the parentheses of the tracking resistance test indicates the number of samples. The 500 V test of Comparative Example 2 showed that the test piece was broken by 13 drops in the first test, but was not broken even by 50 drops in the second test.

[0132] From the results in Table 1, it was confirmed that Example 1 had high heat resistance, high tracking resistance, and high flame retardancy.

[0133] Industrial Applicability

[0134] The epoxy resin of the present invention can be effectively used in insulating materials for electrical and electronic parts (high-reliability semiconductor sealing materials, etc.) and laminated boards (printed wiring boards, BGA substrates, build-up substrates, etc.), adhesives (conductive adhesives, etc.) or various composite materials represented by CFRP, coatings, etc., and can be particularly effectively used in insulating materials for electrical and electronic parts (high-reliability semiconductor sealing materials, etc.) and laminated boards (printed wiring boards, BGA substrates, build-up substrates, etc.) that require tracking resistance.

Claims

1. An epoxy resin represented by the following formula (1): In formula (1), n ​​is the average value of the number of repetitions, 1<n<20.

2. An epoxy resin represented by the following formula (2): In formula (2), n is the average value of the number of repetitions, 1<n<20.

3. The epoxy resin according to claim 1 or 2, wherein The weight average molecular weight determined by gel permeation chromatography was 1,000 to 3,000.

4. A curable resin composition comprising the epoxy resin according to claim 1 or 2. 5 . The curable resin composition according to claim 4 , further comprising a curing accelerator.

6. A cured product obtained by curing the curable resin composition according to claim 4.

7. A cured product obtained by curing the curable resin composition according to claim 5.

Citation Information

Patent Citations

  • Novolac phenol resin and application of the same

    JP2014198755A

  • Modified epoxy resin, and curable resin composition

    JP2015147854A

  • Maleimide resin, curable resin composition and cured product of same

    WO2017170551A1

  • Epoxy resin composition, resin sheet, prepreg and metal-clad laminated sheet, printed circuit board, and semiconductor device

    CN106661195A

  • Epoxy resin, epoxy resin composition and cured product of the epoxy resin

    CN111378093A