Process for producing water-based polyester resin, water-based polyester resin, and water-based coating composition

By controlling the ratio and acid value of recycled polyester to polycarboxylic acid compounds containing metal sulfonate groups, an aqueous polyester resin with excellent water dispersibility and stability is produced, solving the problem of insufficient dispersibility and stability of existing aqueous polyester resins and reducing environmental impact.

CN117120506BActive Publication Date: 2026-11-24GOO CHEM IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280022166.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-10-22
Filing Date
2022-03-09
Publication Date
2026-11-24
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

Existing technologies for producing water-based polyester resins suffer from insufficient water dispersibility and stability, especially when surfactants are not used, and when recycled polyester is used, the environmental impact is significant.

Method used

Aqueous polyester resins are produced by combining recycled polyester with polycarboxylic acid compounds containing metal sulfonate groups, controlling the proportion of each component, and producing water-based polyester resins through ester formation and depolymerization reactions. The acid value is controlled within a specific range, and the crystallinity is reduced to improve water dispersibility and stability.

Benefits of technology

Aqueous polyester resins with excellent water dispersibility and good stability are produced, reducing environmental impact, maintaining adhesion and transparency similar to terephthalic acid derivatives, and improving long-term water dispersibility and aging stability of solution haze.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004453272920000051
    Figure BDA0004453272920000051
  • Figure BDA0004453272920000181
    Figure BDA0004453272920000181
  • Figure BDA0004453272920000201
    Figure BDA0004453272920000201
Patent Text Reader

Abstract

A method for producing a water-based polyester resin includes a first step and a second step. The first step includes using recycled polyester, a polycarboxylic acid component containing polycarboxylic acid residues but not terephthalic acid, and a polyol component to induce an esterification reaction and a depolymerization reaction. The second step includes inducing a polycondensation reaction by reducing pressure. The first step includes: using recycled polyester in an amount such that the proportion of terephthalic acid residues is equal to or greater than 20% by mass and equal to or less than 72% by mass; and using a polycarboxylic acid compound containing metal sulfonate groups in an amount such that the proportion of polycarboxylic acid residues containing metal sulfonate groups is equal to or greater than 5% by mass and equal to or less than 32% by mass. The resin produced thereby has an acid value equal to or less than 10 mg KOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure generally relates to methods for producing waterborne polyester resins, waterborne polyester resins, and waterborne coating compositions. More particularly, this disclosure relates to methods for producing waterborne polyester resins using recycled polyester, waterborne polyester resins produced using recycled polyester, and waterborne coating compositions comprising such waterborne polyester resins. Background Technology

[0002] It has been proposed that, from an environmentally friendly perspective, aqueous polyester resins dispersible in water or water containing hydrophilic solvents should be produced by using recycled polyester as a material and copolymerizing its hydrophilic component (see Patent Documents 1 to 4). However, aqueous polyester resins produced by any of the methods in these documents tend to exhibit relatively low water dispersibility. Furthermore, it is difficult to maintain the dispersion of aqueous polyester resins in a liquid for extended periods. In other words, the resin dispersion tends to have relatively low stability. These trends are particularly pronounced when using polycarboxylic acids with metal sulfonate groups as their hydrophilic components.

[0003] These trends may be due to the following reasons. First, the main component of recycled polyester is polyethylene terephthalate (PET), a resin with high crystallinity. Second, the molecular weight of currently available recycled polyester is inconsistent and varies depending on the type of waste polyester material being recycled or the method of post-processing the waste polyester material. In other words, these trends are related to the rigidity of the molecular structure of aqueous polyester resins and the varying degrees of depolymerization reactions that occur in recycled polyester during its production process.

[0004] On the other hand, examples of methods for improving the water dispersibility of aqueous polyester resins and the stability of their resin dispersions include reducing the blending ratio of recycled polyester and adding surfactants as dispersing aids for resin dispersion. However, from an environmental perspective, it is preferable to make the blending ratio of recycled polyester as high as possible. Furthermore, if surfactants are used, they may leach onto the resin film formed by the resin dispersion, thus sometimes causing a decrease in the physical properties of the resin film or contamination of other materials when the surfactant comes into contact with the material. In addition, the use of dissimilar materials (e.g., surfactants) reduces the recyclability of the material, thereby increasing the environmental impact.

[0005] It can be seen that there is a growing demand for aqueous polyester resins produced from recycled polyester that exhibit excellent water dispersibility, even without any surfactant, and good stability when used as resin dispersions. Furthermore, aqueous polyesters produced using recycled polyesters sometimes need to possess properties comparable to those produced using non-recycled terephthalic acid or terephthalic acid derivatives not derived from recycled polyesters. In particular, aqueous polyester resins need to have good adhesion to resins and metals and excellent transparency (e.g., sufficiently low haze). Moreover, dispersions of aqueous polyester resins not only need to exhibit good long-term water dispersibility but also require improved stability, such as aging stability of solution haze.

[0006] Reference List

[0007] Patent documents

[0008] Patent Document 1: WO 2001 / 016208 A1

[0009] Patent Document 2: JP H05-271612A

[0010] Patent Document 3: WO 2003 / 051956 A1

[0011] Patent Document 4: JP 2001-505608 A Summary of the Invention

[0012] The problem this disclosure addresses is to provide an aqueous polyester resin having the following advantageous characteristics, and an aqueous coating composition comprising such an aqueous polyester resin. Specifically, the aqueous polyester resin provided by this disclosure not only exhibits excellent water dispersibility, for example, even without any surfactant, but also demonstrates good stability when used as a resin dispersion, while reducing environmental impact. Furthermore, the aqueous polyester resin contains terephthalic acid residues derived from recycled polyester and will still possess the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyester. Moreover, the resin dispersion of the aqueous polyester resin not only exhibits good long-term water dispersibility but also improves its stability, such as the aging stability of solution haze.

[0013] A method for producing a water-based polyester resin according to one aspect of this disclosure is a method for producing a water-based polyester resin using recycled polyester. The method includes a first step and a second step. The first step includes initiating an esterification reaction and a depolymerization reaction using recycled polyester, a polycarboxylic acid component containing polycarboxylic acid residues but not terephthalic acid, and a polyol component. The second step includes initiating a polycondensation reaction by reducing pressure. The polycarboxylic acid component comprises: at least one polycarboxylic acid compound containing a metal sulfonate group selected from polycarboxylic acids, their esters, and acid anhydrides, each having a metal sulfonate group and containing a metal sulfonate group; and at least one additional polycarboxylic acid compound selected from polycarboxylic acids other than terephthalic acid and polycarboxylic acid compounds containing metal sulfonate groups, their esters, and acid anhydrides. The first step includes: using recycled polyester in an amount such that the proportion of terephthalic acid residues relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 20% by mass and equal to or less than 72% by mass; and using a polycarboxylic acid compound containing metal sulfonate groups in an amount such that the proportion of polycarboxylic acid residues containing metal sulfonate groups relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 5% by mass and equal to or less than 32% by mass. The resulting aqueous polyester resin has an acid value equal to or less than 10 mg KOH / g.

[0014] According to another aspect of this disclosure, the aqueous polyester resin is produced by the method described above for producing aqueous polyester resin.

[0015] According to another aspect of this disclosure, the aqueous polyester resin comprises: terephthalic acid residues derived from recycled polyester, and polycarboxylic acid residues other than terephthalic acid residues. The polycarboxylic acid residues comprise: polycarboxylic acid residues containing metal sulfonate groups, and other polycarboxylic acid residues other than terephthalic acid residues and polycarboxylic acid residues containing metal sulfonate groups. The proportion of terephthalic acid residues is equal to or greater than 20% by mass and equal to or less than 72% by mass relative to all polycarboxylic acid residues contained in the aqueous polyester resin. The proportion of polycarboxylic acid residues containing metal sulfonate groups is equal to or greater than 5% by mass and equal to or less than 32% by mass relative to all polycarboxylic acid residues contained in the aqueous polyester resin. The acid value of the aqueous polyester resin is equal to or less than 10 mg KOH / g.

[0016] According to another aspect of this disclosure, the aqueous coating composition comprises an aqueous polyester resin. The aqueous polyester resin comprises an aqueous polyester resin produced by the above method or the above-described aqueous polyester resin. Detailed Implementation

[0017] <Method for producing water-based polyester resin>

[0018] A method for producing an aqueous polyester resin according to an exemplary embodiment (hereinafter referred to as "production method (X)") is a method for producing an aqueous polyester resin according to an exemplary embodiment using recycled polyester. Production method (X) includes a first step and a second step.

[0019] The production method (X) according to this embodiment can produce an aqueous polyester resin with the following advantageous characteristics. Specifically, the aqueous polyester resin not only exhibits excellent water dispersibility, for example, even without any surfactant, but also exhibits good stability when used as a resin dispersion, while reducing environmental impact. Furthermore, the aqueous polyester resin contains terephthalic acid residues derived from recycled polyester and still possesses the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyester. Moreover, the resin dispersion of the aqueous polyester resin not only exhibits good long-term water dispersibility but also improved stability, such as aging stability of solution haze. The inventors have discovered that the above-mentioned problems can be solved by: when producing the aqueous polyester resin using not only recycled polyester but also a polycarboxylic acid compound containing metal sulfonate groups as a hydrophilic component, using a polycarboxylic acid compound other than terephthalic acid and the polycarboxylic acid compound containing metal sulfonate groups as the polycarboxylic acid component; setting the corresponding ratio of the recycled polyester to be used and the polycarboxylic acid compound containing metal sulfonate groups within a specific range; and making the acid value of the aqueous polyester resin equal to or less than a specific value. In other words, production method (X) can produce aqueous polyester resins with the aforementioned advantageous characteristics. Specifically, the aqueous polyester resins not only exhibit excellent water dispersibility, for example, even without any surfactant, but also demonstrate good stability when used as resin dispersions, while reducing environmental impact. Furthermore, the aqueous polyester resins contain terephthalic acid residues derived from recycled polyesters and still possess the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyesters. Moreover, resin dispersions of the aqueous polyester resins not only exhibit good long-term water dispersibility but also improved stability, such as aging stability of solution haze.

[0020] For example, these advantages may be achieved for the following reasons. First, setting the proportion of recycled polyester used to a certain value or higher can, for example, reduce the amount of materials derived from fossil fuels and reduce waste, thereby helping to reduce environmental impact. Furthermore, the resin dispersion of the aqueous polyester resin to be produced can be prepared, for example, using water or water containing hydrophilic organic solvents without the use of any surfactants, which also helps to reduce environmental impact. In addition, by using additional polycarboxylic acid compounds, setting the proportion of recycled polyester used to a certain value or lower, setting the proportion of polycarboxylic acid compounds containing metal sulfonate groups to a specific range, and setting the acid value of the aqueous polyester resin to a specific value or lower, the crystallinity of the aqueous polyester resin can be reduced to an appropriate level while achieving a proper balance between the hydrophobic and hydrophilic portions of the aqueous polyester resin. These and other measures taken according to this embodiment will allow the aqueous polyester resin to have excellent water dispersibility, for example, even without any surfactants, and improve the stability of its resin dispersion. It is not entirely clear why setting the acid value to a specific value or lower achieves these advantages. One possible reason is that reducing the interactions between resin molecules in aqueous polyester resins with carboxyl groups on their side chains or ends will help improve the water dispersibility of the aqueous polyester resin and the stability of its resin dispersion. Another possible reason is that using additional polycarboxylic acid compounds as polycarboxylic acid components in production method (X) can appropriately induce depolymerization reactions in recycled polyesters with various molecular weights. Furthermore, for the same reasons as the excellent water dispersibility and good stability of the aforementioned aqueous polyester resins and their resin dispersions, resin properties such as adhesion and transparency, long-term water dispersibility, and their stability such as the aging stability of solution haze will also be significantly improved, regardless of whether the terephthalic acid residues are derived from recycled polyester or from unused terephthalic acid or terephthalic acid derivatives.

[0021] The aqueous polyester resin produced by production method (X) (hereinafter also referred to as "resin (Y)") is a polyester resin and has structural units composed of polycarboxylic acid residues and structural units composed of polyol residues. The polycarboxylic acid residues contained in resin (Y) or the polycarboxylic acid component are generally represented by the following formula (1). The polyol residues contained in resin (Y) or the polyol component are generally represented by the following formula (2). Resin (Y) has terephthalic acid residues derived from recycled polyester as structural units composed of polycarboxylic acid residues.

[0022]

[0023] In equation (1), R 1 It refers to a hydrocarbon group, either substituted or unsubstituted, having 1 to 50 carbon atoms.

[0024] In equation (2), R 2 It refers to a hydrocarbon group, either substituted or unsubstituted, having 1 to 50 carbon atoms.

[0025] In formulas (1) and (2), * represents a group adjacent to the residue represented by formula (1) or formula (2) or a site bonded to an adjacent residue.

[0026] R 1 and R 2 Examples of substituents for hydrocarbon groups include hydroxyl groups such as alcohol hydroxyl and phenolic hydroxyl, carboxyl groups, acyl groups, acyloxy groups, halogen atoms, alkoxy groups, and alkoxycarbonyl groups.

[0027] The following steps will be described.

[0028] [First Step]

[0029] The first step involves using recycled polyester, polycarboxylic acid components, and polyol components as reactants to induce ester formation and depolymerization reactions.

[0030] As used herein, "ester formation reaction" refers to a reaction in which a polycarboxylic acid component and a polyol component form an ester compound through, for example, dehydration condensation or de-alcoholization condensation.

[0031] The depolymerization reaction used in this article refers to the reaction in which recycled polyester and polycarboxylic acid components, polyol components, or ester compounds formed therefrom form polyesters with lower molecular weights.

[0032] In the first step, all components of the reactant material can be mixed at once, or one or more components or a certain amount of components forming part of the reactant material can be mixed sequentially. Alternatively, after some reactant material has been mixed and a reaction has been initiated, other reactant material can be mixed, and a further reaction can be initiated. These mixing and reaction processes can be repeated.

[0033] In the first step, after blending the recycled polyester, the polycarboxylic acid component, and the polyol component, an esterification reaction and a depolymerization reaction can be initiated. Alternatively, after blending the polycarboxylic acid component and the polyol component, an esterification reaction can be initiated, and then recycled polyester can be added, which can then initiate a depolymerization reaction.

[0034] The reaction materials are typically mixed in equipment such as a reactor used to carry out the production method (X).

[0035] The reactants will be described one by one below.

[0036] (Recycled Polyester)

[0037] Recycled polyester contains polyethylene terephthalate as its main component. As used herein, "main component" refers to the component having the highest content ratio. The proportion of polyethylene terephthalate relative to recycled polyester is preferably equal to or greater than 90% by mass, more preferably equal to or greater than 95% by mass, and even more preferably equal to or greater than 99% by mass. This allows the aqueous polyester resin to be converted into a substantially single material. The proportion can even be 100% by mass.

[0038] Examples of recycled polyester include material-recycled polyester, mechanically recycled polyester, and chemically recycled polyester. As used herein, "material-recycled polyester" refers to polyester obtained by sorting, crushing, washing, and other processes to remove contaminants and foreign particles from used or discarded polyester molded products such as bottles, containers, and films, and then converting these so-called products into sheets. As used herein, "mechanically recycled polyester" refers to polyester in which contaminants within the resin have been removed by treating the sheets of material-recycled polyester for a period of time, for example, under high temperature and reduced pressure, and its degree of polymerization has been adjusted by repolymerizing a portion of the polyester. As used herein, "chemically recycled polyester" refers to polyester obtained by breaking down the polyester to the monomer level and then repolymerizing the monomers.

[0039] The intrinsic viscosity (IV value, in dl / g) of the recycled polyester is preferably equal to or greater than 0.40 and equal to or less than 1.20, and more preferably equal to or greater than 0.45 and equal to or less than 1.00, in order to more appropriately induce depolymerization in the second step. Intrinsic viscosity is commonly used as an indicator of the degree of polymerization of a polymer.

[0040] From the perspective of further reducing environmental impact, the recycled polyester preferably includes at least one of material recycled polyester or mechanically recycled polyester, and from the perspective of improving the quality of aqueous polyester resins, it is more preferably to include mechanically recycled polyester. Even more preferably, the recycled polyester includes mechanically recycled polyester obtained by recycling PET bottles or PET films.

[0041] (Polycarboxylic acid components)

[0042] The polycarboxylic acid component is a compound containing polycarboxylic acid residues other than terephthalic acid. The polycarboxylic acid component provides the structural units composed of polycarboxylic acid residues in the resin (Y).

[0043] The polycarboxylic acid component comprises at least one selected from polycarboxylic acids, their esters, and acid anhydrides, each having a metal sulfonate group (hereinafter also referred to as "the polycarboxylic acid compound (A) with a metal sulfonate group"). Furthermore, the polycarboxylic acid component also comprises at least one selected from polycarboxylic acids other than the polycarboxylic acid compound (A) with a metal sulfonate group and terephthalic acid, their esters, and acid anhydrides (hereinafter referred to as "another polycarboxylic acid compound (B)").

[0044] (Polycarboxylic acid compounds containing metal sulfonate groups)

[0045] The polycarboxylic acid compound (A) containing a metal sulfonate group is at least one compound selected from polycarboxylic acids, their esters, and acid anhydrides, each having a metal sulfonate group. The polycarboxylic acid compound (A) containing a metal sulfonate group contains a polycarboxylic acid residue with a metal sulfonate group. The polycarboxylic acid compound (A) containing a metal sulfonate group provides the structural unit in the resin (Y) consisting of polycarboxylic acid residues with metal sulfonate groups.

[0046] As used herein, "metal sulfonate group" refers to a metal base with a sulfonyl group (-SO3H), and can be derived from, for example, -SO3 - (M n+ ) 1 / n (where M) n+ The metal cation is represented as an n-valent metal cation, where n is an integer falling within the range of 1 to 6. In this case, n preferably falls within the range of 1 to 3, more preferably 1 or 2, and even more preferably 1. Examples of metal cations include: monovalent metal cations, such as alkali metal ions, including lithium ions, sodium ions, potassium ions, rubidium ions, and cesium ions; and divalent metal cations, such as alkaline earth metal ions, including magnesium ions, calcium ions, strontium ions, and barium ions. The polycarboxylic acid compound (A) containing a metal sulfonate group may have one, two, or more metal sulfonate groups, but preferably has a single metal sulfonate group.

[0047] Examples of polycarboxylic acid compounds (A) containing metal sulfonate groups include compounds in which one or more metal sulfonate groups are bonded to a hydrocarbon group contained in the polycarboxylic acid compound. Polycarboxylic acid compounds (A) containing metal sulfonate groups preferably include polycarboxylic acid compounds having a single metal sulfonate group.

[0048] Examples of polycarboxylic acid compounds (A) containing metal sulfonate groups include sulfoisophthalates, such as 2-sulfoisophthalate, 4-sulfoisophthalate and 5-sulfoisophthalate, aromatic dicarboxylate such as 4-sulfo-2,6-naphthalenedicarboxylate, and their esters and anhydrides.

[0049] The polycarboxylic acid compound (A) containing a metal sulfonate group preferably comprises at least one selected from aromatic dicarboxylic acids and their esters and acid anhydrides. The polycarboxylic acid compound (A) containing a metal sulfonate group more preferably comprises at least one selected from sulfophenyl dicarboxylic acids and their esters and acid anhydrides. The polycarboxylic acid compound (A) containing a metal sulfonate group even more preferably comprises at least one selected from 5-sulfoisophthalate and its esters and acid anhydrides.

[0050] (Other polycarboxylic acid compounds)

[0051] The additional polycarboxylic acid compound (B) is at least one compound selected from polycarboxylic acid compounds other than terephthalic acid and polycarboxylic acid compounds containing metal sulfonate groups, their esters, and acid anhydrides. The additional polycarboxylic acid compound (B) comprises polycarboxylic acid residues other than terephthalic acid residues and polycarboxylic acid residues containing metal sulfonate groups. The additional polycarboxylic acid compound (B) provides the structural unit in the resin (Y) composed of the additional polycarboxylic acid residues.

[0052] Other examples of polycarboxylic acid compounds (B) include those selected from at least one of the following: aromatic dicarboxylic acids, such as phthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid and 2,5-furandicarboxylic acid; alicyclic dicarboxylic acids, such as 1,4-cyclohexanedicarboxylic acid; dicarboxylic acids, such as aliphatic dicarboxylic acids, including succinic acid, adipic acid, sebacic acid and dodecanoic acid; and their esters and anhydrides.

[0053] Other examples of polycarboxylic acid compounds (B) include those selected from at least one of the following: aromatic tricarboxylic acids, such as trimellitic acid, benzotriic acid, pyromellitic acid, and 1,2,5-naphthalenetricarboxylic acid; alicyclic tricarboxylic acids, such as 1,2,4-cyclohexanetricarboxylic acid; aliphatic tricarboxylic acids, such as 1,2,3-butanetricarboxylic acid; trivalent or higher-valent polycarboxylic acids, such as pyromellitic acid; and their esters and anhydrides.

[0054] From the perspective of reducing environmental impact, it is also preferable to use polycarboxylic acid compounds (B) derived from biomass. Examples of polycarboxylic acid compounds (B) derived from biomass include 2,5-furandicarboxylic acid, succinic acid, adipic acid, and sebacic acid.

[0055] The additional polycarboxylic acid compound (B) preferably comprises at least one selected from dicarboxylic acids and their esters and acid anhydrides. More preferably, the additional polycarboxylic acid compound (B) comprises at least one selected from dicarboxylic acids and their esters and acid anhydrides that do not have functional groups other than a carboxyl group.

[0056] From the perspective of further improving the water dispersibility of waterborne polyester resin and the stability of its resin dispersion by more sufficiently reducing the crystallinity of waterborne polyester resin, the additional polycarboxylic acid compound preferably includes at least one selected from aromatic dicarboxylic acids and their esters and acid anhydrides, and more preferably includes at least one selected from isophthalic acid and 2,6-naphthalenedicarboxylic acid.

[0057] (Polyol component)

[0058] The polyol component is a compound containing polyol residues. The resin (Y) typically has ethylene glycol residues derived from recycled polyester as polyol residues.

[0059] Examples of polyol components include: diol compounds, including: aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; alicyclic diols such as 1,4-cyclohexanediol; aromatic diols such as 1,4-benzyldiethanol and 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene; and ether-containing diols, including diethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, and polytetramethylene ether glycol.

[0060] Examples of polyol components also include ternary or higher-order polyol compounds. Examples of ternary or higher-order polyol compounds include triol compounds, including: aliphatic triols, such as glycerol and trimethylolpropane; alicyclic triols, such as 1,2,4-cyclohexanetriethanol; and aromatic triols, such as benzenetriethanol; and pentaerythritol.

[0061] The polyol component preferably comprises polyol compounds other than ethylene glycol (hereinafter also referred to as "additional polyol compounds"). This can further increase the adhesion of the resin film of resin (Y) to resins, metals, or any other materials with a polar structure. The additional polyol compounds preferably include at least one selected from diol compounds and triol compounds without functional groups other than hydroxyl groups, and more preferably include diol compounds without functional groups other than hydroxyl groups. The additional polyol compounds preferably include at least one selected from diethylene glycol, polyethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanediol, and trimethylolpropane. The other polyol compounds more preferably include at least one selected from diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, and 1,4-cyclohexanediethanol.

[0062] From the perspective of reducing environmental impact, it is also preferable to use polyol components derived from biomass. Examples of biomass-derived polyol components include ethylene glycol, 1,3-propanediol, 1,3-butanediol, and 1,4-butanediol.

[0063] Importantly, in the first step, recycled polyester is used such that the proportion of terephthalic acid residues in the recycled polyester is equal to or greater than 20% by mass and equal to or less than 72% by mass, relative to the total amount of terephthalic acid residues contained in the recycled polyester and the polycarboxylic acid component. If the proportion is less than 20% by mass, the environmental impact reduction is insufficient. If the proportion is greater than 72% by mass, the resin (Y) will not have a low crystallinity, and the water dispersibility will be reduced. The proportion is preferably equal to or greater than 30% by mass, more preferably equal to or greater than 40% by mass, even more preferably equal to or greater than 45% by mass, and particularly preferably equal to or greater than 50% by mass. The proportion is preferably equal to or less than 71% by mass, more preferably equal to or less than 70% by mass, even more preferably equal to or less than 69% by mass, and particularly preferably equal to or less than 68% by mass.

[0064] Equally important is the use of a polycarboxylic acid compound (A) containing metal sulfonate groups in the first step, such that the proportion of the polycarboxylic acid residues containing metal sulfonate groups in the polycarboxylic acid compound (A) is equal to or greater than 5% by mass and equal to or less than 32% by mass relative to the total amount of terephthalic acid residues contained in the recycled polyester and the polycarboxylic acid component. If the proportion is less than 5% by mass, the proportion of the hydrophilic portion of the resin (Y) will be too small to avoid reduced water dispersibility. If the proportion is greater than 32% by mass, the proportion of the hydrophilic portion of the resin (Y) will be too large to frequently cause adhesion of the resin (Y) due to moisture absorption by the resin film. Furthermore, setting the proportion within the aforementioned specific range can further improve the adhesion of the resin (Y) to resins, metals, or any other materials with a polar structure. The proportion is preferably equal to or greater than 6% by mass, more preferably equal to or greater than 7% by mass, even more preferably equal to or greater than 8% by mass, and particularly preferably equal to or greater than 9% by mass. The ratio is preferably equal to or less than 31% by mass, more preferably equal to or less than 29% by mass, even more preferably equal to or less than 27% by mass, and particularly preferably equal to or less than 25% by mass.

[0065] The first step involves using an additional polycarboxylic acid compound (B) in such a proportion, for example, equal to or greater than 3% by mass and equal to or less than 55% by mass, relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component. Setting this proportion within this range allows the resin (Y) to more sufficiently reduce its crystallinity and further improve its water dispersibility and the stability of its resin dispersion. The proportion is preferably equal to or greater than 5% by mass, more preferably equal to or greater than 10% by mass, even more preferably equal to or greater than 13% by mass, and particularly preferably equal to or greater than 15% by mass. The proportion is preferably equal to or less than 50% by mass, more preferably equal to or less than 42% by mass, even more preferably equal to or less than 30% by mass, and particularly preferably equal to or less than 25% by mass.

[0066] If the additional polycarboxylic acid compound (B) contains trivalent or higher-valence polycarboxylic acid compounds, the proportion of the trivalent or higher-valence polycarboxylic acid compound relative to all the additional polycarboxylic acid compounds (B) is preferably equal to or less than 3% by mass. This allows the resin (Y) to further reduce the number of cross-linked structures formed due to the presence of trivalent or higher-valence polycarboxylic acid compounds, thereby further improving its water dispersibility and the stability of its resin dispersion. The proportion is more preferably equal to or less than 2% by mass, even more preferably equal to or less than 1% by mass, and particularly preferably equal to or less than 0.5% by mass. The proportion of trivalent or higher-valence polycarboxylic acid compounds is preferably as small as possible, and can even be 0% by mass.

[0067] The polycarboxylic acid component used in the first step preferably does not contain trivalent or higher-valent polycarboxylic acid compounds. That is, the polycarboxylic acid compound (A) containing metal sulfonate groups to be used and the additional polycarboxylic acid compound (B) to be used preferably do not contain trivalent or higher-valent polycarboxylic acid compounds, and preferably only contain divalent polycarboxylic acid compounds. This can further reduce the acid value of the resin (Y). Furthermore, this allows the resin (Y) to have a smaller number of cross-linked structures formed due to the presence of trivalent or higher-valent polycarboxylic acid compounds. This can further improve the water dispersibility of the resin (Y) and the stability of its resin dispersion.

[0068] If the polyol component contains ternary or higher-order polyol compounds, the proportion of ternary or higher-order polyol compounds relative to the total polyol component is preferably equal to or less than 5% by mass. This allows the resin (Y) to have a smaller amount of cross-linked structure formed due to the presence of ternary or higher-order polyol compounds. As a result, the water dispersibility and stability of the resin dispersion can be further improved. This proportion is more preferably equal to or less than 4% by mass, even more preferably equal to or less than 3% by mass, and particularly preferably equal to or less than 1% by mass. The proportion of ternary or higher-order polyol compounds is preferably as small as possible, and can even be 0% by mass. Therefore, the polyol component used in the first step preferably does not contain ternary or higher-order polyol compounds, or contains ternary or higher-order polyol compounds in a proportion equal to or less than 5% by mass relative to the total polyol component used.

[0069] If the polyol component contains a diol compound, the diol compound preferably has a branched chain. This allows the resin dispersion of resin (Y) to further improve its stability, such as the aging stability of the solution haze.

[0070] If the polyol component contains branched diol compounds, the proportion of the branched diol compounds relative to the total polyol component is preferably equal to or greater than 5% by mass and equal to or less than 50% by mass. This allows the resin dispersion of resin (Y) to further improve its stability, such as the aging stability of solution haze. The proportion is preferably equal to or greater than 10% by mass and equal to or less than 45% by mass, more preferably equal to or greater than 15% by mass and equal to or less than 40% by mass, and even more preferably equal to or greater than 20% by mass and equal to or less than 35% by mass.

[0071] If the polyol component contains polyol compounds other than ethylene glycol, the proportion of ethylene glycol relative to the total polyol component is preferably equal to or greater than 50% by mass. This promotes the depolymerization reaction of the recycled polyester. The proportion is more preferably equal to or greater than 60% by mass, even more preferably equal to or greater than 70% by mass, and particularly preferably equal to or greater than 80% by mass. The proportion can even be 100% by mass. That is, from the perspective of promoting the depolymerization reaction of the recycled polyester, the proportion of additional polyol compounds relative to the total polyol component is preferably equal to or less than 50% by mass, more preferably equal to or less than 40% by mass, even more preferably equal to or less than 30% by mass, and particularly preferably equal to or less than 20% by mass. The proportion can even be 0% by mass.

[0072] In the first step, it is preferable to use a polyol component with a higher molar ratio than the polycarboxylic acid component. This further promotes the depolymerization reaction of the recycled polyester. Furthermore, this reduces the acid value of the resin (Y) and further improves the water dispersibility of the resin (Y) and the stability of its dispersion. Specifically, the molar ratio of the polyol component to the polycarboxylic acid component (polyol component / polycarboxylic acid component) is preferably equal to or greater than 1.5:1 and equal to or less than 5:1. More preferably, the molar ratio is equal to or greater than 1.6:1 and equal to or less than 4.7:1, even more preferably equal to or greater than 1.8:1 and equal to or less than 4.5:1, and particularly preferably equal to or greater than 2.0:1 and equal to or less than 4.2:1.

[0073] From the perspective of reducing environmental impact, the proportion of recycled polyester used is preferably as large as possible relative to the total amount of material used to produce the aqueous polyester resin. Specifically, in the first step, recycled polyester is preferably used in an amount such that the proportion of recycled polyester relative to the total amount of recycled polyester, polycarboxylic acid component, and polyol component is equal to or greater than 20% by mass and equal to or less than 70% by mass. This proportion is more preferably equal to or greater than 30% by mass, and even more preferably equal to or greater than 40% by mass. The proportion is more preferably equal to or less than 65% by mass, and even more preferably equal to or less than 62% by mass.

[0074] Furthermore, from the perspective of reducing environmental impact, the proportion of polyol component used relative to the total amount of material used in the production of water-based polyester resin is preferably as small as possible. Specifically, in the first step, it is preferable to use a polyol component such that the proportion of the polyol component relative to the total amount of recycled polyester, polycarboxylic acid component, and polyol component is equal to or greater than 10% by mass and equal to or less than 40% by mass. This proportion is more preferably equal to or less than 35% by mass, and even more preferably equal to or less than 30% by mass. The proportion is more preferably equal to or greater than 13% by mass, and even more preferably equal to or greater than 15% by mass.

[0075] In the first step, recycled polyester is preferably used in an amount such that the proportion of recycled polyester relative to the total amount of recycled polyester and polycarboxylic acid residues is equal to or greater than 25% by mass and equal to or less than 85% by mass. The proportion is more preferably equal to or greater than 40% by mass, and even more preferably equal to or greater than 55% by mass. The proportion is more preferably equal to or less than 80% by mass, and even more preferably equal to or less than 78% by mass.

[0076] Furthermore, in the first step, a polycarboxylic acid compound (A) containing a metal sulfonate group is preferably used in an amount such that the proportion of the polycarboxylic acid residues containing a metal sulfonate group in the polycarboxylic acid compound (A) relative to the total amount of the recycled polyester and the polycarboxylic acid residues is equal to or greater than 4% by mass and equal to or less than 30% by mass. This proportion is more preferably equal to or greater than 5% by mass, and even more preferably equal to or greater than 6% by mass. This proportion is more preferably equal to or less than 28% by mass, and even more preferably equal to or less than 26% by mass.

[0077] In the first step, it is preferable to use an additional polycarboxylic acid compound (B) in such a proportion that the additional polycarboxylic acid residues contained in the additional polycarboxylic acid compound (B) relative to the total amount of the recycled polyester and the polycarboxylic acid residues are equal to or greater than 1% by mass and equal to or less than 50% by mass. The proportion is more preferably equal to or greater than 4% by mass, and even more preferably equal to or greater than 10% by mass. The proportion is more preferably equal to or less than 40% by mass, and even more preferably equal to or less than 35% by mass.

[0078] In the first step, in addition to the recycled polyester, the polycarboxylic acid component and the polyol component, at least one selected from terephthalic acid and its esters and acid anhydrides, and at least one selected from hydroxycarboxylic acid and its esters and acid anhydrides may be used, provided that the advantages of the present disclosure are not impaired, but preferably not used.

[0079] The reaction in the first step can be accelerated, for example, by heating the mixed reaction materials.

[0080] In the first step, from the perspective of promoting the reaction, a catalyst is preferred. Examples of catalysts include titanium oxalates, such as potassium titanium oxalate and sodium titanium oxalate; titanium alkoxides, such as tetrapropyl titanate and tetrabutyl titanate; fatty acid titanium salts, such as titanium acetate; titanium catalysts, such as inorganic titanium compounds, such as titanium oxides; fatty acid manganese salts, such as manganese acetate; manganese catalysts, such as manganese carbonate; antimony catalysts, such as antimony trioxide; aluminum catalysts, such as aluminum triacetate; germanium catalysts, such as germanium dioxide; and lithium catalysts, such as sec-butyllithium.

[0081] The amount of catalyst used relative to all components blended in the first step may, for example, be equal to or greater than 0.0001% by mass and equal to or less than 0.1% by mass, and preferably equal to or greater than 0.003% by mass and equal to or less than 0.05% by mass.

[0082] To initiate the reaction in the first step, a reaction solvent may or may not be used, but it is preferred not to use one.

[0083] From the perspective of improving the quality of resin (Y), it is preferable to initiate the reaction in the first step in an inert gas atmosphere, such as a nitrogen atmosphere or an argon atmosphere.

[0084] [Second Step]

[0085] The second step involves inducing a polycondensation reaction by reducing the pressure. In this second step, the polycondensation reaction is promoted by reducing the pressure in the reaction system, thereby removing the polyol and other products generated by the reaction.

[0086] As used herein, a polycondensation reaction refers to a reaction in which the ester compound and polyester formed in the first step undergo, for example, a dealcoholization condensation reaction to form a polyester with a higher molecular weight.

[0087] The reaction in the second step can be accelerated by reducing the pressure in the reaction system and by, for example, heating the reaction products generated in the first step.

[0088] After the reaction is initiated in the first step, the second step can be carried out while keeping the pressure in the reaction system low but adjusting the temperature. Alternatively, the second step can be carried out, for example, by separating the reaction products generated in the first step, adding a catalyst, solvent, or any other additive as needed, then reducing the pressure in the reaction system and heating the reaction products.

[0089] Aqueous polyester resin (resin (Y)) was produced by performing the production method (X) described above.

[0090] (Acid value)

[0091] Importantly, the resulting resin (Y) has an acid value equal to or less than 10 mg KOH / g. Setting the acid value of resin (Y) to be equal to or less than 10 mg KOH / g significantly improves its water dispersibility and the stability of the resin dispersion. If the acid value of resin (Y) is greater than 10 mg KOH / g, both the water dispersibility and the stability of the resin dispersion decrease. The acid value is preferably equal to or less than 9 mg KOH / g, more preferably equal to or less than 8 mg KOH / g, even more preferably equal to or less than 7 mg KOH / g, and particularly preferably equal to or less than 6 mg KOH / g. The lower the acid value of resin (Y), the better. The acid value of resin (Y) can even be 0 mg KOH / g. As used herein, the “acid value” of resin (Y) refers to the mass (mg) of potassium hydroxide required to neutralize 1 g of resin (Y). The acid value of resin (Y) is determined by, for example, the presence of carboxyl groups on the side chains or ends of the resin (Y) molecule.

[0092] (Glass transition temperature)

[0093] The glass transition temperature (Tg) of the resin (Y) thus obtained is preferably equal to or higher than 0°C and equal to or lower than 100°C. Setting the Tg at a temperature equal to or higher than 0°C reduces the chance of the resin (Y) becoming too viscous, thereby making the resin (Y) even easier to handle and further reducing the chance of causing excessive tackiness. Setting the Tg at a temperature equal to or lower than 100°C allows the resin (Y) to have better film-forming ability and can further increase the adhesion of the resin (Y) to the substrate and improve its primer properties. More preferably, the Tg is equal to or higher than 10°C, and even more preferably equal to or higher than 20°C. More preferably, the Tg is equal to or lower than 80°C, and even more preferably equal to or lower than 75°C.

[0094] The weight-average molecular weight of the resin (Y) obtained therefrom is preferably equal to or greater than 3,000 and equal to or less than 100,000, more preferably equal to or greater than 5,000 and equal to or less than 80,000, and even more preferably equal to or greater than 6,000 and equal to or less than 60,000.

[0095] Exemplary embodiments of the production method (X) according to this embodiment include production method (X1) and production method (X2) which will be described below.

[0096] [Production Method (X1)]

[0097] According to production method (X1), resin (Y) is produced by performing the following steps: after mixing recycled polyester, polycarboxylic acid component, and polyol component as reactants, an esterification reaction and a depolymerization reaction are induced in the mixed reactants (hereinafter referred to as "step X1-1"), and a condensation reaction is induced by reducing the pressure in the reaction system (hereinafter referred to as "step X1-2"). Production method (X1) enables the production of aqueous polyester resins by a simpler method.

[0098] (Step X1-1)

[0099] Step X1-1 involves mixing the recycled polyester, the polycarboxylic acid component, and the polyol component, and then inducing an ester formation reaction and a depolymerization reaction.

[0100] The reaction temperature in step X1-1 is preferably equal to or higher than 150°C and equal to or lower than 270°C, and more preferably equal to or higher than 180°C and equal to or lower than 260°C. The reaction time is preferably equal to or longer than 1 hour and equal to or shorter than 10 hours, and more preferably equal to or longer than 2 hours and equal to or shorter than 8 hours. From the viewpoint of further promoting the ester formation and depolymerization reactions in step X1-1, the reaction system is preferably under atmospheric pressure. The reaction temperature in step X1-1 can be gradually changed.

[0101] (Steps X1-2)

[0102] Step X1-2 involves inducing a polycondensation reaction by reducing the pressure. Step X1-2 is the same as the second step described above.

[0103] The reaction temperature in steps X1-2 is preferably equal to or higher than 150°C and equal to or lower than 270°C, and more preferably equal to or higher than 200°C and equal to or lower than 260°C. The degree of pressure reduction (absolute pressure) in step X1-2 is preferably equal to or lower than 25 hPa, and more preferably equal to or lower than 10 hPa. The reaction temperature and the degree of pressure reduction in step X1-2 can be gradually changed. Adjusting the reaction temperature, reaction time, and degree of pressure reduction in step X1-2 allows for adjustment of the weight-average molecular weight of the resin (Y) or any other parameter.

[0104] [Production Method (X2)]

[0105] The production method (X2) may include the following steps: a step of inducing an ester formation reaction of the mixed reactants after blending the polycarboxylic acid component and the polyol component as reactants (hereinafter also referred to as "step X2-1"); a step of blending the recycled polyester with the reaction product generated in step X2-1 and then inducing a depolymerization reaction (hereinafter also referred to as "step X2-2"); and a step of inducing a polycondensation reaction by reducing the pressure (hereinafter also referred to as "step X2-3"). Performing the blending and reaction processes in these steps X2-1 to X2-3 respectively can, for example, more appropriately induce the depolymerization reaction of the recycled polyester and further improve the water dispersibility of the aqueous polyester resin and the stability of its resin dispersion.

[0106] (Step X2-1)

[0107] Step X2-1 includes inducing an ester formation reaction after mixing the polycarboxylic acid component and the polyol component.

[0108] The reaction temperature in step X2-1 is preferably equal to or higher than 150°C and equal to or lower than 250°C, and more preferably equal to or higher than 180°C and equal to or lower than 240°C. The reaction time is preferably equal to or longer than 1 hour and equal to or shorter than 8 hours, and more preferably equal to or longer than 2 hours and equal to or shorter than 5 hours. From the perspective of further promoting the ester formation reaction in step X2-1, the reaction system is preferably under atmospheric pressure. The reaction temperature in step X2-1 can be gradually changed.

[0109] (Step X2-2)

[0110] Step X2-2 involves further adding recycled polyester to the reaction product, which then causes the compound to depolymerize.

[0111] The reaction temperature in step X2-2 is preferably equal to or higher than 200°C and equal to or lower than 270°C, and more preferably equal to or higher than 210°C and equal to or lower than 260°C. The reaction time is preferably equal to or longer than 1 hour and equal to or shorter than 8 hours, and more preferably equal to or longer than 2 hours and equal to or shorter than 5 hours. From the perspective of further promoting the depolymerization reaction in step X2-2, the reaction system is preferably under atmospheric pressure. The reaction temperature in step X2-2 can be gradually changed.

[0112] (Steps X2-3)

[0113] Step X2-3 involves inducing a polycondensation reaction by reducing the pressure. Step X2-3 is the same as step two described above.

[0114] The reaction temperature in steps X2-3 is preferably equal to or higher than 150°C and equal to or lower than 270°C, and more preferably equal to or higher than 200°C and equal to or lower than 260°C. The degree of pressure reduction (absolute pressure) in step X2-3 is preferably equal to or lower than 25 hPa, and more preferably equal to or lower than 10 hPa. The reaction temperature and the degree of pressure reduction in step X2-3 can be gradually changed. Adjusting the reaction temperature, reaction time, and degree of pressure reduction in step X2-3 can regulate the weight-average molecular weight of the resin (Y) or any other parameter.

[0115] <Water-based polyester resin>

[0116] The resin (Y) according to this embodiment is produced by the above-described production method (X).

[0117] Another resin (Y) according to this embodiment comprises terephthalic acid residues derived from recycled polyester (hereinafter also referred to as "residue (I)") and polycarboxylic acid residues other than terephthalic acid residues (hereinafter also referred to as "residue (II)"). Residue (II) comprises polycarboxylic acid residues containing metal sulfonate groups (hereinafter also referred to as "residue (IIa)") and other polycarboxylic acid residues other than residues (I) and (IIa) (hereinafter also referred to as "residue (IIb)"). Residue (I) accounts for 20% or more by mass and 72% or less by mass relative to all polycarboxylic acid residues contained in resin (Y), and residue (IIa) accounts for 5% or more by mass and 32% or less by mass. Resin (Y) has an acid value of 10 mg KOH / g or less.

[0118] Resin (Y) not only exhibits excellent water dispersibility, for example, even without any surfactant, but also demonstrates good stability when used as a resin dispersion, while reducing environmental impact. Resin (Y) uses recycled polyester as its material, with the proportion of recycled polyester equal to or greater than a certain value, thus reducing the amount of materials derived from fossil fuels and reducing waste, thereby reducing environmental impact. Furthermore, resin (Y) contains terephthalic acid residues derived from recycled polyester, polycarboxylic acid residues containing metal sulfonate groups, and other polycarboxylic acid residues. By setting the ratio of terephthalic acid residues and polycarboxylic acid residues containing metal sulfonate groups within a specific range, and setting the acid value at a specific value or less, the crystallinity of resin (Y) can be reduced to a sufficient degree while achieving an appropriate balance between the hydrophobic and hydrophilic portions of resin (Y). This and other measures taken according to this embodiment will allow resin (Y) to have excellent water dispersibility, for example, even without any surfactant, and improve the stability of its resin dispersion. Furthermore, resin (Y) contains terephthalic acid residues derived from recycled polyester and still possesses the same excellent resin properties (e.g., adhesion and transparency) as when using unused terephthalic acid or terephthalic acid derivatives not derived from recycled polyester. Moreover, the resin dispersion of resin (Y) not only exhibits good long-term water dispersibility but also improves its stability, such as the aging stability of solution haze. The exact reasons for these advantages are not fully understood. However, these advantages may be achieved for reasons such as the following: As mentioned above, by setting the appropriate residue ratio and acid value within a specific range, the crystallinity of resin (Y) can be reduced to a sufficient degree while achieving a proper balance between the hydrophobic and hydrophilic portions of resin (Y). For the same reasons as the excellent water dispersibility of resin (Y) and the good stability of its resin dispersion, resin properties such as adhesion and transparency, long-term water dispersibility, and stability such as the stability of solution haze will be significantly improved regardless of whether the terephthalic acid residues are derived from recycled polyester or formed from unused terephthalic acid or terephthalic acid derivatives.

[0119] The resin (Y) contains polycarboxylic acid residues and polyol residues.

[0120] (polycarboxylic acid residues)

[0121] Resin (Y) contains residues (I) and (II) as polycarboxylic acid residues.

[0122] (Residue (I))

[0123] Residue (I) is a terephthalic acid residue derived from recycled polyester. As used herein, “terephthalic acid residue derived from recycled polyester” means that the terephthalic acid residue contained in the recycled polyester is converted into the terephthalic acid residue contained in the resin (Y). As used herein, “terephthalic acid residue” refers to a residue represented by the following formula (3):

[0124]

[0125] In formula (3), * represents a group adjacent to the residue represented by formula (3) or a site bonded to an adjacent residue.

[0126] Importantly, the proportion of residue (I) relative to all polycarboxylic acid residues in resin (Y) is equal to or greater than 20% by mass and equal to or less than 72% by mass. If the proportion is less than 20% by mass, the environmental impact will not be sufficiently reduced. If the proportion is greater than 72% by mass, the crystallinity of resin (Y) will not decrease, thus resulting in decreased water dispersibility and stability of the resin dispersion. The proportion is preferably equal to or greater than 30% by mass, more preferably equal to or greater than 40% by mass, even more preferably equal to or greater than 45% by mass, and particularly preferably equal to or greater than 50% by mass. The proportion is preferably equal to or less than 71% by mass, more preferably equal to or less than 70% by mass, even more preferably equal to or less than 69% by mass, and particularly preferably equal to or less than 68% by mass. As used herein, “all polycarboxylic acid residues” in resin (Y) means, for example, the sum of residues (I) and residues (II).

[0127] (Residue (II))

[0128] Residue (II) includes residue (IIa) and residue (IIb).

[0129] Residue (IIa)

[0130] Residue (IIa) is a polycarboxylic acid residue containing a metal sulfonate group.

[0131] Importantly, the proportion of residue (IIa) relative to all polycarboxylic acid residues in resin (Y) is equal to or greater than 5% by mass and equal to or less than 32% by mass. If the proportion is less than 5% by mass, the proportion of the hydrophilic portion will be too small to avoid a decrease in water dispersibility. If the proportion is greater than 32% by mass, the proportion of the hydrophilic portion will be too large to avoid adhesion due to water absorption in the resin film of resin (Y). The proportion is preferably equal to or greater than 6% by mass, more preferably equal to or greater than 7% by mass, even more preferably equal to or greater than 8% by mass, and particularly preferably equal to or greater than 9% by mass. The proportion is preferably equal to or less than 31% by mass, more preferably equal to or less than 29% by mass, even more preferably equal to or less than 27% by mass, and particularly preferably equal to or less than 25% by mass.

[0132] (Residue (IIb))

[0133] Residue (IIb) is a polycarboxylic acid residue other than residue (I) and residue (IIa).

[0134] The proportion of residue (IIb) relative to all polycarboxylic acid residues in resin (Y) is preferably equal to or greater than 3% by mass and equal to or less than 55% by mass. This proportion is more preferably equal to or greater than 5% by mass, even more preferably equal to or greater than 10% by mass, particularly preferably equal to or greater than 13% by mass, and most preferably equal to or greater than 15% by mass. This proportion is more preferably equal to or less than 50% by mass, even more preferably equal to or less than 40% by mass, particularly preferably equal to or less than 30% by mass, and most preferably equal to or less than 25% by mass.

[0135] In addition to residues (I), (IIa), and (IIb), resin (Y) may also contain terephthalic acid residues not derived from recycled polyester as additional polycarboxylic acid residues. However, from the perspective of reducing environmental impact, it is preferable that resin (Y) does not contain terephthalic acid residues not derived from recycled polyester. Furthermore, although resin (Y) may contain hydroxycarboxylic acid residues, it is preferable that resin (Y) does not contain hydroxycarboxylic acid residues.

[0136] The polycarboxylic acid residues preferably do not contain residues of trivalent or higher-valent polycarboxylic acid compounds. In other words, it is preferred that residues (IIa) and (IIb) do not contain residues contained in trivalent or higher-valent polycarboxylic acid compounds, and only contain residues of divalent polycarboxylic acid compounds. This allows for a further reduction in the acid value of the resin (Y) and also allows the resin (Y) to have a smaller number of cross-linked structures formed due to the presence of trivalent or higher-valent polycarboxylic acid compounds. Therefore, the water dispersibility and stability of the resin dispersion can be further improved.

[0137] (polyol residues)

[0138] Polyol residues are residues containing a plurality of hydroxyl groups in a polyol compound. Resin (Y) typically has ethylene glycol residues derived from recycled polyester as polyol residues.

[0139] If the polyol residues do not contain residues of ternary or higher-order polyol compounds, or if they do contain residues of ternary or higher-order polyol compounds, the proportion of residues of ternary or higher-order polyol compounds relative to all polyol residues contained in the resin (Y) is preferably equal to or less than 5% by mass. That is, even if the polyol residues do not contain residues contained in ternary or higher-order polyol compounds, but only contain residues of binary polyol compounds, or if the polyol residues contain residues contained in ternary or higher-order polyol compounds, the proportion of residues contained in ternary or higher-order polyol compounds relative to all polyol residues is preferably equal to or less than 5% by mass. This allows the resin (Y) to have an appropriate number of crosslinked structures, thus further improving the water dispersibility of the resin (Y) and the stability and film-forming ability of its resin dispersion. The proportion of residues of ternary or higher-order polyol compounds relative to all polyol residues contained in the resin (Y) is more preferably equal to or less than 4% by mass, and even more preferably equal to or less than 3% by mass.

[0140] If the polyol residues include residues of a diol compound, then the residues of the diol compound preferably have branches. This allows the resin dispersion of resin (Y) to further improve its stability, such as the aging stability of the solution haze.

[0141] Examples of branched diol compounds include compounds represented by the following formula (4):

[0142]

[0143] In equation (4), R 3 It is a branched divalent hydrocarbon group with 3 to 50 carbon atoms.

[0144] By R 3 Examples of branched divalent hydrocarbon groups include propane-1,2-diyl, butane-1,2-diyl, butane-1,3-diyl, 2-methylpropane-1,3-diyl, pentane-1,2-diyl, pentane-1,3-diyl, pentane-1,4-diyl, 2,2-dimethylpropane-1,3-diyl, 2-methylbutane-1,4-diyl, hexane-1,2-diyl, hexane-2,5-diyl, and 2,4-diethylpentane-1,5-diyl.

[0145] Examples of branched diol compounds include neopentyl glycol, 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 1,2-pentanediol, 1,2-hexanediol, 2,5-hexanediol, and 2,4-diethyl-1,5-pentanediol. Neopentyl glycol, 1,2-propanediol, and 1,3-butanediol are particularly preferred.

[0146] The proportion of branched diol compound residues relative to all polyol residues contained in resin (Y) is preferably equal to or greater than 5% by mass and equal to or less than 50% by mass. This allows the resin dispersion of resin (Y) to further improve its stability, such as the aging stability of solution haze. The proportion is preferably equal to or greater than 10% by mass and equal to or less than 45% by mass, more preferably equal to or greater than 15% by mass and equal to or less than 40% by mass, and even more preferably equal to or greater than 20% by mass and equal to or less than 35% by mass.

[0147] <Water-based Coating Composition>

[0148] The aqueous coating composition according to this embodiment (hereinafter also referred to as "composition (Z)") comprises the above-described resin (Y).

[0149] The composition (Z) may contain, for example, water or water containing a hydrophilic organic solvent. In this case, the suitability of the composition (Z) can be further improved, for example, by appropriately adjusting the viscosity of the composition (Z). If the composition (Z) contains water or water containing a hydrophilic organic solvent, then the composition (Z) is a resin dispersion of resin (Y). This resin dispersion of resin (Y) has excellent stability and can keep the resin dispersed for a long time.

[0150] Examples of hydrophilic organic solvents include: alcohols, such as methanol, ethanol, 2-propanol, and 1,2-propanediol; glycol ethers, such as propylene glycol monomethyl ether, ethyl cellosolve, and n-butyl cellosolve; and ketones, such as acetone and methyl ethyl ketone.

[0151] The composition (Z) can be easily applied by, for example, bar coating, dip coating, spray coating or spin coating.

[0152] The resin film made from composition (Z) (hereinafter also referred to as "resin film (W)") exhibits excellent adhesion to resins with polar structures (e.g., PET films) and to metals (e.g., aluminum vapor deposits). Furthermore, the resin film (W) maintains low haze and excellent transparency. In addition, the resin film (W) also possesses, for example, excellent primer properties.

[0153] The composition (Z) may contain suitable additives, such as other aqueous resins besides resin (Y), homogenizers, antioxidants, UV absorbers, defoamers, crosslinking agents and inorganic particles.

[0154] Example

[0155] Next, specific embodiments of this disclosure will be described. Note that the embodiments described below are merely examples of this disclosure and should not be construed as limiting.

[0156] <Production of water-based polyester resin>

[0157] Aqueous polyester resins are produced using the materials shown in Tables 1 and 2 (to be published later) according to the following procedures. Details of the recycled polyester used in the production are as follows:

[0158] • Recycled Polyester A: A material made from recycled used PET bottles, with an intrinsic viscosity (IV value) of 0.88 dl / g;

[0159] • Recycled Polyester B: A material made from recycled used PET bottles, with an intrinsic viscosity (IV value) of 0.67 dl / g;

[0160] • Recycled Polyester C: A material made from recycled polyester fiber (PET fiber) waste, with an intrinsic viscosity (IV value) of 0.59 dl / g; and

[0161] • Recycled Polyester D: A material made from recycled PET film waste, with an intrinsic viscosity (IV value) of 0.50 dl / g.

[0162] Note that the intrinsic viscosity (IV value) of recycled polyester is determined based on measurements using a Ubbelohde viscometer.

[0163] As used in this article, “intrinsic viscosity” refers to the intrinsic viscosity measured according to the JIS K 7390-1:2015 standard.

[0164] (1) Production by production method (X1) (Examples 1 to 8 and 15 to 17 and Comparative Examples 1 to 3)

[0165] (First step)

[0166] (Step X1-1)

[0167] A reaction vessel with a capacity of 1000 mL is provided, including a stirrer, nitrogen inlet, thermometer, distillation column, and cooling condenser. The recycled polyester, polycarboxylic acid component, polyol component, and potassium titanium oxalate (as catalyst) shown in Tables 1 and 2 are introduced into this reaction vessel to prepare a mixture. The mixture is heated to 200°C under atmospheric pressure and a nitrogen atmosphere while being stirred and mixed, and then gradually heated to 250°C for 6 hours, thereby inducing ester formation and depolymerization reactions.

[0168] (Second Step)

[0169] (Steps X1-2)

[0170] After step X1-1, the pressure is gradually reduced to 0.67 hPa (0.5 mmHg) at 250°C and maintained at this temperature for 2 hours, thereby inducing a polycondensation reaction. Aqueous polyester resins are produced in this manner.

[0171] (2) Production by production method (X2) (Examples 9 to 14 and 18 to 20 and Comparative Example 4)

[0172] (First step)

[0173] (Step X2-1)

[0174] A reaction vessel with a capacity of 1000 mL is provided, including a stirrer, nitrogen inlet, thermometer, distillation column, and cooling condenser. The polycarboxylic acid components, polyol components, and potassium titanium oxalate (as a catalyst) shown in Tables 1 and 2 are introduced into this reaction vessel to prepare a mixture. The mixture is heated to 200 °C under atmospheric pressure and a nitrogen atmosphere while being stirred and mixed, and then gradually heated to 240 °C for 3 hours, thereby initiating an ester formation reaction.

[0175] (Step X2-2)

[0176] After step X2-1, the recycled polyesters shown in Tables 1 and 2 are introduced into the reaction vessel under a nitrogen atmosphere at normal pressure, and heated to 250°C while stirring and mixing, and maintained at this state for 3 hours, thereby inducing a depolymerization reaction.

[0177] (Second Step)

[0178] (Steps X2-3)

[0179] After step X2-2, the pressure is gradually reduced to 0.67 hPa (0.5 mmHg) at 250°C and maintained at this temperature for 2 hours, thereby inducing a polycondensation reaction. Aqueous polyester resin is produced in this manner.

[0180] (3) Reference Examples (Reference Examples 1 to 4)

[0181] Aqueous polyester resins, representing Examples 5, 9, and 13 and Comparative Example 1, were produced using unused terephthalic acid or dimethyl terephthalate as unused terephthalic acid derivatives without the use of recycled polyester. Aqueous polyester resins were produced in this manner as Reference Examples 1 to 4.

[0182] <Preparation of Aqueous Coating Compositions>

[0183] (1) Examples 9, 11 to 13 and 18 to 20 and Comparative Example 2

[0184] A water-based coating composition with a resin concentration of 25% by mass was prepared by mixing 100 parts by mass of the water-based polyester resin produced as described above with 300 parts by mass of water and maintaining the mixture at a temperature of 90°C for 2 hours while stirring.

[0185] (2) Examples 1 to 8, 10 and 14 to 17 and Comparative Examples 1, 3 and 4

[0186] The aqueous polyester resin prepared in this way has too low a water solubility, making it impossible to disperse the polyester resin under the conditions described in item (1). Therefore, n-butyl cellosolve is used as a hydrophilic organic solvent to disperse the aqueous polyester resin. Specifically, an aqueous coating composition with a resin concentration of 25% by mass is prepared by mixing 100 parts by mass of the aqueous polyester resin prepared as described above, 40 parts by mass of n-butyl cellosolve, and 260 parts by mass of water, and maintaining the mixture at a temperature of 90°C for 2 hours while stirring the mixture.

[0187] (3) Reference Examples (Reference Examples 1 to 4)

[0188] Aqueous coating compositions with a resin concentration of 25% by mass were prepared by applying the method described in item (2) to aqueous polyester resins obtained as reference examples 1 and 4, and by applying the method described in item (1) to aqueous polyester resins obtained as reference examples 2 and 3.

[0189] <Assessment>

[0190] [Physical properties of resin]

[0191] The physical properties of each aqueous polyester resin produced as described above were evaluated using the following methods.

[0192] (Acid value (mgKOH / g))

[0193] The acid value of the aqueous polyester resin was determined based on the measurement results obtained by titration using an ethanol solution of potassium hydroxide.

[0194] (weight-average molecular weight)

[0195] The weight-average molecular weight (and equivalent molecular weight of polystyrene) of the aqueous polyester resin was determined based on the results of gel permeation chromatography.

[0196] (Glass transition temperature (°C))

[0197] The glass transition temperature of the aqueous polyester resin was determined based on the measurement results obtained by differential scanning calorimetry.

[0198] [Measurement of physical properties]

[0199] The physical properties of each aqueous coating composition (resin dispersion) prepared as described above were measured using the following methods:

[0200] (Water dispersibility)

[0201] The resin dispersion was observed and graded based on its appearance as follows:

[0202] Grade A: No precipitate was detected in the resin dispersion;

[0203] Grade B: If very small amounts of precipitate are identified in the resin dispersion;

[0204] Grade C: If a large amount of precipitate is identified in the resin dispersion; or

[0205] Grade D: If the resin does not disperse in the solvent.

[0206] (Stability of resin dispersion)

[0207] The resin dispersion was placed in a glass bottle and sealed airtight, then allowed to stand at 20°C for 15 days. Afterwards, the dispersion was observed and graded based on its appearance as follows:

[0208] Grade A: If no separation or precipitate is identified in the dispersion;

[0209] Grade B: If a small amount of separated and / or precipitated material is identified in the dispersion; or

[0210] Grade C: If a large amount of separation and / or precipitate is identified in the dispersion.

[0211] (Aging stability of solution haze)

[0212] The resin dispersion was placed in a glass bottle and sealed airtight, then allowed to stand for 15 days at 5°C, 20°C, and 40°C. Afterward, the haze (%) of the dispersion was measured using a haze meter manufactured by Nippon Denshoku Industries Co., Ltd. Based on the measurement results, the dispersion was classified as follows:

[0213] Grade A: If the haze of the dispersion changes by less than 20% compared to the haze of the dispersion before it has been allowed to stand;

[0214] Grade B: If the haze of the dispersion changes by 20% or more and less than 40% compared to the haze of the dispersion before it has been allowed to stand.

[0215] Grade C: If the haze of the dispersion changes by 40% or more and less than 60% compared to the haze of the dispersion before it has been allowed to stand; or

[0216] Grade D: If the haze of the dispersion changes by 60% or more compared to the haze of the dispersion before it has been allowed to stand, or if the haze of the dispersion changes by 90% or more.

[0217] (Adhesion of PET film)

[0218] An untreated biaxially oriented polyethylene terephthalate (PET) film was provided as the substrate. A resin dispersion was applied to the substrate using a doctor blade coater, followed by heating at 120°C for 5 minutes. In this manner, a primer layer with a thickness of approximately 1 μm was formed on the substrate. Subsequently, cellophane tape was applied to the primer layer on the substrate in close contact, then peeled off, and the remaining primer layer was observed. The primer layer was graded by its appearance as follows:

[0219] Grade A: If no primer peeling is detected;

[0220] Grade B: If partial peeling of the primer layer is identified; or

[0221] Grade C: If most of the primer layer is identified as peeling.

[0222] (Adhesion of aluminum vapor-deposited coating)

[0223] An untreated biaxially oriented polyethylene terephthalate (PET) film was used as a substrate, and a primer layer with a thickness of approximately 1 μm was formed on the substrate using the same method described in the "Adhesion of PET Film" section. Subsequently, an aluminum vapor-deposited layer with a thickness of approximately 1 μm was formed on the primer layer on the substrate using a vacuum deposition process. Cellophane tape was brought into close contact with the aluminum vapor-deposited layer, then peeled off, and the remaining aluminum vapor-deposited layer was observed. The aluminum vapor-deposited layer was graded by its appearance as follows:

[0224] Grade A: If no aluminum vapor deposition peeling is detected;

[0225] Grade B: If partial peeling of the aluminum vapor-deposited layer is identified; or

[0226] Grade C: If most of the aluminum vapor deposition layer is identified as peeling.

[0227] (Haze)

[0228] An untreated biaxially oriented polyethylene terephthalate (PET) film was provided as the substrate. A resin dispersion was applied to the substrate using a doctor blade coater, followed by heating at 120°C for 5 minutes. In this manner, a primer layer with a thickness of approximately 3 μm was formed on the substrate. Subsequently, the haze of the substrate alone and the haze of the substrate combined with the primer layer were measured using a haze meter manufactured by Nippon Denshoku Industries Co., Ltd. The haze (%) of the primer layer was calculated by subtracting the haze of the substrate alone from the haze of the substrate and the primer layer combination.

[0229] Tables 1 and 2 below summarize the evaluation results of the physical property tests regarding water dispersibility, resin dispersion stability, PET film adhesion, aluminum vapor deposition adhesion, and haze. Note that the "—" in the evaluation results of Comparative Example 3 indicates that the sample was graded D in terms of water dispersibility (i.e., the resin is not dispersed in the solvent), and therefore no other evaluation tests were performed.

[0230]

[0231]

[0232] As can be seen from the results shown in Tables 1 and 2, the aqueous polyester resins of each of Examples 1 to 20 not only exhibit excellent water dispersibility, for example, even without any surfactant, but also have good stability when used as resin dispersions, while reducing environmental impact. Furthermore, as can be seen from the comparison with the representative aqueous polyester resins of Reference Examples 1 to 4, which were produced using unused terephthalic acid or dimethyl terephthalate as terephthalic acid derivatives, the aqueous polyester resins of each of Examples 1 to 20 contain terephthalic acid residues derived from recycled polyester and still exhibit the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyester. Moreover, their resin dispersions not only exhibit good long-term water dispersibility but also further improve their stability, such as the aging stability of solution haze. In addition, by using branched diol compounds in specific proportions, the aqueous polyester resins according to Examples 3 and 15 to 20 achieved excellent aging stability (at 5°C, 20°C and 40°C) in terms of solution haze of the resin dispersion (i.e., Grade A).

[0233] On the other hand, the aqueous polyester resin produced by the production method according to Comparative Example 3 cannot be dispersed in water or water containing hydrophilic organic solvents without the use of, for example, surfactants. The aqueous polyester resin produced by the production methods according to any one of Comparative Examples 1, 2 and 4 has poor stability in terms of resin dispersion.

[0234] Note that for each of the representative examples 2 to 6 and examples 9 to 20 of the aqueous polyester resins that are graded A in "Stability of Resin Dispersions", no separation or precipitation was identified in the appearance of the resin dispersion even after the resin dispersion was placed in a glass bottle and sealed airtightly and allowed to stand at 20°C for 30 days.

[0235] (Key points restated)

[0236] As can be seen from the foregoing description, the method for producing a water-based polyester resin according to the first aspect of this disclosure is a method for producing a water-based polyester resin using recycled polyester. The method includes a first step and a second step. The first step includes initiating an esterification reaction and a depolymerization reaction using recycled polyester, a polycarboxylic acid component containing polycarboxylic acid residues but not terephthalic acid, and a polyol component. The second step includes initiating a polycondensation reaction by reducing pressure. The polycarboxylic acid component includes: at least one polycarboxylic acid compound containing a metal sulfonate group selected from polycarboxylic acids, their esters, and acid anhydrides, each having a metal sulfonate group and containing a polycarboxylic acid residue containing a metal sulfonate group; and at least one additional polycarboxylic acid compound selected from polycarboxylic acids other than terephthalic acid and polycarboxylic acid compounds containing metal sulfonate groups, their esters, and acid anhydrides. The first step includes: using recycled polyester in an amount such that the proportion of terephthalic acid residues relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 20% by mass and equal to or less than 72% by mass; and using a polycarboxylic acid compound containing metal sulfonate groups in an amount such that the proportion of polycarboxylic acid residues containing metal sulfonate groups relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 5% by mass and equal to or less than 32% by mass. The resulting aqueous polyester resin has an acid value equal to or less than 10 mg KOH / g.

[0237] Firstly, it is possible to produce aqueous polyester resins with the following advantageous characteristics. Specifically, aqueous polyester resins not only exhibit excellent water dispersibility, for example, even without any surfactant, but also demonstrate good stability when used as resin dispersions, while reducing environmental impact. Furthermore, aqueous polyester resins contain terephthalic acid residues derived from recycled polyesters and still possess the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyesters. Moreover, resin dispersions of aqueous polyester resins not only exhibit good long-term water dispersibility but also further improve their stability, such as the aging stability of solution haze.

[0238] In the method for producing a waterborne polyester resin according to the second aspect (which may be implemented in combination with the first aspect), the first step includes inducing an ester formation reaction and a depolymerization reaction after mixing recycled polyester, a polycarboxylic acid component and a polyol component with each other.

[0239] Secondly, it is possible to produce water-based polyester resins using a relatively simple method.

[0240] In the method for producing a water-based polyester resin according to the third aspect (which may be implemented in combination with the first aspect), the first step includes: inducing an ester formation reaction after mixing a polycarboxylic acid component and a polyol component; and inducing a depolymerization reaction after adding recycled polyester thereto.

[0241] Thirdly, by performing the compounding and reaction in these three steps respectively, it is possible to more appropriately induce depolymerization reactions, such as those of recycled polyester, thereby further improving the water dispersibility of aqueous polyester resins and the stability of resin dispersions.

[0242] In the method for producing a water-based polyester resin according to the fourth aspect (which may be implemented in combination with any of the first to third aspects), the first step further includes using an additional polycarboxylic acid compound in such an amount that the additional polycarboxylic acid residues are equal to or greater than 5% by mass and equal to or less than 50% by mass relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component.

[0243] Fourthly, it can more effectively reduce the crystallinity of water-based polyester resins, thereby further improving water dispersibility and the stability of resin dispersions.

[0244] In the method for producing waterborne polyester resin according to the fifth aspect (which may be implemented in combination with any of the first to fourth aspects), the polycarboxylic acid component used in the first step does not contain trivalent or higher valence polycarboxylic acid compounds.

[0245] The fifth aspect allows for a further reduction in the acid value of aqueous polyester resins and also allows for the presence of even fewer cross-linked structures due to the presence of trivalent or higher-valence polycarboxylic acid compounds. Therefore, the water dispersibility of aqueous polyester resins and the stability of their resin dispersions can be further improved.

[0246] In the method for producing a water-based polyester resin according to the sixth aspect (which may be implemented in combination with any of the first to fifth aspects), the polyol component used in the first step either does not contain a ternary or higher-order polyol compound, or contains a ternary or higher-order polyol compound. The proportion of the ternary or higher-order polyol compound is equal to or less than 5% by mass relative to the total polyol component used.

[0247] The sixth aspect allows aqueous polyester resins to have even fewer cross-linked structures formed due to the presence of ternary or higher-order polyol compounds. Therefore, water dispersibility and the stability of the resin dispersion can be further improved.

[0248] In the method for producing a water-based polyester resin according to the seventh aspect (which may be implemented in combination with any of the first to sixth aspects), the polyol component used in the first step comprises a diol compound. The diol compound has a branched chain. The proportion of the branched diol compound is equal to or greater than 5% by mass and equal to or less than 50% by mass relative to the total polyol component used.

[0249] The seventh aspect allows for further improvement in the stability of aqueous polyester resin dispersions, such as the aging stability of solution haze.

[0250] The waterborne polyester resin according to the eighth aspect is produced by the method for producing waterborne polyester resin according to any one of the first to seventh aspects.

[0251] The eighth aspect is the ability to produce aqueous polyester resins with the aforementioned advantageous characteristics.

[0252] According to aspect nine, the aqueous polyester resin comprises: terephthalic acid residues derived from recycled polyester; and polycarboxylic acid residues other than terephthalic acid residues. The polycarboxylic acid residues comprise: polycarboxylic acid residues containing metal sulfonate groups; and other polycarboxylic acid residues other than terephthalic acid residues and polycarboxylic acid residues containing metal sulfonate groups. The proportion of terephthalic acid residues is equal to or greater than 20% by mass and equal to or less than 72% by mass relative to all polycarboxylic acid residues contained in the aqueous polyester resin. The proportion of polycarboxylic acid residues containing metal sulfonate groups is equal to or greater than 5% by mass and equal to or less than 32% by mass relative to all polycarboxylic acid residues contained in the aqueous polyester resin. The aqueous polyester resin has an acid value equal to or less than 10 mg KOH / g.

[0253] The ninth aspect allows aqueous polyester resins to possess the following advantageous characteristics. Specifically, aqueous polyester resins not only exhibit excellent water dispersibility, for example, even in the absence of surfactants, but also demonstrate good stability when used as resin dispersions, while reducing environmental impact. Furthermore, aqueous polyester resins contain terephthalic acid residues derived from recycled polyesters, but still possess the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyesters. Moreover, resin dispersions of aqueous polyester resins not only exhibit good long-term water dispersibility but also further improve stability, such as the aging stability of solution haze.

[0254] In the aqueous polyester resin according to the tenth aspect (which may be implemented in conjunction with the ninth aspect), the proportion of additional polycarboxylic acid residues is equal to or greater than 5% by mass and equal to or less than 50% by mass relative to all polycarboxylic acid residues contained in the aqueous polyester resin.

[0255] The tenth aspect allows for a more complete reduction in the crystallinity of aqueous polyester resins, thereby further improving their water dispersibility and the stability of their resin dispersions.

[0256] In the aqueous polyester resin according to the eleventh aspect (which may be implemented in conjunction with the ninth or tenth aspect), the polycarboxylic acid residues do not contain trivalent or higher valence polycarboxylic acid compound residues.

[0257] The eleventh aspect allows for a further reduction in the acid value of the aqueous polyester resin and the presence of even fewer cross-linked structures due to the presence of trivalent or higher-valence polycarboxylic acid compounds. Therefore, the water dispersibility of the aqueous polyester resin and the stability of its resin dispersion can be further improved.

[0258] The aqueous polyester resin according to aspect 12 (which may be implemented in combination with any of aspects 9 to 11) further comprises polyol residues. The polyol residues either do not contain ternary or higher-order polyol compound residues, or contain ternary or higher-order polyol compound residues. The proportion of ternary or higher-order polyol compound residues is equal to or less than 5% by mass relative to all polyol residues contained in the aqueous polyester resin.

[0259] The twelfth aspect allows aqueous polyester resins to have a moderate number of crosslinked structures, thereby further improving the water dispersibility of aqueous polyester resins and the stability and film-forming ability of their resin dispersions.

[0260] The aqueous polyester resin according to aspect thirteen (which may be implemented in combination with any of aspects nine through twelfth) further comprises polyol residues. The polyol residues comprise diol compound residues. The diol compound residues are branched. The proportion of branched diol compound residues is equal to or greater than 5% by mass and equal to or less than 50% by mass relative to all polyol residues contained in the aqueous polyester resin.

[0261] The thirteenth aspect allows for further improvement in the stability of aqueous polyester resin dispersions, such as the aging stability of solution haze.

[0262] The aqueous coating composition according to aspect fourteen comprises an aqueous polyester resin. The aqueous polyester resin comprises an aqueous polyester resin produced by the method according to any one of aspects one through seven, or an aqueous polyester resin according to any one of aspects eight through thirteen.

[0263] The fourteenth aspect allows the aqueous coating composition to have the following advantageous characteristics. Specifically, the aqueous coating composition not only exhibits excellent water dispersibility, for example, even in the absence of surfactants, but also demonstrates good stability when used as a resin dispersion, while reducing environmental impact. Furthermore, the aqueous coating composition contains terephthalic acid residues derived from recycled polyesters and still possesses the same good resin properties (e.g., adhesion and transparency) as when using terephthalic acid or terephthalic acid derivatives not derived from recycled polyesters. In addition, the resin dispersion of the aqueous coating composition not only exhibits good long-term water dispersibility but also further improved stability, such as aging stability of solution haze.

Claims

1. A method for producing aqueous polyester resin using recycled polyester, the method comprising: The first step includes inducing an esterification reaction and a depolymerization reaction after mixing the recycled polyester, a polycarboxylic acid component containing polycarboxylic acid residues but not terephthalic acid, and a polyol component; and The second step includes inducing a polycondensation reaction by reducing the pressure, wherein... The polycarboxylic acid component comprises: at least one polycarboxylic acid compound containing a metal sulfonate group selected from polycarboxylic acids, their esters, and acid anhydrides, each having a metal sulfonate group and containing a polycarboxylic acid residue containing a metal sulfonate group; and at least one additional polycarboxylic acid compound selected from polycarboxylic acids, their esters, and acid anhydrides, other than terephthalic acid and the said polycarboxylic acid compound containing a metal sulfonate group. The polyol component used in the first step comprises a diol compound having a branched chain, and the proportion of the branched diol compound relative to the total polyol component used is equal to or greater than 5% by mass and equal to or less than 50% by mass. The first step includes: using the recycled polyester in an amount such that the proportion of terephthalic acid residues relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 20% by mass and equal to or less than 72% by mass; and using the polycarboxylic acid compound containing metal sulfonate groups in an amount such that the proportion of polycarboxylic acid residues containing metal sulfonate groups relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component is equal to or greater than 5% by mass and equal to or less than 32% by mass. The aqueous polyester resin produced thereby has an acid value equal to or less than 10 mgKOH / g.

2. The method according to claim 1, wherein The first step further includes using the additional polycarboxylic acid compound in such an amount that the additional polycarboxylic acid residues are equal to or greater than 5% by mass and equal to or less than 50% by mass relative to the total amount of terephthalic acid residues contained in the recycled polyester and the total amount of polycarboxylic acid residues contained in the polycarboxylic acid component.

3. The method according to claim 1, wherein The polycarboxylic acid component used in the first step does not contain trivalent or higher-valent polycarboxylic acid compounds.

4. The method according to claim 1, wherein The polyol component used in the first step either does not contain ternary or higher-order polyol compounds, or contains ternary or higher-order polyol compounds. The proportion of the ternary or higher-order polyol compound is equal to or less than 5% by mass relative to all polyol components used.

5. A water-based polyester resin produced by the method according to any one of claims 1 to 4.

6. A water-based polyester resin comprising: terephthalic acid residues derived from recycled polyester, polycarboxylic acid residues other than the terephthalic acid residues, and polyol residues. The polycarboxylic acid residues include: polycarboxylic acid residues containing metal sulfonate groups, and other polycarboxylic acid residues besides the terephthalic acid residues and the polycarboxylic acid residues containing metal sulfonate groups. The proportion of terephthalic acid residues relative to all polycarboxylic acid residues contained in the aqueous polyester resin is equal to or greater than 20% by mass and equal to or less than 72% by mass; and the proportion of polycarboxylic acid residues containing metal sulfonate groups relative to all polycarboxylic acid residues contained in the aqueous polyester resin is equal to or greater than 5% by mass and equal to or less than 32% by mass. The polyol residues comprise diol compound residues, the diol compound residues being branched, and the proportion of the branched diol compound residues being equal to or greater than 5% by mass and equal to or less than 50% by mass relative to all polyol residues contained in the aqueous polyester resin. The aqueous polyester resin has an acid value equal to or less than 10 mgKOH / g.

7. The aqueous polyester resin according to claim 6, wherein... The proportion of the additional polycarboxylic acid residues is equal to or greater than 5% by mass and equal to or less than 50% by mass, relative to all the polycarboxylic acid residues contained in the aqueous polyester resin.

8. The aqueous polyester resin according to claim 6, wherein... The polycarboxylic acid residues do not contain trivalent or higher-valent polycarboxylic acid compound residues.

9. The aqueous polyester resin according to claim 6 further comprises polyol residues, wherein... The polyol residues do not contain ternary or higher-order polyol compound residues, or contain ternary or higher-order polyol compound residues, and The proportion of ternary or higher-order polyol compound residues is equal to or less than 5% by mass relative to all polyol residues contained in the aqueous polyester resin.

10. A water-based coating composition comprising a water-based polyester resin, The aqueous polyester resin comprises an aqueous polyester resin produced by the method according to any one of claims 1 to 4 or an aqueous polyester resin according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • Sulfoaryl-modified water-soluble or water-dispersible resins from polyethylene terephthalate or terephthalates

    JP2001505608A

  • Method for reusing polyester chip

    WO2001016208A1

  • Recycled method for a wasted polyester and reclaimed materials thereof

    WO2003051956A1

  • Recycled method for a wasted polyester and reclaimed materials thereof

    CN1747982A

  • Aqueous adhesive and coat produced therefrom

    JP2015229718A