Apparatus and method for producing water-absorbent resin particles

By setting up a sorting machine and sorting components during the manufacturing process of water-absorbing resin particles, resin precursors with high water content are removed, and the surface temperature is ensured to be between 50℃ and 100℃. This achieves stability in the pressurized water absorption capacity and water absorption speed of the water-absorbing resin particles, and solves the quality deviation problem existing in the prior art.

CN117120519BActive Publication Date: 2026-11-20SUMITOMO SEIKA CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280023550.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2022-03-04
Publication Date
2026-11-20
Estimated Expiration
2042-03-04

AI Technical Summary

Technical Problem

In existing technologies, the pressure absorption capacity and absorption rate of water-absorbing resin particles are prone to deviations and are difficult to control effectively.

Method used

In the manufacturing process of water-absorbing resin particles, a sorting machine is set up after the dryer to remove water-absorbing resin precursors with a moisture content of more than 20%. The sorting machine is equipped with sorting components with a surface temperature of 50℃~100℃, and uses mesh or plate components for grading to ensure the uniformity of water-absorbing resin precursors.

Benefits of technology

It effectively suppressed the deviation in the pressure absorption capacity and absorption speed of the water-absorbing resin particles, thus improving the consistency of product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117120519B_ABST
    Figure CN117120519B_ABST
Patent Text Reader

Abstract

A water-absorbent resin particle production apparatus includes a dryer, a classifier, and a sorter. The dryer dries a water-absorbent resin composition to obtain a water-absorbent resin precursor. The classifier classifies the water-absorbent resin precursor to obtain a water-absorbent resin particle. The sorter is arranged on a path connecting the dryer and the classifier. The sorter is configured to sort the water-absorbent resin precursor having a moisture content of 20% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an apparatus and method for manufacturing water-absorbing resin particles. Background Technology

[0002] The manufacturing process of water-absorbing resin particles includes: a process of polymerizing monomers as raw materials to obtain a water-absorbing resin composition; and a process of drying the water-absorbing resin composition to obtain a water-absorbing resin precursor. By classifying the water-absorbing resin precursor after these processes using a classifier, water-absorbing resin particles with a target particle size distribution can be manufactured.

[0003] Patent Document 1 discloses an apparatus for manufacturing a water-absorbing resin, comprising: a dryer for drying a water-absorbing resin composition to obtain powder; a powder flow path member for forming a flow path of the powder; a powder flow rate adjusting discharge member for discharging the powder at a given flow rate; and a trapping member. According to Patent Document 1, by using the trapping member to trap powder lumps larger than a predetermined size in the powder passing through the flow path, it is possible to suppress the increase in drive load of the drive unit of the powder flow rate adjusting discharge member due to powder lumps, thereby enabling the manufacture of water-absorbing resin with high production efficiency. Existing technical documents Patent documents

[0004] Patent Document 1: Japanese Patent No. 6738979 Summary of the Invention The technical problem that the invention aims to solve

[0005] According to Patent Document 1, large powder lumps have poor properties as a water-absorbing resin. Therefore, by capturing and removing large powder lumps with a collecting element, production efficiency can be improved and high-quality water-absorbing resin can be manufactured. However, according to the manufacturing apparatus disclosed in Patent Document 1, deviations in the quality of the water-absorbing resin particles still occur.

[0006] As indicators of the quality of absorbent resin particles, various properties such as water absorption performance (absorption rate, water absorption capacity under pressure, etc.), impact resistance, and flowability are commonly cited. The inventors of this invention conducted research and found that, in particular, water absorption capacity under pressure and water absorption rate are prone to deviation. Therefore, an apparatus is desired that can manufacture absorbent resin particles that further suppress deviations in quality aspects such as water absorption capacity under pressure and water absorption rate.

[0007] The purpose of this invention is to provide an apparatus and a method for manufacturing absorbent resin particles in which deviations in pressure absorption capacity and absorption rate are suppressed. Technical solutions for solving technical problems

[0008] The apparatus for manufacturing superabsorbent resin particles according to the first viewpoint includes a dryer, a classifier, and a separator. The dryer dries the superabsorbent resin composition to obtain a superabsorbent resin precursor. The classifier classifies the superabsorbent resin precursor to obtain superabsorbent resin particles. The separator is positioned on a path connecting the dryer and the classifier. The separator is used to separate superabsorbent resin precursors with a moisture content of 20% or more.

[0009] According to the inventors' research, the water-absorbing resin precursor after drying in the dryer still contains a significant amount of water. If such a water-absorbing resin precursor is fed into a classifier, the quality of the resulting water-absorbing resin particles, particularly their pressure absorption capacity and absorption rate, is prone to deviation. The water-absorbing resin particle manufacturing apparatus according to the above viewpoint separates water-absorbing resin precursors with a moisture content of 20% or more in the path connecting the dryer and the classifier. This removes the separated water-absorbing resin precursors with a moisture content of 20% or more from the path connected to the classifier, reducing deviations in the pressure absorption capacity and absorption rate of the water-absorbing resin particles.

[0010] The apparatus for manufacturing water-absorbing resin particles according to the second viewpoint is configured such that, in the apparatus for manufacturing water-absorbing resin particles according to the first viewpoint, the sorting mechanism sorts the water-absorbing resin precursor with a surface temperature of 50°C to 100°C and exceeding a given size into water-absorbing resin precursors with a water content of 20% or more.

[0011] The apparatus for manufacturing superabsorbent resin particles according to the third viewpoint is configured such that, in the apparatus for manufacturing superabsorbent resin particles according to the second viewpoint, the sorting machine includes: an inlet having an inlet for feeding superabsorbent resin precursor discharged from the dryer; and a sorting member connected to the inlet and having an opening of the given size. The sorting mechanism serves to transport superabsorbent resin precursor fed into the inlet, passing through the opening, to a path connected to the classifier.

[0012] The apparatus for manufacturing water-absorbing resin particles according to the fourth viewpoint is configured such that, in the apparatus for manufacturing water-absorbing resin particles according to the third viewpoint, the sorting member is composed of a mesh member having a plurality of openings of the given size.

[0013] The apparatus for manufacturing water-absorbing resin particles according to the fifth viewpoint is configured such that, in the apparatus for manufacturing water-absorbing resin particles according to the third or fourth viewpoint, the sorting member is configured to impart movement to the water-absorbing resin precursor fed into the inlet.

[0014] The apparatus for manufacturing water-absorbing resin particles according to the sixth viewpoint is configured such that, in the apparatus for manufacturing water-absorbing resin particles according to any one of the second to fifth viewpoints, the given size is 7 mm to 15 mm.

[0015] The seventh viewpoint concerns an apparatus for manufacturing superabsorbent resin particles, which, in any of the first to sixth viewpoints, further includes a cooler disposed on the path connecting the sorter and the classifier. The cooling mechanism cools the superabsorbent resin precursor conveyed from the sorter to the path connected to the classifier.

[0016] The method for manufacturing the water-absorbing resin particles involved in the eighth point includes the following steps. • The step of drying the water-absorbing resin composition to obtain the water-absorbing resin precursor. • The step of sorting and removing the water-absorbing resin precursor with a water content of 20% or more from the water-absorbing resin precursor. • The step of classifying the remaining absorbent resin precursor to obtain classified absorbent resin particles. Invention Effects

[0017] Even after drying in a dryer, the superabsorbent resin precursor still contains a significant amount of moisture. This moisture content contributes to deviations in the pressure absorption capacity and absorption rate of the superabsorbent resin particles after classification by the classifier. Based on this, superabsorbent resin precursors with a moisture content of 20% or higher are separated from the superabsorbent resin precursor along the path connecting the dryer and the classifier. This removes the separated superabsorbent resin precursor from the path connected to the classifier, thus suppressing deviations in the pressure absorption capacity and absorption rate of the superabsorbent resin particles obtained by the classifier. Attached Figure Description

[0018] Figure 1 This is an overall structural diagram of an apparatus for manufacturing water-absorbing resin particles according to one embodiment. Figure 2A Examples of mesh components. Figure 2B Examples of mesh components. Figure 2C Examples of mesh components. Figure 2D Examples of mesh components. Figure 3A Examples of plate-shaped components. Figure 3B Examples of plate-shaped components. Figure 4 A diagram illustrating the calculation method for the aperture ratio. Figure 5A This is an example of the structure of a sorting machine. Figure 5B This is an example of the structure of a sorting machine. Figure 5C This is an example of the structure of a sorting machine. Figure 5D This is an example of the structure of a sorting machine. Figure 6 A diagram illustrating the method for determining the size of the water-absorbing resin precursor. Figure 7 This is a flowchart illustrating a method for manufacturing water-absorbing resin particles according to one embodiment. Figure 8 A diagram showing the structure of the experimental setup. Figure 9A This is a graph showing the water absorption under pressure obtained through experiments. Figure 9B A chart showing the evaluation index of water absorption rate obtained through experiments. Detailed Implementation

[0019] Hereinafter, with reference to the accompanying drawings, an apparatus for manufacturing water-absorbing resin particles and a method for manufacturing water-absorbing resin particles according to an embodiment of the present invention will be described. Furthermore, in this specification, the term "sorting" refers not only to "extracting only a specific subgroup a from a large group X", but also to "extracting a specific subgroup a from a large group X while including other subgroups b (wherein, the proportion of subgroup a included in the large group X is higher than that of subgroup a included in the large group X (quality benchmark))".

[0020] <1. Apparatus for manufacturing water-absorbing resin particles> Figure 1 This diagram shows the overall structure of the apparatus 100 used in the method for manufacturing the absorbent resin particles according to this embodiment. Absorbent resin particles are widely used in various applications, including disposable diapers, sanitary products, pet diapers, food absorbent sheets, cable waterproofing materials, anti-condensation materials, water-retaining agents for landscaping, agriculture, and horticulture, and soil conditioners. Absorbent resin particles are manufactured by polymerizing monomers used as raw materials to produce polymers.

[0021] like Figure 1As shown, the apparatus 100 for manufacturing superabsorbent resin particles includes a polymerizer 1 and a concentrator 2. The polymerizer 1 produces a slurry (liquid containing a hydrogel-like polymer) by polymerizing monomers that become the raw materials for the superabsorbent resin particles. The concentrator 2 removes the liquid component from the slurry from the polymerizer 1 by distillation, concentrating the slurry to produce a superabsorbent resin composition A1 as a polymer concentrate. The apparatus 100 also includes a dryer 3, which dries the superabsorbent resin composition A1 from the concentrator 2 (i.e., evaporates the liquid component). Thus, a superabsorbent resin precursor A2 is obtained before becoming the superabsorbent resin particles P1 as a product. The liquid component mainly includes a hydrocarbon dispersion medium and water when the hydrogel-like polymer is produced using reverse-phase suspension polymerization; and mainly includes water when the hydrogel-like polymer is produced using aqueous solution polymerization.

[0022] like Figure 1 As shown, the manufacturing apparatus 100 also includes a sorting machine 4, a cooler 5, and a classifier 6. The sorting machine 4 sorts the absorbent resin precursor A2 with a moisture content of 20% or more from the absorbent resin precursor A2 fed by the dryer 3 and discharges it from the first outlet 43. Furthermore, in order to convey the remaining absorbent resin precursor A3 to the cooler 5, the sorting machine 4 discharges the remaining absorbent resin precursor A3 from a separate second outlet 44. The cooler 5 cools the absorbent resin precursor A3 discharged from the second outlet 44, removing the heat imparted by the dryer 3, and then conveys the absorbent resin precursor A3 to the classifier 6. The classifier 6 classifies the absorbent resin precursor A3 into several grades. The absorbent resin precursors classified into grades that meet the specifications for the product from the absorbent resin precursor A3 are called absorbent resin particles P1.

[0023] In addition, such as Figure 1 As shown, the manufacturing apparatus 100 also includes a control device 7 that controls the manufacturing process of the absorbent resin by controlling the operation of each of the devices 1 to 6. The control device 7 is typically implemented as a computer controlled by a program. The control device 7 may also be configured to control, in addition to controlling the operation of each of the devices 1 to 6, the piping that forms the path connecting each of the devices 1 to 6 and the first to fourth channel members L1 to L4, as well as the valves that can be installed thereon.

[0024] <2. Structure of each piece of equipment> The following details the details of each of the devices 1 to 6, and also provide appropriate descriptions of the various devices connected to each of these devices 1 to 6.

[0025] [Aggregator] Polymer 1 has a polymerization tank (not shown). The polymerization tank is a container for holding monomers, such as water-soluble olefinic unsaturated monomers, which serve as raw materials for water-absorbent resin particles, and a liquid component, with a gaseous component forming at the top. Inside the polymerization tank, the monomers and liquid component are appropriately stirred using a stirrer (not shown), and heated using a heating device (not shown), thereby carrying out the polymerization reaction of the monomers to produce a hydrogel-like polymer. These stirrers and heating devices are connected to a control device 7, and their operation is controlled. Through the above, a polymer containing a hydrogel-like polymer is contained within the polymerization tank. slurry The slurry is discharged from the polymerizer 1 through a lower opening formed at the bottom of the polymerization tank in order to be sent to the thickener 2.

[0026] One end of a pipe is connected to the lower opening of the polymerization tank. The other end of the pipe is connected to an opening formed in the upper part of the thickener 2. The slurry discharged from the polymerizer 1 is fed into the thickener 2 through the upper opening of the thickener 2 via the pipe. A valve is installed on the pipe, and the opening and closing of the valve is controlled by a control device 7 to control the flow of slurry through the pipe.

[0027] [Concentrator] The concentrator 2 has a concentration tank (not shown). The slurry discharged from the polymerizer 1 flows into the concentration tank through an upper opening formed in the upper part of the concentrator 2, and is contained in such a way that a gaseous component forms in the upper part of the concentration tank. Inside the concentration tank, the slurry is appropriately stirred using a stirrer (not shown) and heated using a heating device (not shown), thereby distilling away the liquid components contained therein and concentrating the slurry. These stirrers and heating devices are connected to a control device 7, and their operation is controlled. Through the above, a concentrate containing a hydrogel-like polymer is contained in the concentration tank. The concentrate containing the hydrogel-like polymer is sent to the dryer 3 as a water-absorbing resin composition A1 and discharged from the concentrator 2 through a lower opening formed in the lower part of the concentration tank.

[0028] One end of a pipe is connected to the lower opening of the concentrator tank. The other end of the pipe is connected to the upper opening formed in the upper part of the dryer 3. The water-absorbing resin composition A1 discharged from the concentrator 2 is introduced into the dryer 3 through the upper opening of the dryer 3 via the pipe. A valve is installed on the pipe, and the opening and closing of the valve is controlled by a control device 7 to control the flow of the water-absorbing resin composition A1 through the pipe.

[0029] [Dryer] The dryer 3 has a drying chamber (not shown). The water-absorbing resin composition A1 discharged from the concentrator 2 flows into the drying chamber through the upper opening of the dryer 3. The dryer 3 heats the water-absorbing resin composition A1 in the drying chamber using a heating device (not shown), removing moisture contained therein. This produces a water-absorbing resin precursor A2 obtained by drying the water-absorbing resin composition A1. The heating device is connected to a control device 7, and its operation is controlled. The heating device dries the water-absorbing resin composition A1 so that the overall moisture content (mass%) of the water-absorbing resin composition A1 contained in the drying chamber is preferably 20% or less, more preferably 10% or less. The dried water-absorbing resin precursor A2 is discharged from the dryer 3 through the lower opening formed in the lower part of the drying chamber in order to be conveyed into the first channel member L1 described later.

[0030] The dryer 3 can also be configured to dry the slurry discharged from the polymerizer 1 as the water-absorbing resin composition A1. That is, the manufacturing apparatus 100 can omit the concentrator 2 and directly connect the polymerizer 1 to the dryer 3. In this case, the slurry discharged from the polymerizer 1 is equivalent to the water-absorbing resin composition A1. Moreover, the dryer 3 simultaneously concentrates and dries the water-absorbing resin composition A1.

[0031] [First Channel Component] The first channel member L1 is a component that defines a channel for moving the absorbent resin precursor A2 in a given direction, and together with the second channel member L2, the third channel member L3, and the fourth channel member L4 (described later), forms a path connecting the dryer 3 and the classifier 6. One end of the first channel member L1 is connected to the lower opening of the drying chamber. The first channel member L1 is constructed of piping, and the absorbent resin precursor A2 can move within the first channel member L1, for example, by gravity, but is not limited thereto. Inside the first channel member L1, a trapping element 30 is arranged in a manner that intersects the direction of movement of the absorbent resin precursor A2. More specifically, the trapping element 30 is disposed in the first channel member L1 such that its outer peripheral end contacts the inner surface of the first channel member L1. Thus, the internal space of the first channel member L1 is divided into a channel on the upstream side of the dryer 3, separated by the trapping element 30, and a channel on the downstream side of the classifier 4, separated by the trapping element 30.

[0032] The trapping member 30 is used to trap powder lumps B1 larger than a predetermined size from the absorbent resin precursor A2 flowing into the first channel member L1 and remove them from the manufacturing apparatus 100. The powder lumps B1 may be, for example, lumps formed by the nucleation of a hydrogel-like polymer or absorbent resin composition A1 adhering to the inner wall of the polymerization tank, concentration tank, or drying chamber, or lumps formed by the agglomeration of the absorbent resin composition A1. Due to their size, the powder lumps B1 cannot pass through the gap defined by the trapping member 30 and will not reach the downstream channel. On the other hand, the remaining absorbent resin precursor A2 passes through the gap defined by the trapping member 30 and reaches the downstream channel, where it moves further. Regarding the specific structure of the trapping member 30, since it is disclosed in Patent Document 1, it is considered to be the structure described in this specification, and detailed description is omitted here. The powder lumps B1 removed by the collecting member 30 are larger than the absorbent resin precursor B2 separated by the separating member 42 of the separator 4 (described later). The particle size of the powder lumps B1 is, for example, 30 mm or more, preferably 50 mm or more.

[0033] A retrieval opening 31 communicating with an upstream channel is formed in the first channel member L1. The retrieval opening 31 defines an opening for removing the powder lumps B1 captured by the collecting member 30 to the outside of the first channel member L1. The collecting member 30 is disposed inside the first channel member L1 such that the captured powder lumps B1 move toward the retrieval opening 31, for example, by gravity. Thus, the powder lumps B1 are removed to the outside of the first channel member L1 via the retrieval opening 31, so as not to block the gap of the collecting member 30 and the upstream channel.

[0034] The absorbent resin precursor A2 flowing into the downstream channel of the first channel member L1 is sent to the sorter 4 via the second channel member L2 connected to the first channel member L1. The first channel member L1 and the second channel member L2 may also be connected via a relay member 32 that relays the path of the absorbent resin precursor A2, such as a hopper for temporarily storing the absorbent resin precursor A2.

[0035] [Second Channel Component] The second channel component L2 is a component that defines a channel for conveying the hygroscopic resin precursor A2 from the first channel component L1 to the separator 4, and forms a path connecting the dryer 3 and the classifier 6. The method of conveying the hygroscopic resin precursor A2 from the first channel component L1 to the separator 4 is not particularly limited; methods such as gravity conveying, conveying using an inactive gas flow, or conveying using a conveyor or other conveying mechanism can be appropriately selected. The method by which the second channel component L2 is configured to input the hygroscopic resin precursor A2 into the inlet 40 of the separator 4 according to the conveying method of the hygroscopic resin precursor A2 is not particularly limited. For example, the second channel component L2 can be constructed using piping, conveying piping that generates airflow therein, a conveyor, a feeder, etc. A valve controlled by the control device 7 may also be installed on the second channel component L2 to adjust the flow rate of the hygroscopic resin precursor A2. Additionally, a surface temperature adjustment device may be provided on the second channel member L2 to adjust the surface temperature of the water-absorbing resin precursor A2 fed into the sorter 4. The surface temperature adjustment device is a device (heater) for heating the second channel member L2 from the outside and / or the inside, and / or a device (cooler) for cooling it. For example, the surface temperature adjustment device has a tubular member wound around the outside of the second channel member L2, through which a heat medium such as water vapor can pass to heat and / or cool the second channel member L2. The lower limit of the surface temperature of the water-absorbing resin precursor A2 introduced into the sorting machine is 50°C or higher, preferably 55°C or higher, and more preferably 60°C or higher. Furthermore, the upper limit is 100°C or lower, preferably 95°C or lower, more preferably 90°C or lower, even more preferably 85°C or lower, and particularly preferably 80°C or lower. In summary, the surface temperature of the water-absorbing resin precursor A2 introduced into the sorting machine can be 50°C to 100°C, and more preferably 60°C to 80°C. According to the inventors' understanding of the present invention, if the surface temperature of the water-absorbing resin precursor A2 is within the above-mentioned range, the water-absorbing resin precursor A2 with a water content of 20% or more can be efficiently separated by a sorting machine (the mixing rate of water-absorbing resin precursor A2 with a water content of less than 20% in the separated water-absorbing resin precursor B2 is suppressed to be low).

[0036] [Sorting Machine] The sorting machine 4 can be configured, for example, as a vibrating sorting machine, a drum screen (rotary sorting machine), or other screening devices. The sorting machine 4 is positioned on the path connecting the dryer 3 and the classifier 6 to separate absorbent resin precursors with a moisture content of 20% or more from the absorbent resin precursor A2 discharged from the dryer 3. The sorting machine 4 includes an inlet portion 41 with an inlet 40 and a sorting member 42. The inlet 40 is an opening for receiving the absorbent resin precursor A2 discharged from the dryer 3 and fed through the second channel member L2. In this embodiment, the inlet portion 41 is a housing that houses the sorting member 42. Inside the inlet portion 41, a sorting area 45 (see reference 45) is defined for separating the absorbent resin precursor A2. Figures 5A-5D The sorting member 42 is connected in a manner that allows for connection to the inlet 41. As described later, the sorting member 42 may also be connected to the inlet 41 via other members connected to it. The sorting area 45 is defined by at least one of the sorting member 42, the inlet 41, and other members. As described later, the sorting member 42 may be configured to be movable in order to impart movement to the absorbent resin precursor A2 within the sorting area 45, and its movement may be controlled by the control device 7.

[0037] The absorbent resin precursor A2, discharged from the dryer 3, is fed into the separator 4 at a surface temperature of 50°C to 100°C. The absorbent resin precursor A2 fed into the separator 4 first enters the sorting zone 45. A first outlet 43 and a second outlet 44 are formed in the housing to connect the inside and outside of the separator. The absorbent resin precursor A2 entering the sorting zone 45 is divided into two parts by the sorting member 42 and discharged from either outlet 43 or 44 out of the separator 4.

[0038] [Sorting Components] The overall shape of the sorting member 42 can be appropriately selected as planar, cylindrical, frustum conical, or rectangular. The sorting member 42 has multiple openings of a given size that connect the inside and outside of the sorting area 45. Therefore, among the absorbent resin precursors A2 entering the sorting area 45, those exceeding the size of the openings in the sorting member 42 cannot pass through and are sorted into those that can pass through the openings. For reasons explained later, the sorted absorbent resin precursors A2 are removed from the path connecting the sorter 4 and the classifier 6. Hereinafter, the absorbent resin precursors A2 that cannot pass through the openings in the sorting member 42 will be referred to as absorbent resin precursor B2, and the absorbent resin precursors that can pass through the openings in the sorting member 42 will be referred to as absorbent resin precursor A3.

[0039] The sorting member 42 in this embodiment is composed of a mesh member 42a having multiple openings (generally also referred to as "mesh"). The mesh member 42a is, for example, as shown in... Figure 2AAs shown, it is formed by weaving wire-like components made of metal or the like into a square grid. Figure 2A In the example shown, the weaving method of the linear components is not particularly limited; it can be a plain weave with a flat top or a twill weave. However, the components constituting the sorting component 42 are not limited to Figure 2A The square grid-like mesh member 42a shown can be modified appropriately. The shape of the sorting member 42 will be described in detail below.

[0040] <The component constituting the sorting component 42 is a square grid-like mesh component 42a> The components constituting the sorting component 42 are Figure 2A In the case of the square grid-like mesh member 42a shown, the size of the openings of the mesh member 42a is defined by the mesh size E, which depends on the number of openings per inch and the wire diameter of the wire member. Specifically, the mesh size E of the sorting member 2 is defined by the following formula (1). Formula (1)...E(mm)=(25.4 / M)-d(mm) In Equation (1), M represents the number of openings per inch (25.4 mm), and d represents the wire diameter of the linear component.

[0041] The lower limit of the wire diameter d can be 0.8 mm or more, preferably 1.0 mm or more, more preferably 1.3 mm or more, and particularly preferably 1.5 mm or more. Furthermore, the upper limit can be 2.2 mm or less, preferably 2.0 mm or less, more preferably 1.8 mm or less, and particularly preferably 1.7 mm or less. In summary, the wire diameter d can be 0.8 mm to 2.2 mm, preferably 1.0 mm to 2.0 mm, more preferably 1.3 mm to 1.8 mm, and particularly preferably 1.5 mm to 1.7 mm. If the wire diameter d is within this range, the adhesion of the water-absorbing resin precursor A2 to the sorting member 42 can be suppressed, and water-absorbing resin particles can be produced with a good yield. Furthermore, the lower limit of the mesh size E can be 7mm or more, 8mm or more, preferably 9mm or more, 9.5mm or more, and more preferably 9.8mm or more. The upper limit can be 15mm or less, 14mm or less, 13mm or less, 12mm or less, 11mm or less, preferably 10.5mm or less, and more preferably 10.2mm or less. In summary, the mesh size E can be 7mm to 15mm or less, preferably 9mm to 11mm, more preferably 9.5mm to 10.5mm, and even more preferably 9.8mm to 10.2mm. If the mesh size E is within the above range, it is possible to efficiently sort the water-absorbing resin precursor A2 with a moisture content of 20% or more.

[0042] In addition, in the sorting component 42 Figure 2A In the case of the square grid shown, the opening ratio defined by the following formula (2) can be 55% or more, preferably 60% or more, more preferably 65% ​​or more, and particularly preferably 70% or more. In addition, its upper limit can be 90% or less, preferably 85% or less, more preferably 80% or less, and particularly preferably 77% or less. Equation (2)... Opening ratio (%) = (E / E+d) 2 ×100 If the opening ratio is within the above range, it can efficiently sort water-absorbing resin precursor A2 with a water content of more than 20%.

[0043] <The component constituting the sorting member is a mesh component 42a other than a square grid.> In addition, for example, Figures 2B-2D As shown, when the shape of the opening of the mesh member 42a is, for example, a rectangle, a parallelogram, a hexagon, etc., the smallest interval E among the intervals of the mutually parallel linear members that define an opening is taken as the size of the opening. In this case, in the mesh member 42a, the average value Em of E measured at 10 randomly selected different openings is taken as the size of the opening of the mesh member 42a.

[0044] Other forms of components constituting the sorting member 42 include, for example, Figure 3A And a plate-like member 42b, as shown in 3B, having multiple openings (similar to mesh member 42a, also referred to as "mesh") formed. Plate-like member 42b is, for example, a metal plate having multiple through holes formed by punching. For example, Figure 3A As shown, when the opening of the plate-shaped member 42b in its unfolded planar state is circular, the diameter E of the circle is taken as the size of the opening. Additionally, for example... Figure 3B As shown, when the opening of the plate member 42b is oblong, the interval E between the parallel peripheries defining the opening is taken as the size of the opening. Furthermore, when the opening of the plate member 42b is, for example, rectangular, parallelogram, or hexagonal, the smallest interval E among the intervals between the parallel peripheries defining the opening is taken as the size of the opening, following the same principle as the mesh member 42a. For the plate member 42b, also similarly to the mesh member 42a, the average value Em of E measured at 10 randomly selected openings is taken as the size of the opening of the plate member 42b.

[0045] In the sorting component 42 Figures 2B to 3B In the case of the illustrated mesh member 42a or plate member 42b, the size (mesh size) of the opening of the sorting member 42 is preferably within the range described above.

[0046] In addition, in the sorting component 42, Figures 2B to 3B In the case of the illustrated mesh member 42a or plate member 42b, the opening ratio of the sorting member 42 can be appropriately selected according to the overall shape of the sorting member 42. Figure 4 This diagram illustrates the calculation method for the opening ratio of the sorting member 42. Regarding the opening ratio, in the sorting member 42 unfolded into a plane, the smallest rectangle R among the rectangles formed by connecting the centers of the opening shapes is defined. The opening ratio can be set as the ratio of the total area SA occupied by the openings within the region enclosed by rectangle R to the area SR of rectangle R. Figure 4 The example shown is of a sorting member 42 with a regular hexagonal opening, but the above method for calculating the opening ratio can also be applied to sorting members 42 with openings of other shapes. In the sorting component 42 Figures 2B to 3B When the illustrated mesh member 42a or plate member 42b is used, its opening ratio is preferably within the range described above.

[0047] [Structure example of a sorting machine] Figures 5A to 5D This illustrates the structure of sorting machine 4. For example... Figures 5A to 5D As shown, the orientation of the inlet 40 and the positional relationship between the inlet 41 and the sorting member 42 are not particularly limited and can be appropriately selected. Furthermore, the shape of the inlet 41 and the orientation of the inlet 40 can also be appropriately selected based on the overall shape of the sorting member 42. The first outlet 43 formed in the sorter 4 is an opening for removing the hygroscopic resin precursor B2 from the sorting area 45 to prevent clogging of the sorting member 42. The second outlet 44 formed in the sorter 4 is an opening for discharging the hygroscopic resin precursor A3 from the sorter 4 and sending it to the third channel member L3, which defines a path connected to the classifier 6, and further to the cooler 5 and the fourth channel member L4.

[0048] Figure 5AThis is an example where the sorting member 42 is flat. In this example, the sorting member 42 is connected to the inlet 41 via a channel member 46 that defines a channel connecting to the inlet 40. The channel member 46, together with the sorting member 42, defines a sorting area 45. The absorbent resin precursor A2 fed into the inlet 40 passes through multiple openings in the sorting member 42, reaches outside the sorting area 45, and is discharged from the second outlet 44. On the other hand, the absorbent resin precursor B2 is discharged from the first outlet 43. Alternatively, the sorting member 42 may be tilted relative to the horizontal direction to allow the absorbent resin precursor B2 to move more quickly toward the first outlet 43. Furthermore, the sorting member 42 may be configured to vibrate via a vibration mechanism (not shown) to impart movement to the absorbent resin precursor A2, preventing blockage of the openings.

[0049] Figure 5B This is an example where the sorting member 42 is cylindrical or rectangular. In this example, both ends of the sorting member 42 are open in the axial direction. The sorting member 42 is connected to the inlet 41 with both ends facing horizontally and connected to the inlet 40 and the first outlet 43, respectively. The absorbent resin precursor A2 fed into the inlet 40 passes through the multiple openings of the sorting member 42, reaches outside the sorting area 45, and is discharged from the second outlet 44. On the other hand, the absorbent resin precursor B2 is discharged from the first outlet 43 via one end of the sorting member 42. The sorting member 42 may also be configured to rotate about the axial direction via a rotating mechanism (not shown) to impart movement to the absorbent resin precursor A2, thereby preventing the opening from being blocked and causing blockage. Furthermore, in order to move the absorbent resin precursor B2 more quickly to the first outlet 43, the sorting member 42 may have a blade member inside that can move from the end on the inlet 40 side to the end on the first outlet 43. Additionally, the sorting member 42 may also be frustoconical in shape.

[0050] Figure 5CThis is another example where the sorting member 42 is cylindrical or rectangular. In this example, the sorting member 42 is connected to the inlet 41 with one end facing upwards in the vertical direction and the other end facing downwards in the vertical direction. The downward end (lower end) of the sorting member 42 is not open and is continuously formed with the side periphery of the sorting member 42. That is, multiple openings of a given size are also formed at the lower end of the sorting member 42. The absorbent resin precursor A2 fed into the inlet 40 passes through the multiple openings of the sorting member 42, reaches outside the sorting area 45, and is discharged from the second outlet 44. Near the lower end, the sorting member 42 is connected to a channel member 47 that defines a channel connecting the sorting area 45 and the first outlet 43. The inner diameter of the channel of the channel member 47 is larger than the size of the absorbent resin precursor B2. Thus, the absorbent resin precursor B2 is discharged from the first outlet 43 through the channel member 47. The sorting member 42 can also be configured to vibrate via a vibration mechanism (not shown) to impart movement to the absorbent resin precursor A2, preventing blockage of the opening. Furthermore, to allow the absorbent resin precursor B2 to move more rapidly toward the channel member 47, the lower end of the sorting member 42 can be inclined relative to the horizontal direction. Moreover, the sorting member 42 can also be frustoconical in shape.

[0051] Figure 5D This is another example where the sorting component 42 of the sorter 4 is cylindrical or square. This example is similar to... Figure 5B The difference in the examples is that the sorting member 42 is arranged with its cylindrical shaft inclined relative to the horizontal direction. The sorting machine 4 can also be configured such that the inclination angle of the sorting member 42 can vary within a certain range. In other respects, regarding... Figure 5B The example is applicable, therefore the explanation is omitted.

[0052] As described above, the sorting machine 4 is configured to sort the water-absorbing resin precursor A2 based on its size (particle size) with a surface temperature of 50°C to 100°C. In this specification, for convenience, the size of the water-absorbing resin precursor A2 used as the sorting criterion is as follows: Figure 6The values ​​are determined as shown. Specifically, the circumscribed rectangles Rx, Ry, and Rz of the projected shapes of the absorbent resin precursor A2 on three mutually orthogonal planes are defined respectively, and the average value of the long sides of these circumscribed rectangles Rx, Ry, and Rz is taken as the size (particle size) of the absorbent resin precursor A2. In this embodiment, absorbent resin precursor A2 with a surface temperature of 50°C to 100°C and a size that exceeds the size of the opening (given size) of the sorting member 42 is sorted as absorbent resin precursor B2. Furthermore, in this embodiment, absorbent resin precursor A2 with a surface temperature of 50°C to 100°C and a size that is less than the size of the opening of the sorting member 42 is conveyed to the classifier 6 as absorbent resin precursor A3.

[0053] [Reasons for sorting water-absorbing resin precursors] The reasons for sorting water-absorbing resin precursor A2 with a moisture content of 20% or more, and the reasons for efficiently sorting water-absorbing resin precursor B2 with a surface temperature of 50°C to 100°C and exceeding the size of the opening of the sorting member 42 for water-absorbing resin precursor A2 with a moisture content of 20% or more, will be explained below.

[0054] The absorbent resin precursor A2 is dried in dryer 3 until its overall moisture content is at least 20% or less. However, due to the temperature distribution within the drying chamber, the degree of drying of each absorbent resin precursor A2 varies. Therefore, some absorbent resin precursors A2 are not fully dried. According to the inventors' research, such absorbent resin precursor A2 contains a significant amount of moisture even at relatively high temperatures after drying, thus affecting the quality of the absorbent resin particles P1, such as their pressure absorption capacity and absorption rate. In other words, the presence of absorbent resin precursor A2 with a moisture content of 20% or more leads to a larger deviation in the pressure absorption capacity and absorption rate of the graded absorbent resin particles P1, making it more difficult to control the pressure absorption capacity and absorption rate of the absorbent resin particles P1.

[0055] The inventors confirmed through experiments described later that if the water-absorbing resin precursor A2 with a surface temperature of 50°C to 100°C after drying is separated using the sorting machine 4, water-absorbing resin precursor A2 with a moisture content of 20% or more can be separated efficiently. The given size is determined by the size of the opening of the sorting member 42 provided by the sorting machine 4. Therefore, the given size of the water-absorbing resin precursor A2 as a sorting reference, as described above for the size of the opening of the sorting member 42, can be 7 mm to 15 mm or less, preferably 9 mm to 11 mm, more preferably 9.5 mm to 10.5 mm, and even more preferably 9.8 mm to 10.2 mm. The experiments described later confirmed that the water content of the water-absorbing resin precursor B2 separated using the sorting machine 4, which has a sorting member 42 with an opening of 10 mm, is 60% or more. In this way, when the water-absorbing resin precursor A2 discharged from the dryer 3 is sorted by the sorter 4, it can be said that the substance with higher water content is sorted as water-absorbing resin precursor B2.

[0056] The water content of the sorted water-absorbing resin precursor B2 can be 20% or more, preferably 30% or more, or 40% or more, more preferably 50% or more, and more preferably 60% or more. Furthermore, its upper limit can be 85% or less, preferably 75% or less, or 70% or less, and more preferably 65% ​​or less.

[0057] Furthermore, the inventors experimentally confirmed the following: if the absorbent resin precursor A2 is sorted at a relatively high surface temperature after drying, and the remaining absorbent resin precursor A3 is classified using the classifier 6, the deviations in pressure absorption capacity and absorption rate of the classified absorbent resin particles P1 become smaller. Based on the above, it can be said that by removing the absorbent resin precursor B2 from the path connecting the dryer 3 and the classifier 6, absorbent resin particles P1 with further suppressed deviations in pressure absorption capacity and absorption rate can be obtained.

[0058] [Third Channel Component] The third channel component L3 is a component connected to the second outlet 44 and the upper opening formed on the upper part of the cooler 5. The third channel component L3 defines a channel for conveying the absorbent resin precursor A3 discharged from the second outlet 44 to the cooler 5, forming a path connecting the dryer 3 and the classifier 6. The method of conveying the absorbent resin precursor A3 to the cooler 5 is not particularly limited; methods such as gravity conveying, conveying using an inert gas flow, or conveying using a conveyor or other conveying mechanism can be appropriately selected. The method of constructing the third channel component L3 is not particularly limited as long as it is configured to feed the absorbent resin precursor A3 into the upper opening formed on the upper part of the cooler 5 according to the conveying method of the absorbent resin precursor A3. For example, the third channel component L3 can be constructed using piping, a conveying piping in which an inert gas flow is generated, a conveyor, a feeder, etc. A valve controlled by a control device 7 can also be installed on the third channel component L3 to adjust the flow rate of the absorbent resin precursor A2.

[0059] [Cooling machine] Cooler 5 is positioned on the path connecting dryer 3 and classifier 6, and has a cooling chamber (not shown). The hygroscopic resin precursor A3 discharged from the second outlet 44 of classifier 4 flows into the cooling chamber through the upper opening of cooler 5. Cooler 5 cools the hygroscopic resin precursor A3 in the cooling chamber using a cooling device (not shown), removing the heat imparted to the hygroscopic resin precursor A3 by dryer 3. The cooling device is connected to control device 7, and its operation is controlled. The cooled hygroscopic resin precursor A3 is discharged from cooler 5 through a lower opening formed in the lower part of cooler 5, which communicates with the cooling chamber, in order to be conveyed to classifier 6.

[0060] [Fourth Channel Component] The fourth channel component L4 is a component that connects to the lower opening of the cooler 5 and the upper opening formed on the upper part of the classifier 6. The fourth channel component L4 defines a channel for conveying the absorbent resin precursor A3 discharged from the lower opening of the cooler 5 to the classifier 6, forming a path connecting the dryer 3 and the classifier 6. The method of conveying the cooled absorbent resin precursor A2 to the classifier 6 is not particularly limited; methods such as gravity conveying, conveying using an inert gas flow, or conveying using a conveyor or other conveying mechanism can be appropriately selected. The fourth channel component L4 is not particularly limited in its configuration as long as the absorbent resin precursor A3 is fed into the classifier 6 from the upper opening according to the conveying method of the absorbent resin precursor A3. For example, the fourth channel component L4 can be constructed using piping connected at one end to the lower opening of the cooler 5 and at the other end to the upper opening of the classifier 6, conveying piping that generates an inert gas flow therein, a conveyor, and a feeder. A valve controlled by the control device 7 can also be installed on the fourth channel component L4 to adjust the flow rate of the absorbent resin precursor A3.

[0061] [Grader] The classifier 6 is a device that separates the superabsorbent resin precursor A3 into groups of superabsorbent resin particles having a desired particle size distribution. Examples of classifiers 6 include vibrating screens (unbalanced weight driven, resonant, vibrating motor type, electromagnetic type, circular vibrating type, etc.), in-plane motion screens (horizontal motion type, horizontal circular-linear motion type, three-dimensional circular motion type, etc.), movable mesh screens, forced stirring screens, mesh vibrating screens, air-powered screens, and acoustic screens. The classifier 6 of this embodiment has multiple in-plane motion screens. These multiple in-plane motion screens are arranged in a sequence with larger mesh sizes at the top and smaller mesh sizes at the bottom. Thus, the superabsorbent resin precursor A3, fed to the classifier 6 and fed into the in-plane motion screens, is classified into grades specified by the in-plane motion screens. The superabsorbent resin particles classified into grades that meet the product standards are obtained as superabsorbent resin particles P1.

[0062] <3. Method for manufacturing water-absorbing resin particles> Hereinafter, a method for manufacturing water-absorbing resin particles according to an embodiment of the present invention will be described with reference to the accompanying drawings. Figure 7 This is a flowchart illustrating the various processes performed during the manufacture of absorbent resin particles using manufacturing apparatus 100. Each process (step) S1 to S7 is mainly controlled by control device 7.

[0063] In step S1, polymerization is carried out in polymerizer 1. The polymerization tank of polymerizer 1 contains monomers and liquid components (hydrocarbon dispersion medium) that form the raw materials for the hydrophilic resin particles. By stirring and heating them in the polymerization tank, the monomers undergo a polymerization reaction to produce a slurry containing a hydrogel-like polymer. The produced slurry is then sent to concentrator 2.

[0064] In step S2, the concentrator 2 performs concentration. The slurry from the polymerizer 1 is contained in the concentration tank of the concentrator 2. The slurry is concentrated by stirring and heating in the concentration tank. As a result, a concentrate containing a hydrogel-like polymer, namely, a water-absorbing resin composition A1, is obtained. The water-absorbing resin composition A1 is then sent to the dryer 3.

[0065] In step S3, the dryer 3 performs drying. The water-absorbing resin composition A1 from the concentrator 2 is contained in the drying chamber of the dryer 3. The water-absorbing resin composition A1 is dried in the drying chamber to remove moisture, becoming a water-absorbing resin precursor A2. Step S3 is an example of the "step of drying the water-absorbing resin composition to obtain a water-absorbing resin precursor" of the present invention. The obtained water-absorbing resin precursor A2 is conveyed to the first channel member L1 connected to the sorter 4.

[0066] In step S4, the powder lumps B1 are captured by the collecting element 30 disposed on the first channel member L1 and removed from the first channel member L1. The remaining water-absorbing resin precursor A2 is sent to the sorting machine 4 at a surface temperature of 50°C to 100°C.

[0067] In step S5, the sorting machine 4 separates the water-absorbing resin precursor A2 into water-absorbing resin precursor B2 and water-absorbing resin precursor A3. Water-absorbing resin precursor B2 is removed because it is water-absorbing resin precursor A2 with a moisture content of 20% or more. The remaining water-absorbing resin precursor A3 is sent to the cooling machine 5. Step S5 is an example of the step of "sorting and removing water-absorbing resin precursors with a moisture content of 20% or more from water-absorbing resin precursors" according to the present invention.

[0068] In step S6, the cooler 5 performs cooling. The water-absorbing resin precursor A3 from the sorter 4 is contained in the cooling chamber of the cooler 5 and cooled to remove the heat imparted by the dryer 3. The cooled water-absorbing resin precursor A3 is then sent to the classifier 6.

[0069] In step S7, the classifier 6 classifies the absorbent resin precursor A3. Thus, the classification is completed, yielding absorbent resin particles P1 that meet the standards for the product. Step S7 is an example of the "step of classifying the remaining absorbent resin precursor to obtain classified absorbent resin particles" of the present invention. Furthermore, the absorbent resin particles P1 also include absorbent resin particles for which additives have been added as needed after classification based on the classifier 6.

[0070] <4. Characteristics> According to the manufacturing apparatus 100 and the method for manufacturing water-absorbing resin particles using the manufacturing apparatus 100 described in the above embodiments, the water-absorbing resin precursor A2 is sorted by a sorting machine 4 disposed in the path connecting the dryer 3 and the classifier 6. This allows the water-absorbing resin precursor A2, which has a high moisture content of 20% or more even after drying, to be sorted into water-absorbing resin precursor B2 and removed from the manufacturing apparatus 100. Furthermore, by classifying the water-absorbing resin precursor A3 after the removal of the water-absorbing resin precursor B2 using the classifier 6, deviations in the quality of the obtained water-absorbing resin particles P1, such as their pressure absorption capacity and absorption rate corresponding to their size, can be suppressed.

[0071] <5. Variations> The present invention has been described above as one embodiment, but the present invention is not limited to the above embodiment. Various modifications can be made without departing from its spirit. For example, the following modifications can be made. (1) Alternatively, the trapping element 30 and step S4 can be omitted. That is, the first channel component L1 can be constructed without setting the trapping element 30. (2) The cooler 5 and step S6 can also be omitted. That is, the manufacturing apparatus 100 may not have the cooler 5, or it may be configured such that the sorter 4 and the classifier 6 are directly connected. (3) The opening of the sorting member 42 can also be slit-shaped. In this case, the average value of the slit spacing corresponds to the size of the opening of the sorting member 42. (4) The relay component 32 and the second channel component L2 can also be omitted. That is, the first channel component L1 can also be configured to serve as the second channel component L2, and the other end of the first channel component L1 is connected to the input port 40 of the sorting machine 4. Example

[0076] The following describes embodiments of the present invention, but the present invention is not limited to the following embodiments.

[0077] <Experiment 1> A manufacturing apparatus identical to the manufacturing apparatus 100 described in the above embodiment was prepared, and water-absorbing resin particles were manufactured using this apparatus by the manufacturing method described in the above embodiment. Then, the moisture content of the water-absorbing resin precursor separated for removal from the manufacturing apparatus 100 and the water-absorbing resin precursor fed to the classifier were measured using the method described later. The detailed manufacturing method of the water-absorbing resin particles will be described below.

[0078] [1. Preparation of the first-stage monomer aqueous solution] In a container for preparing the first-stage monomer, 28.8 parts by mass of an 80% acrylic acid aqueous solution (as a water-soluble olefinic unsaturated monomer) were added. While cooling, 31.9 parts by mass of a 30% sodium hydroxide aqueous solution (as an alkaline neutralizing agent) were added dropwise to neutralize the monomer to a degree of neutralization of 76 mol% of the acid groups in the water-soluble olefinic unsaturated monomer. Next, 1.15 parts by mass of a 2% potassium persulfate aqueous solution (as a free radical polymerization initiator), 0.14 parts by mass of a 3% ethylene glycol diglycidyl ether aqueous solution (as a crosslinking agent), and 11.0 parts by mass of water were added and dissolved to prepare the first-stage monomer aqueous solution, maintained at a temperature of 20°C–21°C.

[0079] [2. Feeding to the polymerizer and adding additives] In the polymerizer, 90.0 parts by mass of n-heptane were added as the hydrocarbon dispersion medium, and 2.02 parts by mass of a 10% by mass n-heptane solution of maleic anhydride-ethylene-propylene copolymer were added as a dispersion stabilizer. These were stirred using the agitator provided with the polymerizer. Next, the total amount of the first-stage monomer aqueous solution was added to the polymerizer. Then, while heating the contents of the polymerizer, 2.02 parts by mass of a 10% by mass n-heptane solution of sucrose fatty acid ester was added to the polymerizer. Nitrogen gas was then purged into the polymerizer body to purge the polymer.

[0080] [3. First-order polymerization reaction] Next, the contents of the polymerizer are heated to 64°C to begin the first stage of polymerization, yielding the first stage reaction mixture.

[0081] [4. Preparation of the second-stage monomer aqueous solution] On the other hand, a second-stage monomer aqueous solution was prepared in another container. Specifically, 41.3 parts by mass of an 80% acrylic acid aqueous solution, acting as a water-soluble olefinic unsaturated monomer, were added to the other container. While cooling, 45.7 parts by mass of a 30% sodium hydroxide aqueous solution, acting as an alkaline neutralizing agent, were added dropwise to neutralize the monomer to a degree of neutralization of 76 mol% of the acid group of the water-soluble olefinic unsaturated monomer. Next, 1.45 parts by mass of a 2% potassium persulfate aqueous solution, acting as a free radical polymerization initiator, 0.12 parts by mass of a 3% ethylene glycol diglycidyl ether aqueous solution, acting as a crosslinking agent, and 1.51 parts by mass of water were added and dissolved to prepare the second-stage monomer aqueous solution.

[0082] [5. Addition of the second-stage monomer aqueous solution] Next, the total amount of the second-stage monomer aqueous solution is added to the polymerizer. Nitrogen gas is then purged into the polymerizer to purge it.

[0083] [6. Second-order polymerization reaction] Next, the contents of the polymerizer are heated to 57°C to begin the second-stage polymerization reaction. After the polymerization reaction is complete, a second-stage reaction mixture (a slurry containing a hydrogel-like polymer) is obtained.

[0084] [7. Concentration Process] The reaction mixture from the second stage is transferred to a concentrator equipped with a stirrer. The reaction mixture from the second stage is stirred while being heated to 80°C–90°C. The n-heptane and water are separated by azeotropic distillation; the n-heptane is returned to the concentrator, and a given amount of water is discharged from the system.

[0085] [8. Drying process] The concentrated water-absorbing resin composition was transferred to a dryer equipped with a stirring device. While stirring the water-absorbing resin composition, the dryer was heated to 80°C–110°C, and n-heptane and water were removed from the system via azeotropic distillation. After removing a given amount of water from the system, 1.4 parts by mass of a 3% aqueous solution of ethylene glycol diglycidyl ether as a post-crosslinking agent was added, followed by further heating and dehydration to obtain the post-crosslinked water-absorbing resin (water-absorbing resin precursor).

[0086] [9. Transfer of water-absorbing resin precursor and adjustment of surface temperature] The absorbent resin precursor discharged from the dryer is transferred to the sorter through piping that serves as the first and second flow path components. At this time, the piping is heated to about 80°C using a heater (surface temperature adjustment device), thereby adjusting the surface temperature of the absorbent resin precursor moving inside the piping to above 60°C.

[0087] Four samples were taken from a portion of the water-absorbing resin precursor passing through the second flow path component. The surface temperature of each sample was measured using a waterproof digital thermometer (SK-1260, manufactured by Sato Measurement Instruments Co., Ltd.), and the results were 63.1℃, 68.2℃, 77.4℃, and 78.2℃, respectively.

[0088] [10. Sorting Process] The absorbent resin precursor transferred from the dryer is treated with a separator (drum screen separator) to remove lumps larger than 10 mm. Specifically, the drum screen separator has Figure 5B The structure shown. A drum screen separator has a housing and a rotating sorting component. The sorting component is equipped with... Figure 2A The sorting member has a square grid shape (1.6 mm wire diameter, 10 mm mesh size, and 74% opening ratio) and is composed of a cylindrical mesh member with an inner diameter of 42 cm and a length of 66 cm. The sorting member is arranged so that the cylindrical axis is approximately parallel to the horizontal plane. The sorting member is configured such that the absorbent resin precursor fed into it through its first opening (the opening closest to the inlet of the sorting machine) moves toward the second opening (the opening closest to the first outlet of the sorting machine). Specifically, a blade member is provided inside the sorting member, and in conjunction with the rotation of the sorting member, the absorbent resin precursor is propelled from the first opening toward the second opening. The absorbent resin precursor fed into the first opening of the sorting member is sorted as it moves toward the second opening. That is, the absorbent resin precursor with smaller particle size moves through the mesh of the sorting member to the second outlet of the sorter, while the absorbent resin precursor with larger particle size (lumps) does not move through the mesh of the sorting member and moves to the first outlet of the sorter.

[0089] [11. Grading process] The absorbent resin precursor, moved to the second outlet of the separator, is transferred to a classifier and classified using a classifier with a mesh size of 298 μm to 805 μm to obtain absorbent resin particles with a median particle size of 380 μm. The method for determining the median particle size is described below. 0.5 parts by mass of silica, as an additive, are mixed with 100 parts by mass of these absorbent resin particles to obtain the final absorbent resin particles.

[0090] Methods for determining moisture content 2.0 g of the water-absorbing resin precursor was accurately weighed (Wb(g)) into a pre-prepared stainless steel petri dish with a constant weight (Wa(g)). The precursor was dried for 2 hours in a hot air dryer (manufactured by ADVANTEC) with an internal temperature set to 105°C, then cooled in the desiccator, and the mass after drying was measured (Wc(g)). The moisture content of the water-absorbing resin precursor was calculated using the following formula. Moisture content (mass%) = [(Wb-Wa)-(Wc-Wa)] / (Wb-Wa)×100

[0091] [Method for determining median particle size] JIS standard sieves were arranged in the following order from top to bottom: 850 μm sieve, 600 μm sieve, 500 μm sieve, 400 μm sieve, 300 μm sieve, 250 μm sieve, 150 μm sieve, and a tray. 100 g of the absorbent resin particles (before adding silica) was added to the top sieve of the assembly, and the mixture was graded by shaking for 10 minutes using a ro-tap shaker. After grading, the percentage of the mass of the absorbent resin particles remaining on each sieve relative to the total mass was calculated, starting with the largest particle size. The relationship between the sieve mesh size and the cumulative percentage of the mass of the absorbent resin particles remaining on the sieve was plotted on logarithmic probability paper. By connecting the plotted points on the probability paper with a straight line, the particle size corresponding to 50% of the cumulative mass percentage was taken as the median particle size (μm) of the absorbent resin particles.

[0092] <Results> In the [10. Sorting Process], a portion of the absorbent resin precursor moving to the first outlet was sampled twice, and the moisture content of each sample was measured. The results were 60.1% by mass and 64.8% by mass, respectively. The moisture content of the absorbent resin precursor moving to the second outlet was also measured similarly, and the result was less than 20% by mass. Therefore, it was confirmed that the absorbent resin precursor with high moisture content was effectively sorted out through the sorting process.

[0093] <Experiment 2> Three samples were taken from each sample: P2 (Example), a final product manufactured using the method described in Experiment 1, and P3 (Comparative Example), a water-absorbing resin particle with a median particle size of 365 μm manufactured using the same method as in Experiment 1, except for omitting the sorting step. For each sample, the pressure absorption capacity and absorption rate, which represent pressure absorption capacity, were measured.

[0094] [Method for determining pressurized water absorption] Figure 8A measuring device 9 for measuring pressurized water absorption. The measuring device 9 includes a burette section 90, a guide tube 91, a measuring stage 92, and a measuring section 93. The burette section 90 includes a burette 900, a first stopcock 902 connected to the lower part of the burette 900, and an air inlet tube 901. The front end of the air inlet tube 901 is connected to a second stopcock 903. The burette section 90 and the measuring stage 92 are connected via the guide tube 91. A through hole communicating with the guide tube 91 is formed in the measuring stage 92. The measuring section 93 includes a cylindrical section 930 made of plexiglass, a nylon mesh 931 bonded to the bottom of the cylindrical section 930, and a counterweight 932.

[0095] The inner diameter of the through hole in the measuring stage is 2 mm, and the inner diameter of the cylindrical part 930 is 20 mm. The nylon mesh 931 used in the experiment has a mesh size of 57 μm (255 mesh). Additionally, the counterweight 932 has a diameter of 19 mm and a mass of 60 g. The counterweight 932 is placed on the samples of absorbent resin particles P2 or P3, applying a load of 0.3 PSI to the absorbent resin particles P2 and P3.

[0096] The determination was conducted indoors at 25°C. First, the first stopcock 902 and the second stopcock 903 were closed, and 0.9% saline solution, adjusted to 25°C, was injected into the burette 900 through the upper opening. Then, the upper opening of the burette 900 was sealed with a rubber stopper. Next, the first stopcock 902 and the second stopcock 903 were opened, and the height of the measuring stage 92 was adjusted so that the level of the 0.9% saline solution in the through-hole of the measuring stage 92 was the same as the level of the upper surface of the measuring stage 92.

[0097] In addition, a measuring unit 93 is prepared for each sample of absorbent resin particles P2 and P3 and placed on the measuring stage 92. Specifically, 0.1000±0.0002g of absorbent resin particles P2 or P3 are evenly distributed on a nylon mesh 931, and the measuring unit 93, with a counterweight 932 placed on it, is placed on the measuring stage 92. The measuring unit 93 is aligned such that the cylindrical shaft of the cylindrical portion 930 passes through the through hole of the measuring stage 92.

[0098] The amount of 0.9% saline solution W (ml) that decreases from the burette 900 represents the amount of 0.9% saline solution absorbed by the absorbent resin particles P2 or P3. Read W (ml) and calculate the pressurized water absorption capacity AUL (ml / g) of absorbent resin particles P2 or P3 60 minutes after they begin absorbing water, according to the following formula. AUL = W / 0.1000

[0099] [Methods for determining water absorption rate] Measure 50±0.1g of physiological saline solution, adjusted to a temperature of 25±0.2℃, into a 100mL beaker in a constant temperature water bath. Then, use a magnetic stirrer ( The acyclic (non-cyclic) solution was stirred at 600 rpm (conventional Vortex method) to generate vortices. 2.0 ± 0.002 g of absorbent resin particles P2 and P3 were added to physiological saline in a single batch. The time [in seconds] from the addition of absorbent resin particles P2 and P3 until the vortex on the liquid surface converged was measured, and this time was taken as the water absorption rate of absorbent resin particles P2 and P3. Furthermore, the water absorption rate is a parameter affected by the particle size of the absorbent resin particles (generally, the larger the particle size, the slower the water absorption rate). Therefore, for convenience, the water absorption rate of absorbent resin particles P2 and P3 was evaluated by dividing the water absorption rate (V (seconds)) by their respective median particle size (MPS (μm)) to obtain the value V / MPS. The method for determining the median particle size is as described in Example 1.

[0100] <Results> The determination results of the water-absorbing resin particles P2 and P3 in the three sample portions are shown below. Figure 9A and 9B The chart. Figure 9A This is a graph of pressurized water absorption capacity (AUL) (ml / g). (Source: [Insert Source Here]) Figure 9A It can be seen that, in the superabsorbent resin particles P2 involved in the examples, the deviation in pressure absorbent capacity (AUL) is smaller compared to the superabsorbent resin particles P3 involved in the comparative examples. Furthermore, the overall value of pressure absorbent capacity (AUL) is higher in the superabsorbent resin particles P2 involved in the examples. Specifically, the average value of pressure absorbent capacity (AUL) for the three sample portions of superabsorbent resin particles P2 is 34.7, while the average value of pressure absorbent capacity (AUL) for the three sample portions of superabsorbent resin particles P3 is 32. That is, it is confirmed that the pressure absorbent capacity (AUL) of the superabsorbent resin particles P2 involved in the examples is increased by 2.7 (ml / g) compared to the superabsorbent resin particles P3 involved in the comparative examples.

[0101] in addition, Figure 9B This is a graph of the water absorption rate evaluation index V / MPS. (Source: [Insert graph here]) Figure 9B It can be seen that, in the water-absorbing resin particles P2 involved in the examples, the deviation of the water absorption rate evaluation index V / MPS is smaller compared with that of the water-absorbing resin particles P3 in the comparative examples. Specifically, the variance of the water absorption rate evaluation index V / MPS for the three sample portions of water-absorbing resin particles P2 is 0.0003, while the variance of the water absorption rate evaluation index V / MPS for the three sample portions of water-absorbing resin particles P3 is 0.004. This confirms that the deviation of the water-absorbing resin particles P2 in the examples is reduced compared with that of the water-absorbing resin particles P3 in the comparative examples. Symbol Explanation

[0102] 1: Aggregator 2: Concentrator 3: Dryer 4: Sorting machine 5: Cooling machine 6: Classifier 40: Input port 41: Inject into the mouth 42: Sorting components 42a: Mesh component 42b: Plate-like member 100: Manufacturing equipment A1: Water-absorbing resin composition A2: Precursor to water-absorbing resin A3: Precursor to water-absorbing resin.

Claims

1. An apparatus for manufacturing water-absorbing resin particles, comprising: A dryer that dries a water-absorbing resin composition to obtain a water-absorbing resin precursor; A classifier that classifies the absorbent resin precursor to obtain absorbent resin particles; and The sorting machine is positioned on the path connecting the dryer and the classifier. The sorting mechanism is used to sort the absorbent resin precursor with a surface temperature of 50°C to 100°C and exceeding a given size into absorbent resin precursors with a water content of 20% or more.

2. The apparatus for manufacturing water-absorbing resin particles according to claim 1, wherein, The sorting machine includes: An inlet, the inlet being formed for feeding the absorbent resin precursor discharged from the dryer; and A sorting component, which is connected to the inlet and has an opening of the given size, The sorting mechanism is configured to transport the absorbent resin precursor, which has passed through the inlet, to a path connected to the classifier.

3. The apparatus for manufacturing water-absorbing resin particles according to claim 2, wherein, The sorting member is composed of a mesh member having a plurality of openings of the given size.

4. The apparatus for manufacturing water-absorbing resin particles according to claim 2 or 3, wherein, The sorting component is configured to impart motion to the absorbent resin precursor fed into the inlet.

5. The apparatus for manufacturing water-absorbing resin particles according to any one of claims 1 to 3, wherein, The given dimensions are 7mm to 15mm.

6. The apparatus for manufacturing water-absorbing resin particles according to any one of claims 1 to 3, wherein, The manufacturing apparatus also includes a cooler disposed on the path connecting the sorter and the classifier. The cooling mechanism is used to cool the water-absorbing resin precursor as it is conveyed from the sorter to the path connected to the classifier.

7. A method for manufacturing water-absorbing resin particles, comprising the following steps: The step of drying the water-absorbing resin composition to obtain the water-absorbing resin precursor; The steps include: sorting the absorbent resin precursors with a surface temperature of 50°C to 100°C and exceeding a given size from the absorbent resin precursors into absorbent resin precursors with a water content of 20% or more and removing them; and... The step of classifying the remaining absorbent resin precursor to obtain classified absorbent resin particles.

Citation Information

Patent Citations

  • Process for preparing water-absorbing polymer particles

    CN101305253A

  • Production of water-absorbing resin

    JP1999292919A