Method for producing 5005-h14 aluminum alloy sheet and strip for anodizing

By optimizing the chemical composition and process parameters of 5005-H14 aluminum alloy sheet and strip, the problems of high surface roughness and insufficient transparency during the anodizing process were solved, achieving high-quality anodizing effect and improving production efficiency.

CN117127069BActive Publication Date: 2026-11-24GUANGXI LIUZHOU YINHAI ALUMINUM IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311113968.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-31
Publication Date
2026-11-24
Estimated Expiration
2043-08-31

AI Technical Summary

Technical Problem

In the existing technology, 5005 alloy aluminum alloy sheets have problems such as high surface roughness, insufficient transparency and poor surface quality during the anodizing process, especially in products with a thickness of 2.0 to 3.0 mm, where the color is uneven and the film layer is opaque after anodizing.

Method used

By optimizing the chemical composition of 5005-H14 aluminum alloy sheet and strip, especially controlling the Si and Fe contents to economically feasible levels (Si≤0.08%, Fe≤0.25%), and combining this with reasonable hot rolling and cold rolling process parameters, such as emulsion concentration, roll roughness, and pass rate, a low-roughness surface is formed, ensuring the transparency and uniformity of the anodized film.

Benefits of technology

The surface roughness Ra of aluminum alloy sheet and strip was reduced to Ra≤0.3μm. After anodizing, the surface was bright, transparent, uniform and delicate, which improved the transparency and surface quality of the anodized film. At the same time, the production process was shortened and the production cost was reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004424543640000041
    Figure BDA0004424543640000041
  • Figure BDA0004424543640000051
    Figure BDA0004424543640000051
  • Figure BDA0004424543640000052
    Figure BDA0004424543640000052
Patent Text Reader

Abstract

This invention belongs to the field of aluminum alloy manufacturing, and specifically relates to a method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, comprising the following steps: melting and casting → sawing → milling → heating → hot rolling → cold rolling → cleaning → finished product leveling; the mass percentage of the aluminum alloy composition is: Si≤0.08%, Fe≤0.25%, Cu≤0.15%, Mn≤0.15%, Mg0.60~1.00%, Cr≤0.08%, Zn≤0.15%, Ti0.01~0.05%, other impurity elements individually ≤0.05%, other impurity elements total ≤0.15%, and the remainder is Al. In the hot rolling step, the hot finishing roll roughness Ra is 0.8~0.9μm, and the emulsion concentration is 7.0~8.0%; in the cold rolling step, the material is cold rolled twice to the finished thickness, with a total processing rate of 40~50%, and the roll roughness Ra is 0.2~0.3μm. The 5005-H14 aluminum alloy sheet and strip prepared by this invention has a thickness of 1.0-4.0 mm, a delicate surface, and a uniform color. After anodizing, the surface has a bright, uniform, and delicate color, which improves the surface quality of the aluminum alloy sheet and strip after anodizing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy manufacturing, and specifically relates to a method for producing 5005-H14 aluminum alloy sheet and strip for anodizing. Background Technology

[0002] Anodizing refers to the electrochemical oxidation of metals or alloys. Taking aluminum and aluminum alloy products (hereinafter referred to as aluminum products) as an example, the aluminum product is placed in a suitable electrolyte as the anode. Under specific conditions and the action of an applied current, a thin film of aluminum oxide forms on the surface of the aluminum product. This aluminum oxide film improves the surface hardness and wear resistance of the aluminum product, enhances its corrosion resistance, and, moreover, utilizes the adsorption capacity of the numerous micropores in the oxide film to color the surface of the aluminum product with various beautiful and vibrant colors, enriching the color expression of the aluminum product and increasing its aesthetic appeal. Anodizing is widely used in aluminum alloys. Aluminum alloys have low hardness and poor wear resistance, and are prone to corrosion and breakage. In industry, anodizing is increasingly widely used to form a thick and dense oxide film layer on the aluminum surface to significantly improve the corrosion resistance, hardness, wear resistance, and decorative properties of aluminum alloys. In existing anodizing technologies, 5-series and 6-series aluminum alloys are generally used for anodizing to protect the aluminum surface. However, 5005 alloy, due to its high strength and lustrous color after anodizing, represents the future trend for anodized aluminum panels and strips for curtain walls. As the market demands increasingly higher levels of color from anodized aluminum panels and strips, higher requirements are being placed on surface roughness and color uniformity after anodizing.

[0003] Patent CN107805746B discloses a 5005H34 aluminum alloy sheet and its production method. It mainly produces 5005H34 sheet products with a thickness of 2.0–3.0 mm by hot rolling followed by a single cold rolling cycle combined with low-temperature baking (130±10℃) during aluminum coil cleaning. This method ensures product performance and shortens the production process. However, due to the limitation of the thinnest hot-rolled thickness, it is only suitable for products with a finished thickness of 2.0–3.0 mm, and the shortened production process only ensures mechanical properties. It also suffers from problems such as obvious rolling marks on the surface after anodizing, batch-to-batch differences in the color of the anodized film, and a darker anodized film.

[0004] Patent CN106906390B discloses aluminum alloy anodizing and its production method. By limiting and optimizing the chemical composition of aluminum alloy anodized plates on the basis of standards, the defects of "black streaks" and "aluminum plating" in aluminum alloys are reduced to the point of being inconspicuous. Although the surface quality and surface roughness of aluminum alloys are greatly improved, the transparency of aluminum alloy anodized plates is insufficient, and their surface quality has not yet reached the ideal requirements. Summary of the Invention

[0005] The purpose of this invention is to provide a method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, overcoming the defects of high surface roughness of aluminum alloy, insufficient transparency of aluminum alloy anodized sheet, and low surface quality.

[0006] To achieve the above objectives, the present invention provides a method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, characterized in that the method includes the following steps: melting and casting → sawing → milling → heating → hot rolling → cold rolling → cleaning → finished product leveling;

[0007] In the casting step, the mass percentage of the chemical composition of 5005 aluminum alloy is as follows: Si≤0.08%, Fe≤0.25%, Cu≤0.15%, Mn≤0.15%, Mg0.60~1.00%, Cr≤0.08%, Zn≤0.15%, Ti0.01~0.05%, other impurity elements individually ≤0.05%, and the total of other impurity elements ≤0.15%, with the remainder being Al. The anodizing effect of aluminum alloy sheet and strip is affected by the chemical composition of the aluminum alloy sheet and strip. Different chemical composition ratios of aluminum alloy will lead to different anodizing characteristics of aluminum alloy sheet and strip, mainly manifested through the different chemical behaviors of intermetallic compounds during anodizing. Surface transparency and uniformity are basic conditions for colorless and transparent anodized films. Among the impurity elements in the chemical composition of 5005 aluminum alloy, other impurity elements have little impact on the anodizing of aluminum alloy sheet and strip, while Si and Fe impurity elements are the main influencing factors. The Si and Fe impurities react with Al to form AlFeSi intermetallic compounds, which can reduce the transparency of the anodic oxide film and even make the film turn gray. Therefore, keeping the Si and Fe content at an economically feasible level (Si≤0.08%, Fe≤0.25%) is beneficial to the transparency of the anodic oxide film of aluminum alloy sheets and strips.

[0008] In the hot rolling step, the roughness Ra of the hot finishing roll is 0.8 to 0.9 μm, and the emulsion is added by spraying during hot rolling, with the concentration of the emulsion being 7.0 to 8.0%.

[0009] In the cold rolling step, the product is cold rolled twice to the finished thickness, with a total processing rate of 40-50%, and the roll roughness is controlled at Ra0.2-0.3μm.

[0010] The anodizing effect of aluminum alloy sheet and strip is affected by the rolling process parameters. The emulsion index, roll parameters, roll parameters and pass rate in the hot rolling process all have a significant impact on the surface quality of the product. This invention controls the emulsion concentration to 7.0-8.0% during the hot rolling process, which can save costs without affecting the lubrication ability of the emulsion during the hot rolling process. The hot rolling roll roughness Ra is 0.8-0.9μm, and the cold rolling roll roughness Ra is 0.2-0.3μm with a pass rate of more than 40-50%, which is conducive to forming aluminum alloy sheet and strip with a low surface roughness, thereby obtaining a highly uniform anodized film.

[0011] Furthermore, in the above-mentioned method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, in the heating step, the ingot heating temperature is 480-510℃, and the holding time is 2-8 hours.

[0012] Furthermore, in the above-mentioned method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, in the hot rolling step, the hot roughing rolling temperature is controlled at 400-460℃, and the hot finishing rolling temperature is 325-345℃; even further, the thickness of the hot-rolled coil is such that 40-50% of the cold rolling processing rate is reserved on the basis of the finished product thickness.

[0013] Furthermore, in the above-mentioned production method of 5005-H14 aluminum alloy sheet and strip for anodizing, in the cleaning step, the rolling oil and aluminum powder on the surface of the aluminum strip are cleaned by water washing or alkaline washing, and the surface is wiped with a dry paper towel to remove aluminum dust; even further, the alkaline washing method uses sodium hydroxide solution for cleaning.

[0014] Furthermore, in the above-mentioned method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, in the finished product leveling step, the aluminum coil is leveled using a stretch straightening machine or the aluminum coil is leveled using a cross-cutting machine and then cut into sheets, and the plastic deformation rate of the aluminum sheet and strip is 0.3 to 0.5%.

[0015] Another object of the present invention is to provide 5005-H14 aluminum alloy sheet and strip prepared by the above-described production method.

[0016] Compared with existing technologies, the present invention has the following advantages:

[0017] 1. The 5005-H14 aluminum alloy sheet and strip produced by this invention, through optimization of impurity element and main element content, and reasonable matching of temperature parameters, hot rolling emulsion index and roll parameters, cold rolling roll parameters and pass processing rate, yields a finished 5005-H14 aluminum alloy sheet and strip with a thickness of 1-4 mm, a surface roughness Ra≤0.3 μm, and a bright, transparent, uniform and delicate surface color after anodizing, exhibiting excellent anodized color, improving the transparency of the anodized film, and thus improving the surface quality of the anodized aluminum alloy sheet and strip.

[0018] 2. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing provided by the present invention can reduce annealing and other processes compared with conventional processes, significantly shorten the production process, save production time, greatly reduce production costs, and improve production efficiency. Detailed Implementation

[0019] The specific embodiments of the present invention will be described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments.

[0020] The emulsions used in the following examples and comparative examples were 95% emulsions purchased from Shenzhen Kewode Technology Co., Ltd., and then diluted with water to 7.0-8.0%.

[0021] Example 1

[0022] This embodiment provides a method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, including the following production process: casting → sawing → milling → heating → hot rolling → cold rolling → cleaning → finished product leveling.

[0023] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 1. The following raw materials are melted and cast to obtain ingots.

[0024] Table 1 shows the mass percentage of the 5005-H14 aluminum alloy composition in this embodiment.

[0025]

[0026] (2) Heating: After the ingot is sawed and milled, it is heated to 505°C and then kept at that temperature for 3 hours.

[0027] (3) Hot rolling: The aluminum alloy ingot that has undergone heating treatment in step (2) is hot rolled to obtain a hot rolled billet with a thickness of 5.0 mm. During the hot rolling process, an emulsion is sprayed, wherein the hot finishing emulsion concentration is 7.8%, the hot roughing finishing temperature is 404℃, the hot finishing roll roughness Ra is 0.81 μm, and the hot finishing finishing temperature is 328℃.

[0028] (4) Cold rolling: The hot-rolled billet is rolled to 3.0 mm through two cold rolling passes, with a total processing rate of 40%. The roll roughness Ra during cold rolling is 0.28 μm, and aluminum coil is obtained.

[0029] (5) Cleaning: After cleaning the surface of the aluminum coil obtained in step (4) with water to remove the rolling oil and aluminum powder, wipe the surface with a dry paper towel to remove any aluminum dust.

[0030] (6) Finished product leveling: The aluminum coil is leveled using a bending straightening machine or the aluminum coil is leveled using a cross-cutting machine and then cut into sheets. The plastic deformation rate of the aluminum sheet and strip is 0.4%.

[0031] Example 2

[0032] The difference between this embodiment and Embodiment 1 lies in the following steps; the remaining steps are the same as in Embodiment 1.

[0033] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 2.

[0034] Table 2 shows the mass percentage of the 5005-H14 aluminum alloy composition in this embodiment.

[0035]

[0036] (2) Heating: The ingot is heated to 480℃ and then kept at that temperature for 8 hours.

[0037] (3) Hot rolling: The hot roughing rolling final rolling temperature is 430℃, the hot finishing rolling emulsion concentration is 7.5%, the hot finishing rolling roll roughness Ra is 0.88μm, the hot finishing rolling final rolling temperature is 335℃, and the hot rolled billet thickness is 2.4mm.

[0038] (4) Cold rolling: The hot-rolled billet is rolled to 1.2mm through two cold rolling passes, with a total processing rate of 50%. The roll roughness Ra during cold rolling is 0.25μm.

[0039] Example 3

[0040] The difference between this embodiment and Embodiment 1 lies in the following steps; the remaining steps are the same as in Embodiment 1.

[0041] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 3.

[0042] Table 3 shows the mass percentage of the 5005-H14 aluminum alloy composition in this embodiment.

[0043]

[0044] (2) Heating: The ingot is heated to 496℃ and then kept at that temperature for 6 hours.

[0045] (3) Hot rolling: The hot roughing rolling final rolling temperature is 457℃, the hot finishing rolling emulsion concentration is 7.0%, the hot finishing rolling roll roughness Ra is 0.84μm, the hot finishing rolling final rolling temperature is 340℃, and the hot rolled billet thickness is 3.6mm.

[0046] (4) Cold rolling: The hot-rolled billet is rolled to 2.0 mm through two cold rolling passes, with a total processing rate of 44%. The roll roughness Ra during cold rolling is 0.2 μm.

[0047] (5) Cleaning: After cleaning the surface of the aluminum coil with sodium hydroxide solution to remove rolling oil and aluminum powder, wipe the surface with a dry paper towel to remove aluminum dust.

[0048] (6) Finished product leveling: The plastic deformation rate of aluminum sheet and strip is 0.3%.

[0049] Example 4

[0050] The difference between this embodiment and Embodiment 1 lies in the following steps; the remaining steps are the same as in Embodiment 1.

[0051] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 4.

[0052] Table 4 shows the mass percentage of the 5005-H14 aluminum alloy composition in this embodiment.

[0053]

[0054] (2) Heating: The ingot is heated to 480℃ and then kept at that temperature for 8 hours.

[0055] (3) Hot rolling: The hot roughing rolling final rolling temperature is 400℃, the hot finishing rolling emulsion concentration is 7.0%, the hot finishing rolling roll roughness Ra is 0.81μm, the hot finishing rolling final rolling temperature is 325℃, and the hot rolled billet thickness is 5.0mm.

[0056] (4) Cold rolling: The hot-rolled billet is rolled to 3.0 mm through two cold rolling passes, with a total processing rate of 40%. The roll roughness Ra is 0.2 μm during cold rolling.

[0057] Example 5

[0058] The difference between this embodiment and Embodiment 1 lies in the following steps; the remaining steps are the same as in Embodiment 1.

[0059] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 5.

[0060] Table 5 shows the mass percentage of the 5005-H14 aluminum alloy composition in this embodiment.

[0061]

[0062] (2) Heating: Heat the ingot to 510℃ and then keep it at that temperature for 2 hours.

[0063] (3) Hot rolling: The hot roughing rolling final rolling temperature is 460℃, the hot finishing rolling emulsion concentration is 8.0%, the hot finishing rolling roll roughness Ra is 0.9μm, the hot finishing rolling final rolling temperature is 345℃, and the hot rolled billet thickness is 5.0mm.

[0064] (4) Cold rolling: The hot-rolled billet is rolled to 2.5mm through two cold rolling passes, with a total processing rate of 50%. The roll roughness Ra is 0.3μm during cold rolling.

[0065] Comparative Example 1

[0066] The difference between this comparative example and Example 1 is that the content of Si and Fe in the aluminum alloy composition is different, but the rest of the steps are the same as in Example 1.

[0067] The mass percentage of the 5005-H14 aluminum alloy composition in this comparative example is shown in Table 6.

[0068] Table 6 shows the mass percentage of the 5005-H14 aluminum alloy composition in this comparative example.

[0069]

[0070] Comparative Example 2

[0071] The difference between this comparative example and Example 1 is the hot rolling parameters; the remaining steps are the same as in Example 1.

[0072] In this comparative example, the hot finishing emulsion concentration is 6.0% and the hot finishing roll roughness Ra is 1.1 μm.

[0073] Comparative Example 3

[0074] The difference between this comparative example and Example 1 is the cold rolling parameters; the remaining steps are the same as in Example 1.

[0075] In this comparative example, the total processing rate in the cold rolling parameters is 60%, and the roll roughness Ra during cold rolling is 0.45μm.

[0076] Comparative Example 4

[0077] The difference between this comparative example and Example 1 lies in the following steps; the remaining steps are the same as in Example 1.

[0078] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 7.

[0079] Table 7 shows the mass percentage of the 5005-H14 aluminum alloy composition in this comparative example.

[0080]

[0081] (2) Heating: The ingot is heated to 498°C and then kept at that temperature for 3 hours.

[0082] (3) Hot rolling: The hot roughing rolling final rolling temperature is 448℃, the hot finishing rolling emulsion concentration is 6.5%, the hot finishing rolling roll roughness Ra is 1.0μm, the hot finishing rolling final rolling temperature is 335℃, and the hot rolled billet thickness is 6.0mm.

[0083] (4) Cold rolling: The hot-rolled billet is rolled to 3.0 mm through two cold rolling passes, with a total processing rate of 50%. The roll roughness Ra during cold rolling is 0.4 μm.

[0084] (5) Cleaning: After cleaning the surface of the aluminum coil with sodium hydroxide solution to remove rolling oil and aluminum powder, wipe the surface with a dry paper towel to remove aluminum dust.

[0085] (6) Finished product leveling: The plastic deformation rate of aluminum sheet and strip is 0.2%.

[0086] Comparative Example 5

[0087] The difference between this comparative example and Example 1 lies in the following steps; the remaining steps are the same as in Example 1.

[0088] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 8.

[0089] Table 8 shows the mass percentage of the 5005-H14 aluminum alloy composition in this comparative example.

[0090]

[0091] (2) Heating: Heat the ingot to 506℃ and then keep it at that temperature for 5 hours.

[0092] (3) Hot rolling: The hot roughing rolling final rolling temperature is 415℃, the hot finishing rolling emulsion concentration is 6.6%, the hot finishing rolling roll roughness Ra is 0.75μm, the hot finishing rolling final rolling temperature is 328℃, and the hot rolled billet thickness is 4.0mm.

[0093] (4) Cold rolling: The hot-rolled billet is rolled to 3.0 mm through one pass of cold rolling, with a total processing rate of 25%. The roll roughness Ra during cold rolling is 0.36 μm.

[0094] (5) Cleaning: Use alkaline washing to clean the rolling oil and aluminum powder from the surface of the aluminum coil. After cleaning, wipe the surface with a dry paper towel to remove any aluminum dust.

[0095] Comparative Example 6

[0096] The difference between this comparative example and Example 1 lies in the following steps; the remaining steps are the same as in Example 1.

[0097] (1) Melting and casting: The mass percentage of the 5005-H14 aluminum alloy composition is shown in Table 9.

[0098] Table 9 shows the mass percentage of the 5005-H14 aluminum alloy composition in this comparative example.

[0099]

[0100] (2) Heating: The ingot is heated to 498°C and then kept at that temperature for 7 hours.

[0101] (3) Hot rolling: The hot roughing rolling final rolling temperature is 416℃, the hot finishing rolling emulsion concentration is 9%, the hot finishing rolling roll roughness Ra is 1.0μm, the hot finishing rolling final rolling temperature is 332℃, and the hot rolled billet thickness is 2.0mm.

[0102] (4) Cold rolling: The hot-rolled billet is rolled to 1.98 mm through two cold rolling passes, with a total processing rate of 50.5%. The roll roughness Ra during cold rolling is 0.35 μm.

[0103] (5) Cleaning: Use alkaline washing to clean the rolling oil and aluminum powder from the surface of the aluminum coil. After cleaning, wipe the surface with a dry paper towel to remove any aluminum dust.

[0104] Table 10 shows a comparison of the anodized surface quality of Example 1 and Comparative Examples 1-3.

[0105] Table 10 shows the comparison of anodic oxidation surface quality between Example 1 and Comparative Examples 1-3.

[0106] Group Anodized film Roughness Ra (μm) Example 1 transparent 0.285 Comparative Example 1 Dark 0.294 Comparative Example 2 There are dark stripes 0.482 Comparative Example 3 There are dark stripes 0.491

[0107] As shown in the table above, compared with Example 1, the amount of Si and Fe added in Comparative Example 1 is higher. Although the roughness is still ≤0.3μm, the surface of its anodic oxide film is dark, indicating that reducing the content of Si and Fe elements can improve the surface quality of the finished anodic oxide film. In Comparative Example 2, the hot finishing emulsion concentration is low and the lubrication is insufficient, resulting in high roughness of the hot finishing rolls. In Comparative Example 3, the total cold rolling processing power is low, while the roll roughness is high during cold rolling. The surface roughness of the aluminum alloy sheet and strip obtained in Comparative Examples 1-3 is >0.48, and the anodic oxide surface quality also has dark stripes. This indicates that reducing the emulsion concentration and the total cold rolling processing rate or increasing the hot and cold rolling roughness are not conducive to forming aluminum alloy sheet and strip with low roughness surface.

[0108] The mechanical properties and anodized surface quality of the finished products of Examples 1-5 and Comparative Examples 1-3 are shown in Table 11.

[0109] Table 11 shows the mechanical properties and anodized surface quality of Examples 1-5 and Comparative Examples 1-3.

[0110]

[0111] As shown in the table above, the tensile strength, yield strength, elongation, and other mechanical properties of the finished products in Examples 1-5 and Comparative Examples 4-6 do not change significantly. However, when the addition of Si and Fe, the main factors affecting the anodic oxide film, exceeds a certain range (Si>0.08%, Fe>0.25%), and the emulsion index, roll parameters, roll parameters, and pass processing rate in the hot rolling process are changed, as shown in Comparative Example 4-6, the finished anodic oxide film becomes dark with a roughness Ra>0.3μm. In contrast, Examples 1-5, through optimization of the content of other impurity elements and main elements, and reasonable matching of temperature parameters, hot rolling emulsion index and roll parameters, cold rolling roll parameters, and pass processing rate, achieve a finished product roughness Ra≤0.3μm. The anodic oxide film is transparent, bright, uniform, and delicate, with better anodic oxidation aesthetics. It improves the transparency and surface quality of the anodic oxide film of aluminum alloy sheet and strip without affecting the mechanical properties of the finished product.

[0112] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A method for producing 5005-H14 aluminum alloy sheet and strip for anodizing, characterized in that, The process includes the following steps: melting and casting → sawing → milling → heating → hot rolling → cold rolling → cleaning → finished product leveling; In the casting step, the mass percentage of the chemical composition of the 5005 aluminum alloy is as follows: Si≤0.08%, Fe≤0.25%, Cu≤0.15%, Mn≤0.15%, Mg0.60~1.00%, Cr≤0.08%, Zn≤0.15%, Ti0.01~0.05%, other impurity elements individually ≤0.05%, and the total of other impurity elements ≤0.15%, with the remainder being Al. In the hot rolling step, the surface roughness Ra of the hot finishing rolls is 0.8–0.9 μm, and the emulsion is added by spraying during hot rolling, with a concentration of 7.0–8.0%. In the cold rolling step, the product thickness is achieved through two cold rolling passes, with a total processing rate of 40-50%, and the roll roughness is controlled at Ra0.2-0.3μm. In the finished product leveling step, the plastic deformation rate of the aluminum sheet / strip is 0.3–0.5%.

2. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 1, characterized in that, In the heating step, the ingot heating temperature is 480-510℃, and the holding time is 2-8 hours.

3. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 1, characterized in that, In the hot rolling step, the final rolling temperature of hot roughing is controlled at 400-460℃, and the final rolling temperature of hot finishing is 325-345℃.

4. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 1, characterized in that, In the hot rolling step, the thickness of the hot-rolled coil is such that 40-50% of the cold rolling processing rate is reserved on the basis of the finished product thickness.

5. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 1, characterized in that, The cleaning process involves either water washing or alkaline washing.

6. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 5, characterized in that, The alkaline solution used in the alkaline washing method is a sodium hydroxide solution.

7. The method for producing 5005-H14 aluminum alloy sheet and strip for anodizing according to claim 1, characterized in that, In the finished product leveling step, the aluminum coil is leveled using a stretch bending straightening machine.

8. A 5005-H14 aluminum alloy sheet / strip for anodizing prepared by the production method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Aluminum alloy anodized plate and its production method

    CN106906390B

  • A 5005H34 aluminum alloy sheet and its production method

    CN107805746B

  • 5005H34 aluminum alloy plate and production method thereof

    CN107805746A