A preparation method and application of a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction
By combining rotary evaporation with solid-phase phosphating, the preparation process of ruthenium phosphide nanoparticles is simplified, solving the problem of cumbersome and time-consuming processes in existing technologies. This improves the utilization rate and electrocatalytic activity of the precious metal, making it suitable for the cathode reaction of water electrolysis to produce hydrogen.
Patent Information
- Application Number
- CN202311054121.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-21
AI Technical Summary
Existing methods for synthesizing ruthenium phosphide nanoparticle electrocatalysts are cumbersome, time-consuming, and require environmentally unfriendly chemical reagents, resulting in low utilization of the precious metal and making it difficult to meet the demand for hydrogen production through water electrolysis.
By combining rotary evaporation and solid-phase phosphating, phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalysts were prepared by directly phosphating ruthenium metal salts on a carbon support, simplifying the process and improving dispersibility and activity.
This method enables efficient and simple preparation of ruthenium phosphide nanoparticles, improving the utilization rate and electrocatalytic activity of the precious metal. It is suitable for hydrogen evolution reactions at the cathodes of acidic and alkaline water electrolysis.
Smart Images

Figure CN117127193B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal electrocatalyst technology, and relates to a method for preparing and applying a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction. Background Technology
[0002] Dependence on fossil fuels and the associated environmental pollution have spurred the development of renewable and clean energy sources. Hydrogen, with its high energy density and zero carbon content, is considered an ideal energy carrier. Currently, industrial hydrogen production mainly involves methane steam reforming and water-gas shift reactions, processes with high CO2 emissions, high energy consumption, and low gas purity. Water electrolysis for hydrogen production offers advantages such as simplicity, high efficiency, zero CO2 emissions, and the ability to absorb renewable energy, making it a highly attractive hydrogen production technology. The water electrolysis reaction consists of hydrogen evolution reaction (HER) at the cathode and oxygen evolution reaction (OER) at the anode. In developing water electrolysis for hydrogen production technology, the HER at the cathode requires a highly efficient and inexpensive electrocatalyst to accelerate the reaction. Pt-based materials have long been considered excellent HER electrocatalysts. However, their high cost and scarce crustal reserves limit their application and hinder the development of water electrolysis for hydrogen production technology. Ru is the cheapest Pt group metal and possesses similar electrocatalytic performance to Pt. Therefore, Ru-based electrocatalysts may become a cost-effective alternative to Pt-based electrocatalysts. However, Ru tends to agglomerate during synthesis and reaction, leading to a decrease in the number of exposed active sites and low utilization efficiency. Therefore, there is a need to synthesize highly dispersed, anti-agglomeration Ru-based HER electrocatalysts. Modulating the electronic structure of Ru by introducing other heteroelements or adding other active sites to improve the utilization rate of noble metals has become a new research hotspot in the field of water electrolysis. Based on this, the HER activity of ruthenium-based phosphides has attracted widespread attention.
[0003] Li Chengchao et al. first loaded ruthenium nanoparticles onto the surface of carbon nanotubes using a sodium borohydride liquid-phase reduction method. Then, they placed a phosphorus source and the ruthenium nanoparticle-loaded carbon nanotube powder into quartz tubes under vacuum, followed by annealing, cleaning, and drying to prepare 10-15 nm ruthenium diphosphide nanoparticles loaded on carbon nanotubes. This method involves two steps and requires high-temperature vacuum conditions, making the process cumbersome and demanding. The resulting ruthenium diphosphide nanoparticles are relatively large, which is detrimental to improving the utilization rate of the precious metal. (Patent Application No.: 201810785466.5)
[0004] He Chunting et al. used methanol as a solvent to mix a Ru metal salt precursor with carbon nanotubes, hexachlorotriphosphazene, 4,4'-dihydroxydiphenyl sulfone, and triethylamine. The mixture was stirred at room temperature for 1-2 days, filtered, washed with methanol, dried, and then kept at 800-1000℃ for 1-3 hours under an inert gas atmosphere to prepare an average ultrafine ruthenium diphosphide nanoparticle electrocatalyst. However, this method involves the use of many highly toxic chemical reagents during synthesis, which is environmentally harmful, and the synthesis process is too time-consuming. (Patent Application No.: 202111388178.4). Li Jisen et al. used copper acetate as a precursor and trimesic acid as a ligand in an ethanol system, stirring for 15-24 hours, followed by centrifugation, washing, and drying to obtain a copper-based metal-organic framework. This framework was then dispersed with a ruthenium source in an aqueous-alcohol system and stirred for 20-24 hours, followed by calcination under an inert atmosphere for 3-5 hours. The copper component was then removed by washing with ferric chloride to obtain porous carbon-supported ruthenium. Finally, this was calcined with ammonium dihydrogen phosphate in a tube furnace at high temperature for 3-5 hours to obtain a porous carbon-supported ruthenium phosphide nanoparticle catalyst. However, the preparation of the metal-organic framework and the ruthenium trichloride stirring and impregnation process are time-consuming, involve multiple water, alcohol, and ferric chloride washing processes, and two-step high-temperature calcination treatments, resulting in a cumbersome and energy-intensive process (Patent Application No.: 202110181251.4). Cui Dayang et al. dissolved calcium and phosphorus sources in an aqueous system with a pH of 2-4 in a specific ratio, adjusted the pH to 10-12 with ammonia, and reacted in a water bath at 40-90℃ for 4-10 hours, followed by aging at room temperature for 18-24 hours. The mixture was then filtered, washed with deionized water, and freeze-dried to obtain a hydroxyapatite carrier. The pH of the ruthenium chloride solution was then adjusted to approximately 7 with ammonia, and the hydroxyapatite was dispersed in the ruthenium chloride solution, stirred at room temperature for 2-5 hours, centrifuged, washed, and dried. Finally, the mixture was reduced at a programmed temperature of 400℃ for 2 hours under a hydrogen atmosphere, followed by further reduction at 600-800℃ for 4-6 hours to obtain micronized monodisperse ruthenium phosphide. This method also suffers from the time-consuming stirring and settling processes, and the high energy consumption of the two-step isothermal calcination.
[0005] In summary, the reported synthesis methods for ruthenium phosphide nanocatalysts often require the use of environmentally unfriendly chemical reagents; the synthesis steps are cumbersome or the resulting spherical metal nanoparticles have low utilization rates. Therefore, researching highly dispersed, ultrafine ruthenium phosphide nanoparticle electrocatalysts suitable for hydrogen evolution reactions at water electrolysis cathodes has significant application value. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing and applying a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction at the cathode of water electrolysis, addressing the shortcomings of existing technologies.
[0007] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0008] This invention provides a method for preparing a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction, the method comprising the following steps:
[0009] (1) Disperse the carbon support in a concentrated acid aqueous solution and sonicate to obtain a uniform dispersion; place the dispersion in a hot water bath at 50-90℃, stir and reflux for 1-3 hours, cool to room temperature, and then vacuum filter, wash, dry and grind with deionized water to obtain a carboxyl-modified carbon support.
[0010] (2) The carboxyl-modified carbon support prepared in step (1) is dispersed in a solvent with ruthenium metal salt and phosphorus source, and ultrasonically mixed to obtain a uniformly mixed slurry; the mixed slurry is rotary evaporated at 60-90℃ to obtain a gray-black precursor solid powder. After thorough grinding, it is calcined at 600-950℃ for 1-3h under an inert atmosphere. The obtained sample is dispersed in deionized water at 60-90℃, soaked, ultrasonicated for 10-30min, vacuum filtered, and finally dried to obtain a black powder, which is the phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticles for acidic and alkaline hydrogen evolution reactions.
[0011] The solvent is water and / or alcohol solvents such as methanol, ethanol, and isopropanol, preferably a mixed solution of water and ethanol, and more preferably a mixed solution of water and ethanol in a volume ratio of 1:1.
[0012] The concentration of the carbon support in the concentrated acid aqueous solution is 0.5–30 mg / ml. -1 Preferably 1–20 mg / ml -1 More preferably 1–10 mg / ml -1 ;
[0013] The concentration of the concentrated acid aqueous solution is 0.5-8 mol / L. -1 Preferably 1–6 mol / L -1 More preferably 2-4 mol / L -1 ;
[0014] The concentration of the ruthenium metal salt in the solvent is 0.002–0.05 mol / L. -1 Preferably, the concentration is 0.002–0.04 mol / L. -1 More preferably, it is 0.002–0.025 mol / L. -1 ;
[0015] The concentration of the phosphorus source in the solvent is 0.125–150 mg / ml. -1 Preferably, the dosage is 0.125–100 mg / ml. -1 More preferably, 0.25–50 mg / ml -1 ;
[0016] The concentration of the carbon support in the solvent is 0.2–20 mg / ml. -1 Preferably 0.2–10 mg / ml -1 More preferably 0.5–5 mg / ml -1 .
[0017] Furthermore, the carbon support is one or more of conductive carbon black, activated carbon, graphene oxide, single-walled carbon nanotubes, and multi-walled carbon nanotubes.
[0018] Furthermore, the acid in the concentrated acid aqueous solution is one or more of permanganic acid, sulfuric acid, nitric acid, and perchloric acid.
[0019] Furthermore, the ultrasonic treatment time in step (1) is 10-50 min; the drying temperature in step (1) is 60-80℃; and the grinding time in step (1) is 15-50 min.
[0020] Further, the ruthenium metal salt is one or more mixtures of hexaammineruthenium monochloride, ruthenic acid, sodium ruthenate, potassium ruthenate, ammonium ruthenate, ammonium ruthenate, potassium hexachlororuthenate(III), ruthenium trichloride, and ruthenium acetylacetonate.
[0021] Furthermore, the phosphorus source is one or a mixture of two or more of the following: red phosphorus, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, phosphoric acid, sodium phosphate, sodium hypophosphite, sodium dihydrogen phosphate, and sodium monohydrogen phosphate.
[0022] Further, the ultrasonic homogenization time in step (2) is 20-50 min; the grinding time in step (2) is 0.5-2 h; the drying temperature in step (2) is 60-80℃; and the concentration of the sample in hot deionized water in step (2) is 1-5 mg / ml. -1 The soaking time in step (2) is 8-24 hours; the drying temperature in step (2) is 60-80℃.
[0023] Furthermore, the protective gas is one or more of nitrogen, argon, and helium.
[0024] Furthermore, the heating rate of the programmed heating process is 0.5-15℃ / min. -1 The airflow rate during the programmed heating process is 10 sccm-400 sccm.
[0025] The present invention also provides a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction prepared by the above preparation method, wherein the phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticles have a Ru loading of 30-40 wt% and a particle size of 3-5 nm.
[0026] The present invention also provides an application of the above-mentioned phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst in the hydrogen evolution reaction at the cathode of water electrolysis, including its application in acidic and alkaline water electrolysis cathode hydrogen evolution reactions.
[0027] This invention combines rotary evaporation with solid-phase phosphating to directly phosphate Ru metal salts, thus preparing ruthenium phosphide electrocatalysts. The ruthenium phosphide nanoparticles obtained by this invention have uniform chemical composition, small size, and good dispersibility, and exhibit high specific activity and excellent electrocatalytic activity, making them suitable for hydrogen evolution reactions at the cathodes of acidic and alkaline water electrolysis.
[0028] Compared with the reported preparation and application of carbon-supported highly dispersed noble metal electrocatalysts, the present invention has the following advantages:
[0029] a) The preparation process of the present invention is simple, and nanoparticle-level ruthenium phosphide electrocatalysts can be directly prepared from ruthenium salts. Moreover, the synthesis process only requires one pyrolysis step, which is time-saving and energy-efficient.
[0030] b) The preparation process of the present invention has strong applicability and can prepare ruthenium phosphide nanoparticle electrocatalysts with different ruthenium phosphide ratios, including ruthenium diphosphide and ruthenium diphosphide, by adjusting the process parameters.
[0031] c) The ruthenium phosphide nanoparticles prepared by this invention have good morphological uniformity and do not exhibit severe agglomeration.
[0032] d) The ruthenium phosphide nanoparticles prepared by this invention have a small diameter, which can effectively improve the utilization rate of metal atoms.
[0033] e) By adjusting the amount of phosphorus source introduced, the present invention can effectively improve the intrinsic activity of ruthenium.
[0034] f) The phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst prepared in this invention has high electrocatalytic activity and is suitable for hydrogen evolution reaction at the cathode of water electrolysis. Attached Figure Description
[0035] Figure 1 This is the X-ray diffraction (XRD) pattern of the sample prepared in Example 1;
[0036] Figure 2 These are high-resolution transmission electron microscopy (HRTEM) images of the sample prepared in Example 1;
[0037] Figure 3 These are transmission electron microscope (TEM) images of the sample prepared in Example 1;
[0038] Figure 4 This is a particle size distribution diagram of the sample prepared in Example 1;
[0039] Figure 5 This is the thermogravimetric analysis (TG) curve of the sample prepared in Example 1;
[0040] Figure 6 The polarization curve of the sample prepared in Example 1 in a 0.5M H2SO4 aqueous solution is normalized to its mass.
[0041] Figure 7 The polarization curve of the sample prepared in Example 1 in a 1.0M KOH aqueous solution is normalized to its mass.
[0042] Figure 8 This is the XRD pattern of the sample prepared in Example 2;
[0043] Figure 9 These are HRTEM images of the samples prepared in Example 2;
[0044] Figure 10 These are TEM images of the samples prepared in Example 2;
[0045] Figure 11 This is a particle size distribution diagram of the sample prepared in Example 2;
[0046] Figure 12 This is the TG curve of the sample prepared in Example 2;
[0047] Figure 13 The XRD pattern of the sample prepared in Comparative Example 1 is shown below.
[0048] Figure 14 The transition frequency (TOF) curve of the sample prepared in Comparative Example 1 in 0.5M H2SO4 aqueous solution;
[0049] Figure 15 The transition frequency (TOF) curve of the sample prepared in Comparative Example 1 in 1.0 M KOH aqueous solution;
[0050] Figure 16 The XRD pattern of the sample prepared in Comparative Example 2 is shown below.
[0051] Figure 17 This is the XRD pattern of the sample prepared in Comparative Example 3. Detailed Implementation
[0052] The following embodiments will further illustrate the present invention, but are not intended to limit the invention.
[0053] Example 1
[0054] Conductive carbon black (2 mg / ml) -1 Dispersed in 50 ml of concentrated nitric acid aqueous solution (3 mol / L) -1The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 3 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 Sodium hypophosphite (3 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1 The temperature was increased to 900℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 16 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0055] like Figure 1 XRD results showed that the nanoparticle product obtained from the reaction was composed of ruthenium phosphide.
[0056] like Figure 2 HRTEM results showed that the lattice stripe widths of the obtained phosphorus-doped carbon-supported ruthenium phosphide nanoparticles were 0.24 nm and 0.22 nm, respectively, corresponding to the (112) and (211) crystal planes of Ru2P.
[0057] like Figure 3 TEM results showed that the phosphorus-doped carbon-supported ruthenium phosphide nanoparticles had a uniform morphology.
[0058] like Figure 4 Statistical analysis shows that the particle size of ruthenium phosphide nanoparticles is 4.6 ± 1.2 nm.
[0059] like Figure 5 TG determined that the Ru loading in the obtained product was 35 wt%.
[0060] like Figure 6 The prepared electrocatalyst exhibited a specific activity of 734.4 mA mg in 0.5 M H₂SO₄. -1 Ru @50mV.
[0061] like Figure 7 The prepared electrocatalyst exhibited a specific activity of 1044.6 mA mg in 1.0 M KOH. -1Ru @50mV.
[0062] Example 2
[0063] Conductive carbon black (2 mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / L) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 3 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 Sodium hypophosphite (24 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1 The temperature was increased to 900℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 16 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0064] like Figure 1 XRD results showed that the nanoparticle product obtained from the reaction was composed of ruthenium diphosphide.
[0065] like Figure 2 HRTEM results showed that the lattice stripe width of the obtained phosphorus-doped carbon-supported ruthenium diphosphide nanoparticles was 0.39 nm, corresponding to the (110) crystal plane of RuP2.
[0066] like Figure 3 TEM results showed that the phosphorus-doped carbon-supported ruthenium diphosphide nanoparticles had a uniform morphology.
[0067] like Figure 4 Statistical analysis shows that the particle size of ruthenium diphosphide nanoparticles is 4.1 ± 1.2 nm.
[0068] like Figure 5 TG determined that the Ru loading in the obtained product was 37 wt%.
[0069] Example 3
[0070] Conductive carbon black (1 mg / ml) -1Dispersed in concentrated nitric acid aqueous solution (2.0 mol / L) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 3 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 Sodium hypophosphite (24 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further sintered at 5 °C under a 100 sccm Ar atmosphere. -1 The temperature was increased to 600℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 24 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0071] Example 4
[0072] Conductive carbon black (5mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / mL) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 2 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mmol / ml) -1 Sodium hypophosphite (24 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1 The temperature was increased to 700℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 24 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0073] Example 5
[0074] Conductive carbon black (2 mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / L) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 2 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 Sodium hypophosphite (6 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1 The temperature was increased to 800℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 24 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0075] Example 6
[0076] Conductive carbon black (2 mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / L) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 2 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 Sodium hypophosphite (1.5 mg / ml) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1The temperature was increased to 900℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 24 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to finally obtain a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst.
[0077] Comparative Example 1
[0078] Conductive carbon black (2 mg / ml) -1 Dispersed in 50 ml of concentrated nitric acid aqueous solution (3 mol / L) -1 The mixture was ultrasonically treated for 15 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 3 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 The mixture was dispersed in 50 ml of a 1:1 water-ethanol mixture and sonicated for 20 min to obtain a homogeneous solution. The solution was then rotary evaporated at 80 °C to obtain a gray-black solid powder. After grinding for 30 min, the powder was further processed under an Ar atmosphere of 100 sccm at 5 °C. -1 The carbon-supported ruthenium nanoparticle electrocatalyst was obtained by heating to 900℃ for 2 hours using a programmed heating rate.
[0079] like Figure 13 XRD results showed that the nanoparticle product obtained from the reaction was composed of ruthenium.
[0080] like Figure 14 In a 0.5M H2SO4 aqueous solution, the TOF of the sample from Example 1 was significantly higher than that of the sample from Comparative Example 1.
[0081] like Figure 15 In a 1.0 M KOH aqueous solution, the TOF of the sample from Example 1 was significantly higher than that of the sample from Comparative Example 1.
[0082] Comparing the TOF curves of Example 1 and Comparative Example 1 shows that the appropriate introduction of a phosphorus source can enhance the intrinsic HER activity of ruthenium.
[0083] Comparative Example 2
[0084] Conductive carbon black (2 mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / L) -1A homogeneous dispersion was obtained by ultrasonic treatment for 15 min. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 2 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. The resulting carbon support was then vacuum dried at 80°C and ground to obtain a carboxyl-modified carbon support. This carboxyl-modified carbon support was mixed with ruthenium trichloride and sodium hypophosphite at a mass ratio of 1:2:6 and ground for 30 min. The mixture was then subjected to an Ar atmosphere of 100 sccm and heated at 5°C for 1 min. -1 The temperature was increased to 900℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 12 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to obtain the final product.
[0085] like Figure 16 XRD results showed that the obtained reaction product had Ru impurity peaks, indicating insufficient phosphating.
[0086] Comparative Example 3
[0087] Conductive carbon black (2 mg / ml) -1 Dispersed in concentrated nitric acid aqueous solution (3.0 mol / L) -1 The mixture was ultrasonically treated for 5 min to obtain a homogeneous dispersion. The homogeneous dispersion was then placed in a water bath and stirred under reflux at 80°C for 2 h. After cooling to room temperature, it was vacuum filtered with deionized water until the pH reached 7. After vacuum drying at 80°C and grinding for 1 h, a carboxyl-modified carbon support was obtained. The carboxyl-modified carbon support (1 mg / ml) was then... -1 ) and ruthenium trichloride (0.01 mol l) -1 The ruthenium chloride was dispersed in water and sonicated for 20 min to obtain a homogeneous mixture. The mixture was then rotary evaporated at 80 °C to obtain a grayish-black solid powder. This powder was mixed with sodium hypophosphite (ruthenium trichloride to sodium hypophosphite mass ratio 1:2) and ground for 30 min. Under an Ar atmosphere of 100 sccm, the mixture was then evaporated at 5 °C for 1 min. -1 The temperature was increased to 900℃ and calcined for 2 hours to obtain a black mixture. The black mixture was dispersed in 150 ml of 80℃ deionized water and soaked for 12 hours, then sonicated for 30 minutes. Vacuum filtration was then performed, and the filter residue was dried in a 65℃ forced-air dryer and ground for 5 minutes to obtain the final product.
[0088] like Figure 17 XRD results showed that the obtained reaction product had Ru impurity peaks, indicating insufficient phosphating.
Claims
1. A method for preparing a phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction, characterized in that, Includes the following steps: (1) Disperse the carbon support in a concentrated acid aqueous solution and stir to obtain a uniform dispersion; place the dispersion in a water bath at 50-90°C, stir and reflux for 1-3 h, cool to room temperature, and then perform vacuum filtration, washing, drying and grinding to obtain a carboxyl-modified carbon support. (2) The carboxyl-modified carbon support prepared in step (1) is dispersed in a solvent with ruthenium metal salt and phosphorus source and ultrasonically homogenized; the mixed slurry is rotary evaporated and ground at 60-90℃, and then calcined at 600-950℃ for 1-3 h under an inert atmosphere. The resulting sample is dispersed in deionized water at 60-90℃ and soaked. After ultrasonication for 10-30 min, it is vacuum filtered and dried to finally obtain phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for acidic and alkaline hydrogen evolution reactions. The solvent is water and / or an alcohol solvent; The carbon carrier is conductive carbon black; The acid in the concentrated acid aqueous solution is nitric acid; The concentration of the carbon support in the concentrated acid aqueous solution is 1~30 mg / ml. -1 ; The concentration of the concentrated acid aqueous solution is 0.5-8 mol / L. -1 ; The concentration of the ruthenium metal salt in the solvent is 0.002~0.05 mol / L. -1 ; The concentration of the phosphorus source in the solvent is 0.125~250 mg / ml. -1 ; The concentration of the carbon support in the solvent is 0.2~20 mg / ml. -1 ; The phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticles have a Ru loading of 30–40 wt% and a particle size of 3–5 nm.
2. The preparation method according to claim 1, characterized in that, The ruthenium metal salt is one or a mixture of hexaammineruthenium monochloride, ruthenic acid, sodium ruthenate, potassium ruthenate, ammonium ruthenate, ammonium ruthenium chloride, potassium hexachlororuthenate(III), ruthenium trichloride, and ruthenium acetylacetonate. The phosphorus source is one or a mixture of two or more of the following: red phosphorus, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, phosphoric acid, sodium phosphate, sodium hypophosphite, sodium dihydrogen phosphate, and sodium monohydrogen phosphate.
3. The preparation method according to claim 1, characterized in that, The inert atmosphere is one or more of helium, argon, and nitrogen; The alcohol solvent is one or more of methanol, ethanol, and isopropanol.
4. The preparation method according to claim 1, characterized in that, In step (1), the stirring time during the preparation of a uniform dispersion is 10-50 min; the drying temperature in step (1) is 60-80℃; and the grinding time in step (1) is 15-50 min.
5. The preparation method according to claim 1, characterized in that, The ultrasonic homogenization time in step (2) is 20-50 min; the grinding time in step (2) is 0.5-2 h; the drying temperature in step (2) is 60-80℃; the volume of hot deionized water in step (2) is 80-200 ml; the soaking time in step (2) is 8-24 h; and the drying temperature in step (2) is 60-80℃.
6. The preparation method according to claim 1, characterized in that, The heating rate of the programmed temperature rise process is 0.5-15℃ / min. -1 The airflow rate during the programmed heating process is 10 sccm-400 sccm.
7. The phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst for hydrogen evolution reaction prepared by the preparation method according to any one of claims 1-6.
8. The application of the phosphorus-doped carbon-supported ultrafine ruthenium phosphide nanoparticle electrocatalyst according to claim 7 in the hydrogen evolution reaction at the cathode of acidic and alkaline water electrolysis.
Citation Information
Patent Citations
A ruthenium phosphide / carbon nanotube composite material, its preparation method and application
CN109112563B
Preparation method and application of porous carbon supported ruthenium phosphide catalyst
CN112877715A
Synthesis method of superfine ruthenium diphosphide nanoparticle electrocatalyst
CN114293222A
New method for preparing loaded Ru2P under mild condition
CN101862673A