Gas sensitive paste, method for preparing the same, gas sensor and method for preparing the same

By treating tin dioxide with aluminum and cerium salts and adding a platinum-palladium catalyst in a SnO₂-based gas sensor, a gas-sensitive slurry resistant to ethanol interference was prepared, solving the problem of false alarms caused by ethanol gas interference and improving the stability and lifespan of the sensor.

CN117129532BActive Publication Date: 2026-11-20SUZHOU HUIWEN NANO TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311094490.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2026-11-20
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

Existing SnO₂-based gas sensors are sensitive to interference from ethanol gas, leading to false alarms, and the filter layer is prone to saturation, affecting the stability and lifespan of the sensor.

Method used

Tin dioxide was treated by hydrolysis of aluminum salts and/or cerium salts, and combined with platinum and palladium catalysts to prepare a gas-sensitive slurry resistant to ethanol interference. Temperature and time were controlled during the sintering process to form a stable gas-sensitive coating.

Benefits of technology

The gas sensor's resistance to interference from ethanol has been improved, enhancing the sensor's stability and lifespan, and reducing false alarms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117129532B_ABST
    Figure CN117129532B_ABST
Patent Text Reader

Abstract

The application relates to a gas-sensitive slurry, a preparation method thereof, a gas sensor and a preparation method thereof, which comprises the following steps: S1, providing tin dioxide and an aqueous metal salt solution containing an aluminum salt or containing an aluminum salt and a cerium salt; S2, adding the tin dioxide into the aqueous metal salt solution to obtain a mixed solution; S3, adjusting the mixed solution to be weakly alkaline, and drying to obtain a substrate; S4, adding a catalyst into the substrate and mixing to obtain a powder material; and S5, dissolving the powder material in a solvent to obtain the gas-sensitive slurry. The preparation method can improve the ethanol resistance of the gas-sensitive slurry, thereby improving the stability and service life of the gas sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a gas-sensitive slurry resistant to ethanol interference, its preparation method, a gas sensor and its preparation method, belonging to the field of gas sensor technology. Background Technology

[0002] Semiconductor metal oxide gas sensors are widely used for detecting pollutants, flammable, and toxic gases. SnO2-based gas sensors offer advantages such as low cost, simple design, and fast response. Their basic working principle is that SnO2, as an n-type semiconductor, exhibits increased conductivity in the presence of reducing gases. Therefore, a drawback of SnO2-based gas sensors is their sensitivity to most reducing gases. To overcome this drawback, various methods have been employed to improve the sensor's selectivity. For example, doping SnO2 with noble metals such as platinum and palladium, combined with optimizing the sensor's operating temperature, can enhance its selectivity for alkanes such as methane and propane.

[0003] In addition, another important method is to use a filter layer (such as an activated carbon adsorption layer) or a membrane to prevent interfering gases from passing through the sensor's sensing element. The main drawback of using this method is that the adsorption layer tends to reach adsorption saturation over time, and adding an external filter layer also has certain structural and cost disadvantages.

[0004] Sensors used in household / industrial gas alarm scenarios operate in complex environments and are often subject to interference from other gases, such as ethanol gas in a kitchen environment. Due to the similarity in properties between ethanol gas and alkane gases such as methane / propane, false alarms are frequently triggered.

[0005] Therefore, it is necessary to explore and study new preparation methods to further improve the performance of methane / propane sensitive materials against ethanol interference. Summary of the Invention

[0006] The purpose of this application is to provide a gas-sensitive slurry resistant to ethanol interference, its preparation method, a gas sensor and its preparation method, which can improve the ethanol resistance of the gas-sensitive slurry, thereby improving the stability and lifespan of the gas sensor.

[0007] To achieve the above objectives, this application provides the following technical solution:

[0008] In a first aspect, this application provides a method for preparing a gas-sensitive slurry resistant to ethanol interference, comprising the following steps:

[0009] S1. Provide an aqueous solution of tin dioxide and a metal salt, wherein the aqueous solution of the metal salt contains an aluminum salt, or contains an aluminum salt and a cerium salt;

[0010] S2. Add tin dioxide to an aqueous solution of a metal salt to obtain a mixed solution;

[0011] S3. Adjust the mixture to a weakly alkaline state, and dry it to obtain the substrate;

[0012] S4. Add a catalyst to the substrate and mix to obtain a powder material;

[0013] S5. Dissolve the powder material in a solvent to obtain a gas-sensitive slurry.

[0014] The technical solution of this embodiment allows for the hydrolysis reaction to make the solution acidic in an aqueous environment containing aluminum salts and cerium salts or only aluminum salts. Tin dioxide is then surface-acidified, and its pH is adjusted to weakly alkaline. After adding a catalyst, a gas-sensitive slurry with better ethanol resistance can be obtained, which is suitable for household / industrial gas alarms.

[0015] In some possible implementations, in step S1, the aluminum salt content in the aqueous metal salt solution is 0.5-20 mol% of tin dioxide.

[0016] In one preferred embodiment, the aluminum salt content is 2 mol% of tin dioxide.

[0017] In some possible implementations, the aluminum salt is an aluminum nitrate and / or chloride salt.

[0018] In some possible implementations, the cerium salt is a nitrate and / or chloride salt of cerium.

[0019] In some possible implementations, step S2, adding tin dioxide to an aqueous metal salt solution to obtain a mixture, includes:

[0020] Tin dioxide is added to an aqueous solution of metal salt and stirred at a constant temperature of 20-40℃ for 2-10 hours. The heating method is either water bath heating or oil bath heating.

[0021] As one preferred embodiment, the stirring temperature is 25°C and the stirring time is 6 hours.

[0022] In some possible implementations, in step S3, the pH of the mixture is adjusted to 7.1-8.5, and then dried.

[0023] Preferably, the pH of the mixture is adjusted to 8.

[0024] In some possible implementations, in step S4, the catalyst comprises a platinum catalyst and a palladium catalyst, the content of each of the platinum catalyst and palladium catalyst being independently 0.5-5 at% of tin.

[0025] In one preferred embodiment, the content of platinum catalyst and palladium catalyst in each group is independently 1-2 at% of tin.

[0026] In some possible implementations, step S4 further includes adding cerium oxide to the substrate, wherein the content of cerium salt or cerium oxide is 2-20 mol% of tin.

[0027] In some possible implementations, in step S5, the mass ratio of solvent to powder material is 0.8-1.2.

[0028] In some possible implementations, it also includes:

[0029] S6. After coating, the obtained gas-sensitive slurry is sintered to obtain a gas-sensitive coating.

[0030] In some possible implementations, the sintering temperature is 350-550°C and the sintering time is 1-3 hours.

[0031] As one preferred embodiment, the sintering temperature is 400°C and the sintering time is 2 hours.

[0032] Secondly, this application provides an ethanol-resistant gas-sensitive slurry prepared according to the preparation method of the ethanol-resistant gas-sensitive slurry of the first aspect.

[0033] Thirdly, this application provides a method for preparing a gas sensor, which includes: coating a gas-sensitive slurry from the second aspect onto a heating element to form a gas-sensitive coating, and then sintering and encapsulating it to obtain a gas sensor.

[0034] Through the technical solution of this embodiment, the alumina produced by thermal decomposition during the sintering process has strong thermal stability, which can inhibit grain growth and help stabilize the crystal structure, thereby improving the stability and service life of the gas sensor.

[0035] In some possible implementations, the sintering temperature is 400°C and the sintering time is 2 hours.

[0036] Fourthly, this application provides a gas sensor prepared according to the gas sensor preparation method of the third aspect.

[0037] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, the preferred embodiments of this application are described in detail below with reference to the accompanying drawings. Attached Figure Description

[0038] Figure 1 This is a flowchart illustrating the preparation method of the gas-sensitive slurry resistant to ethanol interference provided in this application.

[0039] Figures 2A to 2CThis is a SEM image of the gas-sensitive coating formed by the gas-sensitive slurry provided in Embodiment 1 of this application;

[0040] Figure 3A This is an EDS image of the gas-sensitive coating formed by the gas-sensitive slurry provided in Embodiment 1 of this application;

[0041] Figure 3B This is the EDS energy spectrum of the gas-sensitive coating formed by the gas-sensitive slurry provided in Embodiment 1 of this application;

[0042] Figure 4 This is a propane response curve of the gas sensor provided in Embodiment 1 of this application;

[0043] Figure 5 This is a graph showing the propane sensitivity and ethanol resistance test data of the gas sensor provided in Embodiment 1 of this application. Detailed Implementation

[0044] The specific embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The following examples are used to illustrate this application, but are not intended to limit the scope of this application.

[0045] It should be noted that the terms "upper", "lower", "left", "right", "inner", and "outer" used in this application are only for illustrative purposes with reference to the accompanying drawings and are not intended to be limiting terms.

[0046] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, at least one of a, b, or c means: a, b, c, ab, ac, bc, or abc, where a, b, and c are single or multiple.

[0047] It should be understood that in the various embodiments of this application, the order of the above-mentioned processes does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0048] Figure 1 A flowchart illustrating the preparation method of the ethanol-resistant gas-sensitive slurry of this application is shown, as follows: Figure 1 As shown, the preparation method includes:

[0049] S1. Provide an aqueous solution of tin dioxide and a metal salt, wherein the aqueous solution of the metal salt contains an aluminum salt, or contains an aluminum salt and a cerium salt;

[0050] S2. Add tin dioxide to an aqueous solution of a metal salt to obtain a mixed solution;

[0051] S3. Adjust the mixture to a weakly alkaline state, and dry it to obtain the substrate;

[0052] S4. Add a catalyst to the substrate and mix to obtain a powder material;

[0053] S5. Dissolve the powder material in a solvent to obtain a gas-sensitive slurry.

[0054] Optionally, in step S4, after adding the catalyst, cerium oxide can be selectively added to the substrate. Specifically, when the metal salt aqueous solution does not contain cerium salt, cerium oxide needs to be added after adding the catalyst; when the metal salt aqueous solution contains cerium salt, cerium oxide can be selectively added.

[0055] Optionally, when preparing an aqueous solution containing aluminum salt and cerium salt or containing only aluminum salt, the aluminum salt is added at 0.5-20 mol% of tin dioxide, preferably 2 mol%, and the cerium salt or cerium oxide is added at 2-20 mol% of the total tin ions.

[0056] Optionally, the catalyst includes a platinum catalyst and a palladium catalyst, wherein the amount of platinum catalyst and palladium catalyst added is 0.5-5 at% of Sn, preferably 1-2 at%.

[0057] Optionally, the mass ratio of solvent to powder material is 0.8-1.2.

[0058] Optionally, the solvent is an organic solvent such as ethylene glycol or polyethylene glycol.

[0059] Alternatively, after obtaining the gas-sensitive slurry, it can be coated and then sintered to obtain a gas-sensitive coating.

[0060] Alternatively, in order to complete the mixing for generating the precipitate within a specified time, a mixing device such as a stir bar can be used.

[0061] Based on the above preparation method, this application also provides a method for preparing a gas sensor, in which the obtained gas-sensitive slurry is coated onto a heating element and then sintered to obtain a gas-sensitive coating. After encapsulation, a gas sensor is obtained.

[0062] The present application will be further described in detail below with reference to specific embodiments.

[0063] Example 1

[0064] First, prepare an aqueous solution containing aluminum and cerium salts. Add tin dioxide to the aqueous solution, with aluminum salt at 2 mol% of tin dioxide and cerium salt at 15 mol% of tin ions. Stir at 25°C for 6 hours. Then, add ammonia dropwise to adjust the pH to 8. After drying, obtain a tin dioxide substrate. Subsequently, add 2 at% Pt and 2 at% Pd chlorides, and mix to obtain a powder material. Then, add polyethylene glycol at a mass ratio of 1.1 to the powder and mix thoroughly to obtain a gas-sensitive slurry.

[0065] The prepared gas-sensitive slurry was coated onto a micro-heating plate and sintered at 400°C for 2 hours. After encapsulation, a gas sensor was obtained.

[0066] In this embodiment, the fabricated sensor film was analyzed by SEM and EDS. Figures 2A to 2C An SEM image of the gas-sensitive coating of this embodiment is shown. Figures 2A to 2C As shown, the results indicate that the film layer is uniformly distributed on the micro-heating plate without obvious cracks.

[0067] Figure 3A The EDS diagram of the gas-sensitive coating of this embodiment is shown; Figure 3B The EDS energy spectrum of the gas-sensitive coating in this embodiment is shown below. The specific energy spectrum data are shown in Table 1 below:

[0068] element Wt% Wt%Sigma C 3.80 0.30 O 18.48 0.20 Al 0.65 0.05 Si 1.51 0.05 Zr 1.02 0.14 Pd 3.47 0.18 Sn 47.44 0.39 Ce 23.63 0.43 Total 100

[0069] The results show that the elements are relatively evenly distributed in the material system.

[0070] This embodiment tested the response curve of the prepared sensor to propane and obtained the change in the sensor's response performance with aging time based on the response curve. Figure 4 As shown, the results indicate that the sensor is highly sensitive to propane, at V CC Under a test condition of 5V, the response difference to 2000ppm propane is approximately 2.0V; at the same time, the sensor exhibits good stability with minimal zero-point drift as the aging time increases.

[0071] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol. For example... Figure 5 As shown, the results indicate that the sensor exhibits a significant response gradient to different concentrations of propane, and the response value is less than 0.5V after running for half an hour in an environment with 2000ppm ethanol.

[0072] Example 2

[0073] First, prepare an aqueous solution containing aluminum and cerium salts. Add tin dioxide to the aqueous solution, with aluminum salt at 2 mol% of tin dioxide and cerium salt at 20 mol% of tin ions. Stir at 25°C for 6 hours. Then, add ammonia dropwise to adjust the pH to 8. After drying, obtain a tin dioxide substrate. Subsequently, add 2 at% Pt and 2 at% Pd chlorides and mix to obtain a powder material. Then, add polyethylene glycol at a mass ratio of 1.2 to the powder and mix thoroughly to obtain a gas-sensitive slurry.

[0074] The prepared gas-sensitive slurry was coated onto a micro-heating plate and sintered at 400°C for 2 hours. After encapsulation, a gas sensor was obtained.

[0075] This embodiment tested the methane sensitivity of the fabricated sensor, and the results showed that in V... CC Under a test condition of 5V, the response difference to 5000ppm methane is approximately 2.0V; simultaneously, the sensor exhibits excellent stability with minimal zero-point drift as the aging time increases.

[0076] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol, and the results showed that the response difference was <0.5V.

[0077] Example 3

[0078] First, an aqueous solution containing aluminum salt was prepared. Tin dioxide was added to the aqueous solution, with the amount of aluminum salt being 2 mol% of the tin dioxide content. The solution was stirred at a constant temperature of 25°C for 6 hours. Then, ammonia was added dropwise to adjust the pH of the solution to 8. After drying, a tin dioxide substrate was obtained. Subsequently, 2 at% Pt, 2 at% Pd chloroplatinic acid, chloropalladium acid, and 15 mol% Ce oxide were added and mixed to obtain a powder material. Finally, ethylene glycol at a mass ratio of 1.1 to the powder was added and mixed thoroughly to obtain a gas-sensitive slurry.

[0079] The prepared gas-sensitive slurry was coated onto a ceramic plate and sintered at 400°C for 2 hours. After encapsulation, a gas sensor was obtained.

[0080] This embodiment tested the propane sensitivity of the fabricated sensor, and the results showed that in V... CC Under a test condition of 5V, the response difference to 2000ppm propane is approximately 2.1V; simultaneously, the sensor exhibits excellent stability with minimal zero-point drift as the aging time increases.

[0081] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol, and the results showed that the response difference was <0.5V.

[0082] Example 4

[0083] In this embodiment, the pretreatment process of Example 3 above is repeated to obtain a tin dioxide substrate. Then, 2 at% Pt, 2 at% Pd chloroplatinic acid, chloropalladium acid, and 20 mol% Ce oxide are added and mixed to obtain a powder material. Then, ethylene glycol at a mass ratio of 1.2 is added and mixed evenly to obtain a gas-sensitive slurry.

[0084] The prepared gas-sensitive slurry was coated onto a ceramic tube and sintered at 400°C for 2 hours. After encapsulation, the gas sensor was obtained.

[0085] This embodiment tested the methane sensitivity of the fabricated sensor, and the results showed that in V... CC Under a test condition of 5V, the response difference to 5000ppm methane is approximately 2.0V; simultaneously, the sensor exhibits excellent stability with minimal zero-point drift as the aging time increases.

[0086] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol, and the results showed that the response difference was <0.5V.

[0087] In other, undemonstrated embodiments, ammonia may be added dropwise to adjust the pH of the solution to any value excluding 8, from 7.1 to 8.5.

[0088] Example 5

[0089] The gas-sensitive slurry was obtained by repeating the process of Example 4 above, except that the amount of Ce oxide was 10 mol% of tin dioxide, and the mass ratio of ethylene glycol to powder was 1.1. The gas-sensitive slurry was coated on a ceramic plate and sintered at 400°C for 2 hours. After encapsulation, a gas sensor was obtained.

[0090] This embodiment tested the propane sensitivity of the fabricated sensor, and the results showed that in V... CC Under a test condition of 5V, the response difference to 2000ppm propane is approximately 2.0V; simultaneously, the sensor exhibits excellent stability with minimal zero-point drift as the aging time increases.

[0091] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol, and the results showed that the response difference was <0.5V.

[0092] Example 6

[0093] The gas-sensitive slurry was obtained by repeating the process of Example 5 above, except that 1 at% Pt and 1 at% Pd chlorides were added, and the amount of Ce oxide was 2 mol% of tin dioxide. Triton solvent was selected, and its mass ratio with the powder was 1.0. The gas-sensitive slurry was then coated on a ceramic plate and sintered at 400°C for 2 hours. After encapsulation, the gas sensor was obtained.

[0094] This embodiment tested the propane sensitivity of the fabricated sensor, and the results showed that in V... CC Under a test condition of 5V, the response difference to 2000ppm propane is approximately 2.0V; simultaneously, the sensor exhibits excellent stability with minimal zero-point drift as the aging time increases.

[0095] This embodiment tested the response of the prepared sensor to 2000 ppm ethanol, and the results showed that the response difference was <0.5V.

[0096] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0097] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for preparing a gas-sensitive slurry resistant to ethanol interference, characterized in that, Includes the following steps: S1. Provide an aqueous solution of tin dioxide and a metal salt, wherein the aqueous solution of the metal salt contains an aluminum salt, or contains an aluminum salt and a cerium salt, wherein the aluminum salt content in the aqueous solution of the metal salt is 0.5-20 mol% of tin dioxide, and the oxide of the cerium salt is added at 2-20 mol% of the total tin ions; S2. Add the tin dioxide to the aqueous solution of the metal salt to obtain a mixed solution; S3. Adjust the pH of the mixture to 7.1-8.5, and dry it to obtain the substrate; S4. Add a catalyst to the substrate and mix to obtain a powder material. The catalyst includes a platinum catalyst and a palladium catalyst, and the content of each of the platinum catalyst and palladium catalyst is independently 0.5-5 at% of tin. S5. Dissolve the powder material in a solvent to obtain the gas-sensitive slurry; In step S2, adding the tin dioxide to the aqueous solution of the metal salt to obtain a mixture includes: The tin dioxide is added to the aqueous solution of the metal salt and stirred at a constant temperature of 20-40°C for 2-10 hours. The heating method is water bath heating or oil bath heating.

2. The method for preparing the ethanol-resistant gas-sensitive slurry as described in claim 1, characterized in that, The aluminum salt is an aluminum nitrate and / or chloride; and / or, the cerium salt is a cerium nitrate and / or chloride.

3. The method for preparing the gas-sensitive slurry resistant to ethanol interference as described in any one of claims 1 to 2, characterized in that, Step S4 further includes adding cerium oxide to the substrate, wherein the content of the cerium salt or cerium oxide is 2-20 mol of tin.

4. The method for preparing the gas-sensitive slurry resistant to ethanol interference as described in claim 1, characterized in that, In step S5, the mass ratio of the solvent to the powder material is 0.8-1.

2.

5. The gas-sensitive slurry resistant to ethanol interference prepared by the method for preparing the gas-sensitive slurry resistant to ethanol interference according to any one of claims 1 to 4.

6. A method for preparing a gas sensor, characterized in that, The gas-sensitive slurry described in claim 5 is coated onto the heating element to form a gas-sensitive coating, and then sintered and encapsulated to obtain the gas sensor.

7. The method for preparing a gas sensor as described in claim 6, characterized in that, During the sintering process, the sintering temperature is 350-550℃ and the sintering time is 1-3 hours.

8. A gas sensor prepared by the method of preparing a gas sensor according to claim 6 or 7.

Citation Information

Patent Citations

  • Supported palladium-based catalyst as well as preparation method and application thereof

    CN114602465A

  • Anti-interference gas-sensitive coating for semiconductor combustible gas sensor as well as preparation method and application of anti-interference gas-sensitive coating