A method for manufacturing a matrix type LED chip
By forming an opening groove with an inner arc surface on the epitaxial layer of a matrix LED chip and using an Ag mirror to reflect lateral light, the problem of sidewall divergence in the rectangular epitaxial layer is solved, the vertical light extraction efficiency is improved, and the light extraction performance of the LED chip is enhanced.
Patent Information
- Application Number
- CN202311206458.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-19
AI Technical Summary
In existing matrix LED chips, the sidewall divergence of the rectangular epitaxial layer during light emission reduces the vertical light emission efficiency, thus affecting the light emission performance of the LED chip.
By coating a photoresist composite layer with progressively decreasing thickness and viscosity on the epitaxial layer, an opening groove with an arc-shaped inner wall is formed. When light is emitted from the side, an Ag mirror is used to reflect the light, converting it into vertical light and reducing the side light emission.
It improves the luminous efficacy of vertical light emission and enhances the light emission performance of LED chips.
Smart Images

Figure CN117153972B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a method for fabricating a matrix LED chip. Background Technology
[0002] LED chips have advantages such as high efficiency and energy saving, long service life and small size, and are now widely used in home lighting, landscape lighting, backlight display, digital display, direct display and other fields.
[0003] Existing LED chips are formed by sequentially stacking and growing a flat N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer on a substrate to form a rectangular epitaxial layer. After completing the setting of conductive layers, electrode layers, etc., an LED chip is formed, and then light is emitted through the rectangular epitaxial layer.
[0004] However, when light is emitted from the rectangular epitaxial layer, it not only emits light vertically, but the light also diffuses outward through the sidewalls of the rectangular epitaxial layer, thereby reducing the luminous efficiency of vertical light emission and affecting the light emission performance of the LED chip. Summary of the Invention
[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for fabricating a matrix LED chip, which aims to solve the technical problem in the prior art where the growth of a rectangular epitaxial layer results in an excessively large light emission angle during subsequent LED chip light emission, causing some light to diverge from the sidewalls of the rectangular epitaxial layer, reducing the vertical light emission efficiency, and thus affecting the light emission performance of the LED chip.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing a matrix LED chip, comprising the following steps:
[0007] Provide a substrate for growth, and deposit an epitaxial layer on the substrate;
[0008] A photoresist composite layer is coated on the epitaxial layer. The photoresist composite layer includes a first photoresist layer, a second photoresist layer, a third photoresist layer, and a fourth photoresist layer, which are arranged sequentially from bottom to top and whose thickness and viscosity decrease sequentially from bottom to top.
[0009] A first opening groove is formed on the photoresist composite layer, penetrating the photoresist composite layer and having an inner wall of a first arc surface, so as to form a second opening groove on the epitaxial layer through the etching process, penetrating the epitaxial layer and having an inner wall of a second arc surface. A plurality of second opening grooves divide the epitaxial layer into a plurality of epitaxial sublayers.
[0010] A first insulating protective layer is deposited on the epitaxial layer and covered on the second arc surface. The end of the first insulating protective layer away from the substrate encloses a accommodating space on the side of the epitaxial sublayer facing away from the substrate.
[0011] An Ag reflector is deposited on the epitaxial layer, and a portion of the Ag reflector is deposited on the first insulating protective layer.
[0012] Compared with the prior art, the beneficial effects of the present invention are as follows: by setting the first photoresist layer, the second photoresist layer, the third photoresist layer and the fourth photoresist layer with decreasing thickness and viscosity, a first opening groove with the inner wall of the first arc surface can be formed on the photoresist composite layer stacked by photolithography. Then, the first opening groove is copied to the epitaxial layer by etching, and a second opening groove with the inner wall of the second arc surface is formed on the epitaxial layer. When the epitaxial layer emits light, its lateral light emission can be diffused through the second arc surface. Through the Ag reflector covered on the first insulating layer, when the lateral light emission of the epitaxial layer is diffused along the second arc surface, it can be reflected by the Ag reflector, thereby converting the light into vertical light, effectively converging the emission angle, reducing lateral light emission, improving the luminous efficiency of vertical light emission, and thus improving the light emission performance of the LED chip.
[0013] Furthermore, the step of coating a photoresist composite layer on the epitaxial layer, wherein the photoresist composite layer comprises a first photoresist layer, a second photoresist layer, a third photoresist layer, and a fourth photoresist layer arranged sequentially from bottom to top, with their thickness and viscosity decreasing sequentially from bottom to top, specifically includes:
[0014] A first photoresist layer is coated on the epitaxial layer, wherein the thickness ratio of the first photoresist layer to the epitaxial layer is 0.55:1 to 0.65:1, and the viscosity of the first photoresist layer is 300 CPS to 400 CPS.
[0015] A second photoresist layer is coated on the first photoresist layer, the thickness ratio of the second photoresist layer to the epitaxial layer is 0.4:1 to 0.5:1, and the viscosity of the second photoresist layer is 200 CPS to 260 CPS.
[0016] A third photoresist layer is coated on the second photoresist layer, wherein the thickness ratio of the third photoresist layer to the epitaxial layer is 0.25:1 to 0.35:1, and the viscosity of the third photoresist layer is 100 CPS to 140 CPS.
[0017] A fourth photoresist layer is coated on the third photoresist layer. The thickness ratio of the fourth photoresist layer to the epitaxial layer is 0.1:1 to 0.2:1, and the viscosity of the fourth photoresist layer is 40 CPS to 60 CPS. The first photoresist layer, the second photoresist layer, the third photoresist layer, and the fourth photoresist layer constitute the photoresist composite layer.
[0018] Furthermore, the step of forming a first opening groove penetrating the photoresist composite layer and having an inner wall of a first arc surface on the photoresist composite layer, so as to form a second opening groove penetrating the epitaxial layer and having an inner wall of a second arc surface on the epitaxial layer by an etching process, includes:
[0019] A portion of the photoresist composite layer is exposed and developed, and the exposed and developed photoresist composite layer is baked at a preset temperature and for a preset time to form a first opening groove that penetrates the photoresist composite layer and has a first arc surface on its inner wall.
[0020] The epitaxial layer coated with the photoresist composite layer is subjected to inductively coupled plasma etching to form a second opening groove on the epitaxial layer that penetrates the epitaxial layer and has an inner wall that is a second arc surface;
[0021] Remove the first photoresist layer remaining on the side of the epitaxial layer facing away from the substrate.
[0022] Furthermore, the step of performing inductively coupled plasma etching on the epitaxial layer coated with the photoresist composite layer to form a second opening groove penetrating the epitaxial layer and having an inner wall of a second arc surface specifically includes:
[0023] Ar gas is introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm, and the radio frequency power of the upper radio frequency is controlled at 1000W to 1200W for 5S to 10S to ionize the Ar gas. BCl3 gas is then introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm for 5S to 10S to complete the ionization of the BCl3 gas, so that B atoms are adsorbed on the inner wall of the first open groove.
[0024] Cl2 and O2 are simultaneously introduced into the reaction chamber and maintained for 5 to 10 seconds. The flow rate of Cl2 is 150 to 200 Sccm and the flow rate of O2 is 5 to 8 Sccm. The lower radio frequency is turned on, and the radio frequency power of the lower radio frequency is 600 W to 800 W, so as to form a second opening groove with an inner wall of a second arc surface on the epitaxial layer until the second opening groove penetrates the epitaxial layer.
[0025] The lower radio frequency is turned off, and the supply of Ar, BCl3, Cl2 and O2 to the reaction chamber is stopped. N2 is then introduced into the reaction chamber and maintained for 30 to 60 seconds. After that, the supply of N2 is stopped, and the upper radio frequency is turned off.
[0026] Furthermore, the step of depositing a first insulating protective layer on the epitaxial layer covering the second arcuate surface includes:
[0027] A SiO2 thin film is deposited on the epitaxial layer;
[0028] A fifth photoresist layer is coated on the SiO2 thin film, and a portion of the fifth photoresist layer is exposed and developed to form a first open region and a second open region on the SiO2 thin film. The first open region is located on the side of the epitaxial sublayer facing away from the substrate, and the second open region is located at the bottom of the second opening groove.
[0029] The SiO2 thin film located in the first open region and the second open region is etched by SiO2 etching solution;
[0030] The remaining fifth photoresist layer is removed, and the remaining SiO2 film forms a first insulating protective layer. The first insulating protective layer is disposed on the second arc surface, with one end of the first insulating protective layer abutting the substrate and the other end of the first insulating protective layer placed on the side edge of the epitaxial sublayer facing away from the substrate.
[0031] Furthermore, the step of depositing a SiO2 thin film on the epitaxial layer includes:
[0032] A first flow rate of N2 is introduced into the reaction chamber, the radio frequency is turned on with a first power, and then the radio frequency is turned off after a first time to clean the reaction chamber.
[0033] The reaction chamber is evacuated, and N2 at a second flow rate is introduced into the reaction chamber.
[0034] A mixed gas, comprising SiH4 and N2O, is introduced into the reaction chamber, and the radio frequency is turned on with a second power to deposit a SiO2 thin film on the epitaxial layer.
[0035] After a second period of time, the power of the radio frequency is adjusted to a third power, and the introduction of N2O is stopped to remove the dangling bonds of O on the surface of the SiO2 thin film.
[0036] Furthermore, the step of depositing an Ag reflector on the epitaxial layer, with a portion of the Ag reflector covering the first insulating protective layer, includes:
[0037] A first positive photoresist is coated on the epitaxial layer, and a first exposure is performed through a first photolithography plate. A negative photoresist is coated on the first positive photoresist after the first exposure, and a second exposure is performed through a second photolithography plate. A second positive photoresist is coated on the negative photoresist after the second exposure, and a third exposure is performed through a third photolithography plate.
[0038] After development, a fifth photoresist layer, a sixth photoresist layer, and a seventh photoresist layer are formed on the epitaxial sublayer in sequence from bottom to top. The end of the fifth photoresist layer facing the epitaxial sublayer is placed in the accommodating space, and a hollow portion is formed between the fifth photoresist layer and the first insulating protective layer.
[0039] The epitaxial layer is placed in a plating pan, and Ag metal is used as a target for Ag metal thin film evaporation. An acute angle is formed between the plating pan and the horizontal plane where the target is located, so that the target enters the cutout. Part of the Ag metal thin film is placed on the side of the seventh photoresist layer that is away from the substrate, and the remaining Ag metal thin film is placed on the epitaxial layer.
[0040] The substrate is heated to soften the fifth, sixth, and seventh photoresist layers and cover one end of the Ag metal film located on the epitaxial layer.
[0041] After removing the Ag metal film on the side of the seventh photoresist layer facing away from the substrate using a blue film stripping process, the fifth, sixth, and seventh photoresist layers are removed. The Ag metal film located on the epitaxial layer forms the Ag mirror, and part of the Ag mirror is covered on the first insulating protective layer.
[0042] Furthermore, the width of the fifth photoresist layer is smaller than the width of the sixth photoresist layer, the width of the sixth photoresist layer is equal to the width of the seventh photoresist layer, the viscosity of the fifth photoresist layer is 30 CPS to 50 CPS, the viscosity of the sixth photoresist layer is 200 CPS to 240 CPS, the viscosity of the seventh photoresist layer is 150 CPS to 200 CPS, the thickness ratio of the fifth photoresist layer to the Ag mirror is 2:1 to 10:1, the thickness ratio of the sixth photoresist layer to the fifth photoresist layer is 5:1 to 10:1, and the thickness ratio of the seventh photoresist layer to the sixth photoresist layer is 1.5:1 to 3:1.
[0043] Furthermore, the energy of the single exposure is 200 mJ / cm². 2 ~230mj / cm 2 The energy of the second exposure is 300 mJ / cm. 2 ~350mj / cm 2The energy of the three exposures was 250 mJ / cm². 2 ~300mj / cm 2 The first exposure time is 0.4S to 0.6S, the second exposure time is 0.6S to 0.8S, and the third exposure time is 0.8S to 1.0S. The wavelength of the light in the third exposure is greater than the wavelength of the light in the second exposure.
[0044] Furthermore, after the step of depositing an Ag reflector on the epitaxial layer and partially covering the first insulating protective layer with the Ag reflector, the method further includes:
[0045] A second insulating protective layer, an N-type conductive layer, a third insulating protective layer, an N-type pad, and a P-type pad are sequentially disposed on the epitaxial layer. The N-type pad is electrically connected to the N-type conductive layer, and the P-type pad is electrically connected to the Ag reflector. Attached Figure Description
[0046] Figure 1 This is a flowchart of the method for fabricating a matrix LED chip in an embodiment of the present invention;
[0047] Figure 2 This is a structural diagram of the first opening groove after it has been prepared in the method for preparing a matrix LED chip according to an embodiment of the present invention;
[0048] Figure 3 This is a structural diagram of the second opening groove after it has been prepared in the method for preparing a matrix LED chip according to an embodiment of the present invention;
[0049] Figure 4 This is a structural diagram showing the structure after the residual first photoresist layer is removed in the fabrication method of the matrix LED chip in this embodiment of the invention.
[0050] Figure 5 This is a structural diagram of the first insulating protective layer after its preparation in the matrix LED chip fabrication method of this invention.
[0051] Figure 6 This is a structural diagram of the fifth, sixth, and seventh photoresist layers after they have been prepared in the matrix LED chip fabrication method of this embodiment of the invention.
[0052] Figure 7 This is a structural diagram of the Ag metal thin film after evaporation in the fabrication method of the matrix LED chip in this embodiment of the invention;
[0053] Figure 8 This is a structural diagram of the Ag reflector after its fabrication in the matrix LED chip fabrication method of this invention.
[0054] Figure 9This is a structural diagram of the completed epitaxial recess in the fabrication method of the matrix LED chip in this embodiment of the invention;
[0055] Figure 10 This is a structural diagram of the second insulating protective layer after its fabrication is completed in the method for fabricating a matrix LED chip according to an embodiment of the present invention;
[0056] Figure 11 This is a structural diagram of the matrix LED chip fabrication method in this embodiment of the invention after the N-type conductive layer is fabricated.
[0057] Figure 12 This is a structural diagram of the third insulating protective layer after its fabrication is completed in the method for fabricating a matrix LED chip according to an embodiment of the present invention.
[0058] Figure 13 This is a structural diagram of the matrix LED chip fabrication method in this embodiment of the invention after the N-type and P-type pads are fabricated.
[0059] Explanation of key component symbols:
[0060] 10. Substrate; 111. N-type semiconductor layer; 112. Active light-emitting layer; 113. P-type semiconductor layer; 114. Second opening trench; 115. Epitaxial recess; 121. First photoresist layer; 122. Second photoresist layer; 123. Third photoresist layer; 124. Fourth photoresist layer; 125. First opening trench; 13. First insulating protective layer; 141. Fifth photoresist layer; 142. Sixth photoresist layer; 143. Seventh photoresist layer; 15. Ag reflector; 16. Second insulating protective layer; 17. N-type conductive layer; 18. Third insulating protective layer; 181. N-type via; 182. P-type via; 191. N-type pad; 192. P-type pad.
[0061] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation
[0062] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.
[0063] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0064] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0065] Please see Figure 1 The method for fabricating a matrix LED chip in this embodiment of the invention includes the following steps:
[0066] S10: Provide a substrate for growth, and deposit an epitaxial layer on the substrate;
[0067] The epitaxial layer is fabricated on the substrate 10 using an MOCVD process. The epitaxial layer includes an N-type semiconductor layer 111, an active light-emitting layer 112, and a P-type semiconductor layer 113 arranged sequentially from bottom to top. That is, the N-type semiconductor layer 111, the active light-emitting layer 112, and the P-type semiconductor layer 113 are deposited sequentially on the epitaxial layer to form the epitaxial layer.
[0068] S20: A photoresist composite layer is coated on the epitaxial layer. The photoresist composite layer includes a first photoresist layer, a second photoresist layer, a third photoresist layer, and a fourth photoresist layer, which are arranged sequentially from bottom to top and whose thickness and viscosity decrease sequentially from bottom to top.
[0069] Specifically, step S20 includes:
[0070] S210: A first photoresist layer is coated on the epitaxial layer, wherein the thickness ratio of the first photoresist layer to the epitaxial layer is 0.55:1 to 0.65:1, and the viscosity of the first photoresist layer is 300 CPS to 400 CPS;
[0071] S220: A second photoresist layer is coated on the first photoresist layer, wherein the thickness ratio of the second photoresist layer to the epitaxial layer is 0.4:1 to 0.5:1, and the viscosity of the second photoresist layer is 200 CPS to 260 CPS;
[0072] S230: A third photoresist layer is coated on the second photoresist layer, wherein the thickness ratio of the third photoresist layer to the epitaxial layer is 0.25:1 to 0.35:1, and the viscosity of the third photoresist layer is 100 CPS to 140 CPS;
[0073] S240: A fourth photoresist layer is coated on the third photoresist layer, wherein the thickness ratio of the fourth photoresist layer to the thickness of the epitaxial layer is 0.1:1 to 0.2:1, and the viscosity of the fourth photoresist layer is 40 CPS to 60 CPS. The first photoresist layer, the second photoresist layer, the third photoresist layer, and the fourth photoresist layer constitute the photoresist composite layer.
[0074] Understandably, the thickness ratio of the photoresist composite layer to the epitaxial layer is 1.3:1 to 1.7:1. By making the thickness of the photoresist composite layer greater than the thickness of the epitaxial layer, a portion of the first photoresist layer 121 will remain on the side of the epitaxial layer facing away from the substrate 10 after subsequent etching of the epitaxial layer, thus avoiding surface damage to the epitaxial layer caused by etching.
[0075] S30: A first opening groove is formed on the photoresist composite layer, penetrating the photoresist composite layer and having an inner wall of a first arc surface, so as to form a second opening groove on the epitaxial layer through the etching process, penetrating the epitaxial layer and having an inner wall of a second arc surface, and a plurality of second opening grooves divide the epitaxial layer into a plurality of epitaxial sublayers.
[0076] Please see Figures 2 to 4 Step S30 includes:
[0077] S310: Expose and develop a portion of the photoresist composite layer, and bake the exposed and developed photoresist composite layer at a preset temperature and a preset time to form a first opening groove that penetrates the photoresist composite layer and has a first arc surface on its inner wall.
[0078] Exposure of a portion of the photoresist composite layer provides a positioning basis for the first opening groove 125. After development with a developer, the exposure position forms the first opening groove 125. It can be understood that, through exposure and development alone, the inner wall of the first opening groove 125 is perpendicular to the epitaxial layer.
[0079] The substrate 10 is heated and baked using a hot plate to achieve the purpose of baking the photoresist composite layer. Preferably, the preset temperature is 80℃~100℃ and the preset time is 5min~7min. In this embodiment, the preset temperature is 90℃ and the preset time is 6min. After baking, the first photoresist layer 121 can form a first angle between the sidewall of the first opening groove 125 and the bottom of the photoresist composite layer; the second photoresist layer 122 can form a second angle between the sidewall of the first opening groove 125 and the bottom of the photoresist composite layer; the third photoresist layer 123 can form a third angle between the sidewall of the first opening groove 125 and the bottom of the photoresist composite layer; and the fourth photoresist layer 124 can form a fourth angle between the sidewall of the first opening groove 125 and the bottom of the photoresist composite layer. It can be understood that the first angle, the second angle, and the third angle are all formed by the same angle. The first angle and the fourth included angle are both acute angles. Since the thickness and viscosity of the first photoresist layer 121, the second photoresist layer 122, the third photoresist layer 123 and the fourth photoresist layer 124 decrease sequentially, the angles of the first included angle, the second included angle, the third included angle and the fourth included angle can gradually decrease. Through the parameter settings in step S20, in this embodiment, the first included angle is 60° to 70°, the second included angle is 40° to 50°, the third included angle is 20° to 30°, and the fourth included angle is 10° to 15°, thereby forming the first arc surface on the inner wall of the first opening groove 125.
[0080] S320: Perform inductively coupled plasma etching on the epitaxial layer coated with the photoresist composite layer to form a second opening groove on the epitaxial layer that penetrates the epitaxial layer and has an inner wall that is a second arc surface;
[0081] Because the first opening groove 125 penetrating the photoresist composite layer is provided on the photoresist composite layer, during the etching process, the exposed epitaxial layer and the photoresist composite layer are etched simultaneously, thereby replicating the first opening groove 125 to the epitaxial layer to form the second opening groove 114.
[0082] Specifically, Ar gas is introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm, and the radio frequency power of the upper radio frequency is controlled at 1000W to 1200W for 5S to 10S to ionize the Ar gas. BCl3 gas is then introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm for 5S to 10S to complete the ionization of the BCl3 gas, so that B atoms are adsorbed on the inner wall of the first opening groove 125 to protect its morphology and prevent deformation of the inner wall of the first opening groove 125 during the etching process.
[0083] Cl2 and O2 are simultaneously introduced into the reaction chamber and maintained for 5 to 10 seconds. The flow rate ratio of Cl2 to O2 is 30:1 to 40:1, that is, the flow rate of Cl2 is 150 Sccm to 200 Sccm and the flow rate of O2 is 5 Sccm to 8 Sccm. The lower radio frequency is turned on, and the radio frequency power of the lower radio frequency is 600W to 800W, so as to form the second opening groove 114 with the inner wall of the second arc surface on the epitaxial layer until the second opening groove 114 penetrates the epitaxial layer.
[0084] The lower radio frequency is turned off, and the flow of Ar, BCl3, Cl2, and O2 into the reaction chamber is stopped. N2 is then introduced into the reaction chamber and maintained for 30-60 seconds before the N2 flow is stopped, and the upper radio frequency is turned off. This process utilizes the upper radio frequency to ionize N2, thereby cleaning the surface of the remaining photoresist composite layer and facilitating subsequent removal of the remaining photoresist composite layer. Understandably, due to thickness control of the photoresist composite layer, after etching, only a portion of the first photoresist layer 121 remains on the side of the epitaxial layer facing away from the substrate 10.
[0085] S330: Remove the first photoresist layer remaining on the side of the epitaxial layer facing away from the substrate.
[0086] The residual first photoresist layer 121 is removed by using one or a mixture of alcohols, phenols, benzenes, and esters at a temperature of 80℃ to 90℃.
[0087] S40: A first insulating protective layer is deposited on the epitaxial layer and covered on the second arc surface, wherein the end of the first insulating protective layer away from the substrate encloses a receiving space on the side of the epitaxial sublayer facing away from the substrate;
[0088] Please see Figure 5 Step S40 includes:
[0089] S410: Deposit a SiO2 thin film on the epitaxial layer;
[0090] Specifically, a first flow rate of N2 is introduced into the reaction chamber, the radio frequency is turned on with a first power, and after a first time, the radio frequency is turned off to clean the reaction chamber;
[0091] Preferably, the first flow rate is 200 Sccm to 300 Sccm, the first power is 30W to 60W, and the first time is 30S to 60S. In this embodiment, the first flow rate is 260 Sccm, the first power is 50W, and the first time is 40S.
[0092] The reaction chamber is evacuated, and N2 at a second flow rate is introduced into the reaction chamber.
[0093] Preferably, the pressure in the reaction chamber is 120 Pa to 180 Pa, and the second flow rate is 1500 Sccm to 2000 Sccm. In this embodiment, the pressure in the reaction chamber is 150 Pa, and the second flow rate is 1800 Sccm.
[0094] A mixed gas, comprising SiH4 and N2O, is introduced into the reaction chamber, and the radio frequency is turned on with a second power to deposit a SiO2 thin film on the epitaxial layer.
[0095] Preferably, the second power is 90W to 120W. In this embodiment, the second power is 100W.
[0096] After a second period of time, the power of the radio frequency is adjusted to a third power, and the introduction of N2O is stopped to remove the dangling bonds of O on the surface of the SiO2 thin film.
[0097] The introduction time of the mixed gas is set according to the thickness of the SiO2 film. The longer the second time lasts, the thicker the SiO2 film becomes. Preferably, the third power is 30W to 60W; in this embodiment, the third power is 50W. Stopping the introduction of N2O, i.e., at the third power, only introduces SiH4. The ionized Si atoms react with the dangling bonds of O on the surface of the SiO2 film, avoiding subsequent oxidation residues of the O dangling bonds, which would affect the reflectivity of the Ag reflector 15.
[0098] S420: A fifth photoresist layer is coated on the SiO2 thin film, and a portion of the fifth photoresist layer is exposed and developed to form a first open region and a second open region on the SiO2 thin film. The first open region is located on the side of the epitaxial sublayer facing away from the substrate, and the second open region is located at the bottom of the second opening groove.
[0099] The purpose of coating the fifth photoresist layer 141 is to protect a portion of the SiO2 film, making it easier to remove the SiO2 film from the first open region and the second open region.
[0100] S430: Etching the SiO2 film located in the first open region and the second open region by SiO2 etching solution;
[0101] S440: Remove the remaining fifth photoresist layer, and the remaining SiO2 film forms a first insulating protective layer. The first insulating protective layer is disposed on the second arc surface, and one end of the first insulating protective layer abuts against the substrate, and the other end of the first insulating protective layer is placed on the side edge of the epitaxial sublayer facing away from the substrate.
[0102] Understandably, part of the first insulating protective layer 13 is located within the first opening groove 125, and part of the first insulating protective layer 13 is located on the epitaxial sublayer.
[0103] S50: An Ag reflector is deposited on the epitaxial layer, and a portion of the Ag reflector is covered on the first insulating protective layer;
[0104] Please see Figures 6 to 8 Step S50 specifically includes:
[0105] S510: A first positive photoresist is coated on the epitaxial layer, and a first exposure is performed through a first photolithography plate. A negative photoresist is coated on the first positive photoresist after the first exposure, and a second exposure is performed through a second photolithography plate. A second positive photoresist is coated on the negative photoresist after the second exposure, and a third exposure is performed through a third photolithography plate.
[0106] S520: After developing the substrate, a fifth photoresist layer, a sixth photoresist layer, and a seventh photoresist layer are formed on the epitaxial sublayer in sequence from bottom to top. The end of the fifth photoresist layer facing the epitaxial sublayer is placed in the accommodating space, and a hollow portion is formed between the fifth photoresist layer and the first insulating protective layer.
[0107] The width of the fifth photoresist layer 141 is smaller than the width of the sixth photoresist layer 142, and the width of the sixth photoresist layer 142 is equal to the width of the seventh photoresist layer 143. The viscosity of the fifth photoresist layer 141 is 30 CPS to 50 CPS, the viscosity of the sixth photoresist layer 142 is 200 CPS to 240 CPS, and the viscosity of the seventh photoresist layer 143 is 150 CPS to 200 CPS. The thickness ratio of the fifth photoresist layer 141 to the Ag mirror 15 is 2:1 to 10:1, the thickness ratio of the sixth photoresist layer 142 to the fifth photoresist layer 141 is 5:1 to 10:1, and the thickness ratio of the seventh photoresist layer 143 to the sixth photoresist layer 142 is 1.5:1 to 3:1.
[0108] Understandably, the distance between the light-transmitting area of the first photoresist and the distance between the opaque area of the second photoresist are greater than the distance between the light-blocking areas of the third photoresist, and the distance between the light-transmitting areas of the third photoresist is equal to the distance between the opaque areas of the second photoresist, so that the opening spacing of the first positive photoresist is greater than the opening spacing of the negative photoresist, and the opening spacing of the second positive photoresist is equal to the opening spacing of the negative photoresist, thereby completing the width control between the fifth photoresist layer 141, the sixth photoresist layer 142 and the seventh photoresist layer 143. At the same time, the cutout portion can be formed between the fifth photoresist layer 141 and the first insulating protective layer 13.
[0109] The energy of the single exposure was 200 mJ / cm². 2 ~230mj / cm 2 The energy of the second exposure is 300 mJ / cm. 2 ~350mj / cm 2 The energy of the three exposures was 250 mJ / cm². 2 ~300mj / cm 2 The first exposure time is 0.4S to 0.6S, the second exposure time is 0.6S to 0.8S, and the third exposure time is 0.8S to 1.0S. The wavelength of the light used in the third exposure is longer than that used in the second exposure. By controlling the exposure energy, exposure time, and exposure light wavelength, damage to the negative photoresist during the third exposure can be avoided, thus preventing incomplete development.
[0110] S530: The epitaxial layer is placed in a plating pan, and Ag metal thin film is deposited using Ag metal as a target. An acute angle is formed between the plating pan and the horizontal plane where the target is located, so that the target enters the cutout. Part of the Ag metal thin film is placed on the side of the seventh photoresist layer that is away from the substrate, and the remaining Ag metal thin film is placed on the epitaxial layer.
[0111] Preferably, the acute angle is 30° to 60°, and in this embodiment, the acute angle is 50°.
[0112] During the vapor deposition process, the plating pot revolves around the center of the machine platform and rotates on its own axis around the center, with the directions of revolution and rotation being the same. For every increase in the thickness of the Ag metal film by a first thickness, the directions of revolution and rotation change simultaneously. In this embodiment, the first thickness is... By repeatedly adjusting the revolution and rotation directions of the plating pan, the uniformity of the Ag metal film thickness can be reduced, ensuring that the uniformity of the Ag metal film thickness is less than 5%.
[0113] S540: Heat the substrate to soften the fifth, sixth, and seventh photoresist layers and cover one end of the Ag metal film located on the epitaxial layer;
[0114] The substrate 10 is placed on a hot plate and heated. Due to the control of the viscosity and thickness of the fifth photoresist layer 141, the sixth photoresist layer 142 and the seventh photoresist layer 143, after heating, they will soften into an arched shape that gradually diffuses outward, thereby covering the Ag metal film located at the hollow part.
[0115] S550: After removing the Ag metal film on the side of the seventh photoresist layer facing away from the substrate by the blue film stripping process, the fifth photoresist layer, the sixth photoresist layer and the seventh photoresist layer are removed. The Ag metal film on the epitaxial layer forms the Ag mirror, and part of the Ag mirror is covered on the first insulating protective layer.
[0116] Understandably, the Ag reflector 15 is the Ag metal thin film. Preferably, the thickness of the Ag reflector 15 is... In this embodiment, the thickness of the Ag reflector 15 is By controlling the thickness of the Ag reflector 15, production costs can be controlled while ensuring that the reflectivity of the Ag reflector 15 is greater than that of the Ag metal itself.
[0117] One end of the Ag reflector 15 is placed within the accommodating space of a certain epitaxial sublayer, and the other end of the Ag reflector 15 extends from the epitaxial sublayer toward an adjacent epitaxial sublayer and is placed within the accommodating space of the adjacent epitaxial sublayer. It can be understood that, for a certain epitaxial sublayer, the Ag reflector 15 forms a fabricated portion on the side of the epitaxial sublayer facing away from the substrate 10, and the fabricated portion, together with the cutout portion, forms the accommodating space.
[0118] By setting a first photoresist layer 121, a second photoresist layer 122, a third photoresist layer 123, and a fourth photoresist layer 124 with decreasing thickness and viscosity, a first opening groove 125 with the inner wall of the first arc surface can be formed on the photoresist composite layer stacked together by photolithography. Then, the first opening groove 125 is copied to the epitaxial layer by etching, and a second opening groove 114 with the inner wall of the second arc surface is formed on the epitaxial layer. When the epitaxial layer emits light, its lateral light emission can be diffused through the second arc surface. Through the Ag reflector 15 covering the first insulating layer, when the lateral light emission of the epitaxial layer is diffused along the second arc surface, it can be reflected by the Ag reflector 15, thereby converting the light into vertical light, effectively converging the emission angle, reducing lateral light emission, improving the luminous efficiency of vertical light emission, and thus improving the light emission performance of the LED chip.
[0119] Preferably, the matrix LED chip fabrication method further includes:
[0120] S60: A second insulating protective layer, an N-type conductive layer, a third insulating protective layer, an N-type pad, and a P-type pad are sequentially disposed on the epitaxial layer. The N-type pad is electrically connected to the N-type conductive layer, and the P-type pad is electrically connected to the Ag reflector.
[0121] The overall structure can be fabricated by setting the second insulating protective layer 16, the N-type conductive layer 17, the third insulating protective layer 18, the N-type pad 191, and the P-type pad 192.
[0122] Please see Figures 9 to 13 Step S60 includes:
[0123] S610: An epitaxial recess is etched on the side of the epitaxial sublayer facing away from the substrate, and the bottom of the epitaxial recess is connected to the N-type semiconductor layer;
[0124] An eighth photoresist layer is coated on the epitaxial layer, and the eighth photoresist layer is exposed and developed to expose a portion of the P-type semiconductor layer 113 on the epitaxial sublayer. Then, the epitaxial recess 115 is formed by etching.
[0125] S620: A second insulating protective layer is provided on the epitaxial layer, and the second insulating protective layer forms a first opening at the epitaxial recess;
[0126] A first SiO2 protective film is deposited on the epitaxial layer using a vapor deposition process. SiH4 and N2O are then reacted using a PECVD process to form a second SiO2 protective film. The first and second SiO2 protective films constitute the second insulating protective layer 16, which, as understood, covers the Ag reflector 15. The thickness of the second SiO2 protective film is greater than the thickness of the first SiO2 protective film. Preferably, the thickness of the second SiO2 protective film is [missing information]. The thickness of the first SiO2 protective film is In this embodiment, the thickness of the first SiO2 protective film is The thickness of the second SiO2 protective film is Because O ions are involved when the second SiO2 protective film is deposited by PECVD, it will cause the Ag reflector 15 to oxidize, thereby reducing the reflectivity. Therefore, by first evaporating the first SiO2 protective film, the direct deposition can avoid affecting the reflectivity of the Ag reflector 15. However, the first SiO2 protective film formed by evaporation has poor protection for the epitaxial recess 115. By setting the second SiO2 protective film, the coverage of the epitaxial recess 115 by the second insulating protective layer 16 is ensured.
[0127] By coating a ninth photoresist layer on the side of the second insulating protective layer 16 facing away from the substrate 10, and then forming the first opening through exposure and development, it can be understood that the N-type semiconductor layer 111 communicates with the outside through the first opening and the epitaxial recess 115.
[0128] S630: An N-type conductive layer electrically connected to the N-type semiconductor layer 111 is deposited on the second insulating layer by vapor deposition;
[0129] The N-type conductive layer 17 is formed by sequentially depositing Cr, Al, Ti, Ni, Au, Ti, Pt, Ti, Pt, Ti, Pt, and Ti metals using an electron beam evaporation process. One end of the N-type conductive layer 17 is placed on the side of a certain epitaxial sublayer facing away from the substrate 10, and the other end of the N-type conductive layer 17 passes through the epitaxial recess 115 and the second opening groove 114 on the epitaxial sublayer, and is placed on the side edge of the adjacent epitaxial sublayer facing away from the substrate 10. That is, the N-type conductive layer 17 is electrically connected to the N-type semiconductor layer 111 through the first opening, and two adjacent epitaxial sublayers are connected in parallel through the N-type conductive layer 17.
[0130] S640: A third insulating protective layer is provided on the epitaxial layer, wherein the third insulating protective layer forms N-type through holes and P-type through holes at two adjacent second opening slots, respectively;
[0131] A plurality of periodic structures are formed on the epitaxial layer. Each periodic structure includes a sequentially deposited Al₂O₃ thin film and a third SiO₂ protective film. These periodic structures form the third insulating protective layer 18. Preferably, the third insulating protective layer 18 includes 3 to 5 of the periodic structures. The third insulating protective layer 18 is used to prevent the chip from being contaminated or oxidized by the external environment. Understandably, the third insulating protective layer 18 covers the N-type conductive layer 17 and the second insulating protective layer 16.
[0132] A tenth photoresist layer is coated on the side of the third insulating layer facing away from the substrate 10. Through exposure and development, the N-type via 181 and the P-type via 182 are formed. The N-type via 181 is located at one of its second opening slots 114 and communicates with the N-type conductive layer 17. The P-type via 182 is located at another second opening slot 114 adjacent to its second opening slot 114. The second insulating protective layer 16 is removed at the other second opening slot 114 by an etching process, so that the P-type via 182 communicates with the Ag reflector 15.
[0133] S650: An N-type pad electrically connected to the N-type conductive layer is provided at the N-type through-hole, and a P-type pad electrically connected to the Ag reflector is provided at the P-type through-hole.
[0134] This completes the fabrication of the matrix LED chip.
[0135] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0136] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.
Claims
1. A method for fabricating a matrix-type LED chip, characterized in that, Includes the following steps: Provide a substrate for growth, and deposit an epitaxial layer on the substrate; A photoresist composite layer is coated on the epitaxial layer. The photoresist composite layer includes a first photoresist layer, a second photoresist layer, a third photoresist layer, and a fourth photoresist layer, which are arranged sequentially from bottom to top and whose thickness and viscosity decrease sequentially from bottom to top. The step of coating a photoresist composite layer on the epitaxial layer, wherein the photoresist composite layer comprises a first photoresist layer, a second photoresist layer, a third photoresist layer, and a fourth photoresist layer arranged sequentially from bottom to top, with their thickness and viscosity decreasing sequentially from bottom to top, specifically includes: A first photoresist layer is coated on the epitaxial layer, wherein the thickness ratio of the first photoresist layer to the epitaxial layer is 0.55:1 to 0.65:1, and the viscosity of the first photoresist layer is 300 CPS to 400 CPS. A second photoresist layer is coated on the first photoresist layer, the thickness ratio of the second photoresist layer to the epitaxial layer is 0.4:1 to 0.5:1, and the viscosity of the second photoresist layer is 200 CPS to 260 CPS. A third photoresist layer is coated on the second photoresist layer, wherein the thickness ratio of the third photoresist layer to the epitaxial layer is 0.25:1 to 0.35:1, and the viscosity of the third photoresist layer is 100 CPS to 140 CPS. A fourth photoresist layer is coated on the third photoresist layer. The thickness ratio of the fourth photoresist layer to the epitaxial layer is 0.1:1 to 0.2:1, and the viscosity of the fourth photoresist layer is 40 CPS to 60 CPS. The first photoresist layer, the second photoresist layer, the third photoresist layer, and the fourth photoresist layer constitute the photoresist composite layer. A first opening groove is formed on the photoresist composite layer, penetrating the photoresist composite layer and having an inner wall of a first arc surface, so as to form a second opening groove on the epitaxial layer through the etching process, penetrating the epitaxial layer and having an inner wall of a second arc surface. A plurality of second opening grooves divide the epitaxial layer into a plurality of epitaxial sublayers. A first insulating protective layer is deposited on the epitaxial layer and covered on the second arc surface. The end of the first insulating protective layer away from the substrate encloses a accommodating space on the side of the epitaxial sublayer facing away from the substrate. An Ag reflector is deposited on the epitaxial layer, and a portion of the Ag reflector is disposed on the first insulating protective layer; The step of depositing an Ag reflector on the epitaxial layer, with a portion of the Ag reflector covering the first insulating protective layer, includes: A first positive photoresist is coated on the epitaxial layer, and a first exposure is performed through a first photolithography plate. A negative photoresist is coated on the first positive photoresist after the first exposure, and a second exposure is performed through a second photolithography plate. A second positive photoresist is coated on the negative photoresist after the second exposure, and a third exposure is performed through a third photolithography plate. After development, a fifth photoresist layer, a sixth photoresist layer, and a seventh photoresist layer are formed on the epitaxial sublayer in sequence from bottom to top. The end of the fifth photoresist layer facing the epitaxial sublayer is placed in the accommodating space, and a hollow portion is formed between the fifth photoresist layer and the first insulating protective layer. The epitaxial layer is placed in a plating pan, and Ag metal is used as a target for Ag metal thin film evaporation. An acute angle is formed between the plating pan and the horizontal plane where the target is located, so that the target enters the cutout. Part of the Ag metal thin film is placed on the side of the seventh photoresist layer that is away from the substrate, and the remaining Ag metal thin film is placed on the epitaxial layer. The substrate is heated to soften the fifth, sixth, and seventh photoresist layers and cover one end of the Ag metal film located on the epitaxial layer; After removing the Ag metal film on the side of the seventh photoresist layer facing away from the substrate using a blue film stripping process, the fifth, sixth, and seventh photoresist layers are removed. The Ag metal film located on the epitaxial layer forms the Ag mirror, and part of the Ag mirror is covered on the first insulating protective layer.
2. The method for fabricating a matrix LED chip according to claim 1, characterized in that, The step of forming a first opening groove penetrating the photoresist composite layer and having an inner wall of a first arc surface on the photoresist composite layer, and forming a second opening groove penetrating the epitaxial layer and having an inner wall of a second arc surface on the epitaxial layer by an etching process, includes: A portion of the photoresist composite layer is exposed and developed, and the exposed and developed photoresist composite layer is baked at a preset temperature and for a preset time to form a first opening groove that penetrates the photoresist composite layer and has a first arc surface on its inner wall. The epitaxial layer coated with the photoresist composite layer is subjected to inductively coupled plasma etching to form a second opening groove on the epitaxial layer that penetrates the epitaxial layer and has an inner wall that is a second arc surface; Remove the first photoresist layer remaining on the side of the epitaxial layer facing away from the substrate.
3. The method for fabricating a matrix LED chip according to claim 2, characterized in that, The step of performing inductively coupled plasma etching on the epitaxial layer coated with the photoresist composite layer to form a second opening groove penetrating the epitaxial layer and having an inner wall of a second arc surface specifically includes: Ar gas is introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm, and the radio frequency power of the upper radio frequency is controlled at 1000W to 1200W for 5S to 10S to ionize the Ar gas. BCl3 gas is then introduced into the reaction chamber at a flow rate of 20 Sccm to 30 Sccm for 5S to 10S to complete the ionization of the BCl3 gas, so that B atoms are adsorbed on the inner wall of the first open groove. Cl2 and O2 are simultaneously introduced into the reaction chamber and maintained for 5 to 10 seconds. The flow rate of Cl2 is 150 to 200 Sccm and the flow rate of O2 is 5 to 8 Sccm. The lower radio frequency is turned on, and the radio frequency power of the lower radio frequency is 600 W to 800 W, so as to form a second opening groove with an inner wall of a second arc surface on the epitaxial layer until the second opening groove penetrates the epitaxial layer. The lower radio frequency is turned off, and the supply of Ar, BCl3, Cl2 and O2 to the reaction chamber is stopped. N2 is then introduced into the reaction chamber and maintained for 30 to 60 seconds. After that, the supply of N2 is stopped, and the upper radio frequency is turned off.
4. The method for fabricating a matrix LED chip according to claim 1, characterized in that, The step of depositing a first insulating protective layer on the epitaxial layer and covering the second arcuate surface includes: A SiO2 thin film is deposited on the epitaxial layer; A fifth photoresist layer is coated on the SiO2 thin film, and a portion of the fifth photoresist layer is exposed and developed to form a first open region and a second open region on the SiO2 thin film. The first open region is located on the side of the epitaxial sublayer facing away from the substrate, and the second open region is located at the bottom of the second opening groove. The SiO2 thin film located in the first open region and the second open region is etched by SiO2 etching solution; The remaining fifth photoresist layer is removed, and the remaining SiO2 film forms a first insulating protective layer. The first insulating protective layer is disposed on the second arc surface, with one end of the first insulating protective layer abutting the substrate and the other end of the first insulating protective layer placed on the side edge of the epitaxial sublayer facing away from the substrate.
5. The method for fabricating a matrix LED chip according to claim 4, characterized in that, The step of depositing a SiO2 thin film on the epitaxial layer includes: A first flow rate of N2 is introduced into the reaction chamber, the radio frequency is turned on with a first power, and then the radio frequency is turned off after a first time to clean the reaction chamber. The reaction chamber is evacuated, and N2 at a second flow rate is introduced into the reaction chamber. A mixed gas, comprising SiH4 and N2O, is introduced into the reaction chamber, and the radio frequency is turned on with a second power to deposit a SiO2 thin film on the epitaxial layer. After a second period of time, the power of the radio frequency is adjusted to a third power, and the introduction of N2O is stopped to remove the dangling bonds of O on the surface of the SiO2 thin film.
6. The method for fabricating a matrix LED chip according to claim 1, characterized in that, The width of the fifth photoresist layer is smaller than the width of the sixth photoresist layer, and the width of the sixth photoresist layer is equal to the width of the seventh photoresist layer. The viscosity of the fifth photoresist layer is 30 CPS to 50 CPS, the viscosity of the sixth photoresist layer is 200 CPS to 240 CPS, and the viscosity of the seventh photoresist layer is 150 CPS to 200 CPS. The thickness ratio of the fifth photoresist layer to the Ag mirror is 2:1 to 10:1, the thickness ratio of the sixth photoresist layer to the fifth photoresist layer is 5:1 to 10:1, and the thickness ratio of the seventh photoresist layer to the sixth photoresist layer is 1.5:1 to 3:
1.
7. The method for fabricating a matrix LED chip according to claim 1, characterized in that, The energy of the single exposure was 200 mJ / cm². 2 ~230mj / cm 2 The energy of the second exposure is 300 mJ / cm. 2 ~350mj / cm 2 The energy of the three exposures was 250 mJ / cm². 2 ~300mJ / cm 2 The exposure time for the first exposure is 0.4S~0.6S, the exposure time for the second exposure is 0.6S~0.8S, and the exposure time for the third exposure is 0.8S~1.0S. The wavelength of the light in the third exposure is greater than the wavelength of the light in the second exposure.
8. The method for fabricating a matrix LED chip according to claim 1, characterized in that, After the step of depositing an Ag reflector on the epitaxial layer, and partially covering the Ag reflector onto the first insulating protective layer, the method further includes: A second insulating protective layer, an N-type conductive layer, a third insulating protective layer, an N-type pad, and a P-type pad are sequentially disposed on the epitaxial layer. The N-type pad is electrically connected to the N-type conductive layer, and the P-type pad is electrically connected to the Ag reflector.
Citation Information
Patent Citations
Flip LED chip and preparation method thereof
CN113782649A
Flip high-voltage light-emitting diode chip and preparation method thereof